Methods for fabricating driving substrates and methods for fabricating light-emitting diode substrates
By forming a patterned photoresist layer on the bonding pad as a shield and electroplating a second metal layer in a high-temperature process, the problem of bonding pad oxidation is solved, the electrical connection reliability of the drive substrate is improved, and the process is simplified.
Patent Information
- Application Number
- CN202310793217.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-29
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-06-29
AI Technical Summary
During the high-temperature manufacturing process of the drive substrate, the bonding pads are easily oxidized, resulting in poor conductivity and affecting electrical connections.
After the bonding pad is formed, a second metal layer is electroplated on the exposed electroplating seed layer using a patterned photoresist layer as a mask, while retaining the photoresist layer covering the bonding pad to reduce the risk of oxidation during the high-temperature process.
It effectively reduces the risk of oxidation of the bonding pad during high-temperature processes, improves the reliability of electrical connections, and saves process steps.
Smart Images

Figure CN117476697B_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of display technology, specifically to a method for preparing a driving substrate and a method for preparing a light-emitting diode substrate. Background Technology
[0002] Currently, driver substrates are mostly used in display panels or backlight substrates. For example, they can serve as array substrates for liquid crystal panels, driver backplanes for organic light-emitting diode (OLED) display panels, and driver backplanes for Mini-LED / Micro-LED display panels and backlight substrates. Driver substrates typically have bonding pads for bonding and connecting with driving devices such as flip-chip films or flexible circuit boards.
[0003] The fabrication of bonding pads is a precision process, and oxidation of the bonding pads can significantly affect electrical connectivity. However, in the conventional manufacturing process of driver substrates, high-temperature processes are used to solidify other film layers. Because the bonding pads are exposed during these high-temperature processes, they are easily oxidized, resulting in poor conductivity. Summary of the Invention
[0004] This application provides a method for preparing a driving substrate and a method for preparing a light-emitting diode substrate, which can reduce the risk of bonding pads being oxidized.
[0005] This application provides a method for preparing a driving substrate, which includes the following steps:
[0006] A substrate is provided, the substrate including a first region and a second region disposed on one side of the first region;
[0007] A patterned first metal layer is formed on the substrate, the first metal layer including bonding pads disposed in the second region;
[0008] An insulating layer is formed on the first metal layer, the insulating layer covering the first metal layer, and the insulating layer exposing the bonding pad;
[0009] An electroplating seed layer is formed on the insulating layer, the electroplating seed layer at least covering the first region;
[0010] A patterned photoresist layer is formed on the electroplating seed layer. The photoresist layer includes a first portion located in the first region and a second portion located in the second region. The second portion covers the bonding pad. An opening is provided on the first portion to expose the electroplating seed layer.
[0011] A second metal layer is electroplated inside the opening;
[0012] Remove the portion of the electroplated seed layer located in the first region and the first portion of the photoresist layer, leaving the second portion covering the bonding pad;
[0013] At least one film layer is formed on the second metal layer, and the film layer is cured under baking.
[0014] Remove the second portion of the photoresist layer to expose the bonding pad.
[0015] Optionally, in some embodiments of this application, forming a patterned photoresist layer on the electroplated seed layer includes the following steps:
[0016] A photoresist layer is formed on the electroplated seed layer;
[0017] Expose the photoresist material layer;
[0018] The photoresist material layer is developed to form an opening in the first region that exposes the electroplating seed layer;
[0019] The photoresist material layer is baked to form a patterned photoresist layer, wherein the adhesion of the first part of the photoresist layer is less than the adhesion of the second part of the photoresist layer.
[0020] Optionally, in some embodiments of this application, exposing the photoresist material layer includes the following steps:
[0021] A first light beam is used to expose the portion of the photoresist material layer located in the first region, and a second light beam is used to expose the portion of the photoresist material layer located in the second region. The light intensity of the first light beam is less than the light intensity of the second light beam, and / or the illumination time of the first light beam is less than the illumination time of the second light beam.
[0022] Optionally, in some embodiments of this application, exposing the photoresist material layer includes the following steps:
[0023] A mask template is provided, the mask template including a plurality of first cutouts and a second cutout;
[0024] The photoresist material layer is blocked by the mask template. The first cutout corresponds to the first region, and the second cutout corresponds to the second region. The second cutout exposes all areas where the bonding pads are located, so that the light intensity transmitted through the second cutout is greater than the light intensity transmitted through the first cutout.
[0025] Optionally, in some embodiments of this application, baking the photoresist material layer includes the following steps:
[0026] The photoresist material layer is baked so that the curing rate of the first part of the photoresist layer is less than the curing rate of the second part of the photoresist layer.
[0027] Optionally, in some embodiments of this application, baking the photoresist material layer includes the following steps:
[0028] At a first set temperature, the portion of the photoresist material layer corresponding to the first region is baked;
[0029] At a second set temperature, the portion of the photoresist material layer corresponding to the second region is baked, where the first set temperature is lower than the second set temperature.
[0030] Optionally, in some embodiments of this application, forming a photoresist material layer on the electroplated seed layer includes the following steps:
[0031] A first photoresist layer is formed on the portion of the electroplated seed layer corresponding to the first region;
[0032] A second photoresist layer is formed on the portion of the electroplated seed layer corresponding to the second region, wherein the solid content of the first photoresist layer is less than the solid content of the second photoresist layer.
[0033] Optionally, in some embodiments of this application, forming an electroplating seed layer on the insulating layer includes the step of: forming a patterned electroplating seed layer on the insulating layer, wherein the electroplating seed layer only covers the first region;
[0034] Forming a patterned photoresist layer on the electroplating seed layer includes the steps of: forming a patterned photoresist layer on the electroplating seed layer, wherein a first portion of the photoresist layer is disposed on the electroplating seed layer, and a second portion of the photoresist layer directly covers the bonding pad;
[0035] Removing the second portion of the photoresist layer to expose the bonding pad includes the steps of: removing the second portion of the photoresist layer with a cleaning solution and cleaning the bonding pad.
[0036] Optionally, in some embodiments of this application, forming an electroplating seed layer on the insulating layer includes the step of: forming a patterned electroplating seed layer on the insulating layer, the electroplating seed layer covering the first region and the second region;
[0037] Forming a patterned photoresist layer on the electroplating seed layer includes the steps of: forming a patterned photoresist layer on the electroplating seed layer, wherein the photoresist layer is disposed on the electroplating seed layer;
[0038] Removing the second portion of the photoresist layer to expose the bonding pad includes the steps of: removing the second portion of the photoresist layer and the electroplated seed layer corresponding to the second region, and exposing the bonding pad.
[0039] This application also relates to a method for preparing a driving substrate, which includes the following steps:
[0040] A substrate is provided, the substrate including a first region and a second region disposed on one side of the first region;
[0041] A patterned first metal layer is formed on the substrate, the first metal layer including bonding pads disposed in the second region;
[0042] An insulating layer is formed on the first metal layer, the insulating layer covering the first metal layer, and the insulating layer exposing the bonding pad;
[0043] A patterned second metal layer is formed on the portion of the insulating layer corresponding to the first region;
[0044] A patterned photoresist layer is formed on the second metal layer, the photoresist layer comprising a first portion located in the first region and a second portion located in the second region, the second portion covering the bonding pad;
[0045] Remove the first portion of the photoresist layer, leaving the second portion covering the bonding pad;
[0046] At least one film layer is formed on the second metal layer, and the film layer is cured under baking.
[0047] Remove the second portion of the photoresist layer to expose the bonding pad.
[0048] Optionally, in some embodiments of this application, a patterned second metal layer is formed on the portion of the insulating layer corresponding to the first region, including the following steps:
[0049] An electroplating seed layer is formed on the insulating layer, the electroplating seed layer at least covering the first region;
[0050] A patterned photoresist layer is formed on the electroplating seed layer, the photoresist layer covering the first region and the second region, and the photoresist layer has an opening in the portion corresponding to the first region to expose the electroplating seed layer.
[0051] A second metal layer is electroplated inside the opening;
[0052] Remove the portions of the photoresist layer and the electroplating seed layer that overlap with the photoresist layer.
[0053] Optionally, in some embodiments of this application, forming a patterned photoresist layer on the second metal layer includes the following steps:
[0054] A photoresist layer is formed on the second metal layer;
[0055] Expose the photoresist material layer;
[0056] Develop the photoresist material layer;
[0057] The photoresist material layer is baked to form a patterned photoresist layer, wherein the adhesion of the first part of the photoresist layer is less than the adhesion of the second part of the photoresist layer.
[0058] Optionally, in some embodiments of this application, exposing the photoresist material layer includes the following steps:
[0059] A first light beam is used to expose the portion of the photoresist material layer located in the first region, and a second light beam is used to expose the portion of the photoresist material layer located in the second region. The light intensity of the first light beam is less than the light intensity of the second light beam, and / or the illumination time of the first light beam is less than the illumination time of the second light beam.
[0060] Optionally, in some embodiments of this application, exposing the photoresist material layer includes the following steps:
[0061] A mask template is provided, the mask template including a plurality of first cutouts and a second cutout;
[0062] The photoresist material layer is blocked by the mask template. The first cutout corresponds to the first region, and the second cutout corresponds to the second region. The second cutout exposes all areas where the bonding pads are located, so that the light intensity transmitted through the second cutout is greater than the light intensity transmitted through the first cutout.
[0063] Optionally, in some embodiments of this application, baking the photoresist material layer includes the following steps:
[0064] The photoresist material layer is baked so that the curing rate of the first part of the photoresist layer is less than the curing rate of the second part of the photoresist layer.
[0065] Optionally, in some embodiments of this application, baking the photoresist material layer includes the following steps:
[0066] At a first set temperature, the portion of the photoresist material layer corresponding to the first region is baked;
[0067] At a second set temperature, the portion of the photoresist material layer corresponding to the second region is baked, where the first set temperature is lower than the second set temperature.
[0068] Optionally, in some embodiments of this application, forming a photoresist material layer on the second metal layer includes the following steps:
[0069] A first photoresist layer is formed on the portion of the electroplated seed layer corresponding to the first region;
[0070] A second photoresist layer is formed on the portion of the electroplated seed layer corresponding to the second region, wherein the solid content of the first photoresist layer is less than the solid content of the second photoresist layer.
[0071] Optionally, in some embodiments of this application, forming an electroplating seed layer on the insulating layer includes the step of: forming a patterned electroplating seed layer on the insulating layer, wherein the electroplating seed layer only covers the first region.
[0072] Optionally, in some embodiments of this application, forming an electroplating seed layer on the insulating layer includes the step of: forming a patterned electroplating seed layer on the insulating layer, the electroplating seed layer covering the first region and the second region.
[0073] Optionally, in some embodiments of this application, removing the second portion of the photoresist layer to expose the bonding pad includes the steps of: removing the second portion of the photoresist layer with a cleaning solution, while cleaning the bonding pad and exposing the bonding pad.
[0074] Accordingly, this application also provides a method for fabricating a light-emitting diode substrate, which includes the following steps:
[0075] A substrate is provided, the substrate including a first region and a second region disposed on one side of the first region;
[0076] A patterned first metal layer is formed on the substrate, the first metal layer including bonding pads disposed in the second region;
[0077] An insulating layer is formed on the first metal layer, the insulating layer covering the first metal layer, and the insulating layer exposing the bonding pad;
[0078] An electroplating seed layer is formed on the insulating layer, the electroplating seed layer at least covering the first region;
[0079] A patterned photoresist layer is formed on the electroplating seed layer. The photoresist layer includes a first portion located in the first region and a second portion located in the second region. The second portion covers the bonding pad. An opening is provided on the first portion to expose the electroplating seed layer.
[0080] A second metal layer is electroplated inside the opening;
[0081] Remove the portion of the electroplated seed layer located in the first region and the first portion of the photoresist layer, leaving the second portion covering the bonding pad;
[0082] Multiple film layers are formed on the second metal layer to form a driving circuit structure layer, the driving circuit structure layer including thin film transistors;
[0083] Light-emitting diode devices are disposed on the drive circuit structure layer by reflow soldering.
[0084] Remove the second portion of the photoresist layer to expose the bonding pad.
[0085] Optionally, in some embodiments of this application, forming a patterned photoresist layer on the electroplated seed layer includes the following steps:
[0086] A photoresist layer is formed on the electroplated seed layer;
[0087] Expose the photoresist material layer;
[0088] The photoresist material layer is developed to form an opening in the first region that exposes the electroplating seed layer;
[0089] The photoresist material layer is baked to form a patterned photoresist layer, wherein the adhesion of the first part of the photoresist layer is less than the adhesion of the second part of the photoresist layer.
[0090] Optionally, in some embodiments of this application, exposing the photoresist material layer includes the following steps:
[0091] A first light beam is used to expose the portion of the photoresist material layer located in the first region, and a second light beam is used to expose the portion of the photoresist material layer located in the second region. The light intensity of the first light beam is less than the light intensity of the second light beam, and / or the illumination time of the first light beam is less than the illumination time of the second light beam.
[0092] Optionally, in some embodiments of this application, exposing the photoresist material layer includes the following steps:
[0093] A mask template is provided, the mask template including a plurality of first cutouts and a second cutout;
[0094] The photoresist material layer is blocked by the mask template. The first cutout corresponds to the first region, and the second cutout corresponds to the second region. The second cutout exposes all areas where the bonding pads are located, so that the light intensity transmitted through the second cutout is greater than the light intensity transmitted through the first cutout.
[0095] Optionally, in some embodiments of this application, baking the photoresist material layer includes the following steps:
[0096] The photoresist material layer is baked so that the curing rate of the first part of the photoresist layer is less than the curing rate of the second part of the photoresist layer.
[0097] Optionally, in some embodiments of this application, baking the photoresist material layer includes the following steps:
[0098] At a first set temperature, the portion of the photoresist material layer corresponding to the first region is baked;
[0099] At a second set temperature, the portion of the photoresist material layer corresponding to the second region is baked, where the first set temperature is lower than the second set temperature.
[0100] Optionally, in some embodiments of this application, forming a photoresist material layer on the electroplated seed layer includes the following steps:
[0101] A first photoresist layer is formed on the portion of the electroplated seed layer corresponding to the first region;
[0102] A second photoresist layer is formed on the portion of the electroplated seed layer corresponding to the second region, wherein the solid content of the first photoresist layer is less than the solid content of the second photoresist layer.
[0103] Optionally, in some embodiments of this application, forming an electroplating seed layer on the insulating layer includes the step of: forming a patterned electroplating seed layer on the insulating layer, wherein the electroplating seed layer only covers the first region;
[0104] Forming a patterned photoresist layer on the electroplating seed layer includes the steps of: forming a patterned photoresist layer on the electroplating seed layer, wherein a first portion of the photoresist layer is disposed on the electroplating seed layer, and a second portion of the photoresist layer directly covers the bonding pad;
[0105] Removing the second portion of the photoresist layer to expose the bonding pad includes the steps of: removing the second portion of the photoresist layer with a cleaning solution and cleaning the bonding pad.
[0106] Optionally, in some embodiments of this application, forming an electroplating seed layer on the insulating layer includes the step of: forming a patterned electroplating seed layer on the insulating layer, the electroplating seed layer covering the first region and the second region;
[0107] Forming a patterned photoresist layer on the electroplating seed layer includes the steps of: forming a patterned photoresist layer on the electroplating seed layer, wherein the photoresist layer is disposed on the electroplating seed layer;
[0108] Removing the second portion of the photoresist layer to expose the bonding pad includes the steps of: removing the second portion of the photoresist layer and the electroplated seed layer corresponding to the second region, and exposing the bonding pad.
[0109] The method for fabricating the driving substrate and the light-emitting diode substrate in this application embodiment involves forming a second metal layer on the exposed electroplating seed layer after the step of forming bonding pads, using a patterned photoresist layer as a shield, and then retaining the photoresist layer covering the bonding pads. This reduces the risk of the bonding pads being oxidized in subsequent high-temperature processes and saves process steps. The high-temperature process can be a film layer process that requires baking and curing, or a reflow soldering process in component assembly. Attached Figure Description
[0110] Figure 1 This is a schematic diagram of step B1 in the method for preparing the driving substrate provided in the embodiments of this application;
[0111] Figure 2 This is a schematic diagram of step B2 in the method for preparing the driving substrate provided in the embodiments of this application;
[0112] Figure 3 This is a schematic diagram of step B3 in the method for preparing the driving substrate provided in the embodiments of this application;
[0113] Figure 4 This is a schematic diagram of step B4 in the method for preparing the driving substrate provided in the embodiments of this application;
[0114] Figure 5 This is a schematic diagram of step B5 in the method for preparing the driving substrate provided in the embodiments of this application;
[0115] Figure 6 This is a schematic diagram of step B6 in the method for preparing the driving substrate provided in the embodiments of this application;
[0116] Figure 7 This is a schematic diagram of step B7 in the method for preparing the driving substrate provided in the embodiments of this application;
[0117] Figure 8 This is a schematic diagram of step B8 in the method for preparing the driving substrate provided in the embodiments of this application;
[0118] Figure 9 This is a schematic diagram of step B9 in the method for preparing the driving substrate provided in the embodiments of this application;
[0119] Figure 10 This is a schematic flowchart of a method for fabricating a driving substrate according to another embodiment of this application;
[0120] Figure 11 This is a schematic diagram of step B104 in the method for preparing a driving substrate according to another embodiment of this application;
[0121] Figure 12 This is a schematic diagram of step B105 in the method for preparing a driving substrate according to another embodiment of this application;
[0122] Figure 13 This is a schematic diagram of step B106 in the method for preparing a driving substrate according to another embodiment of this application;
[0123] Figure 14 This is a schematic diagram of step B107 in the method for preparing a driving substrate according to another embodiment of this application;
[0124] Figure 15 This is a schematic diagram of step B108 in the method for preparing a driving substrate according to another embodiment of this application;
[0125] Figure 16 This is a schematic diagram of step B28 in the method for fabricating a light-emitting diode substrate provided in this application embodiment;
[0126] Figure 17 This is a schematic diagram of step B29 in the method for fabricating a light-emitting diode substrate provided in this application embodiment;
[0127] Figure 18 This is a schematic diagram of step B210 in the method for preparing a light-emitting diode substrate provided in this application embodiment. Detailed Implementation
[0128] The technical solutions in the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of this application, and not all of the embodiments. Based on the embodiments in this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application. In addition, it should be understood that the specific embodiments described herein are only for illustration and explanation of this application and are not intended to limit this application. In this application, unless otherwise stated, directional terms such as "upper" and "lower" generally refer to the upper and lower positions of the device in actual use or operation, specifically the drawing directions in the accompanying drawings; while "inner" and "outer" refer to the outline of the device; the terms "first," "second," "third," etc., are used only as indications and do not impose numerical requirements or establish a sequence.
[0129] This application provides a method for fabricating a driving substrate and a method for fabricating a light-emitting diode (LED) substrate. The driving substrate is commonly used in display panels or backlight substrates, such as as an array substrate for a liquid crystal panel, a driving backplane for an organic light-emitting diode (OLED) display panel, a driving backplane for a Mini-LED / Micro-LED display panel, and a driving backplane for a Mini-LED / Micro-LED backlight substrate, etc. The LED substrate can be a Mini-LED / Micro-LED display panel or a Mini-LED / Micro-LED backlight substrate. A detailed description follows. It should be noted that the order of description of the following embodiments is not intended to limit the preferred order of the embodiments.
[0130] This application provides a method for preparing a driving substrate, which includes the following steps:
[0131] Step B1: Provide a substrate, the substrate including a first region and a second region disposed on one side of the first region;
[0132] Step B2: A patterned first metal layer is formed on the substrate, the first metal layer including bonding pads disposed in the second region;
[0133] Step B3: An insulating layer is formed on the first metal layer, the insulating layer covering the first metal layer and exposing the bonding pad;
[0134] Step B4: Form an electroplating seed layer on the insulating layer, the electroplating seed layer at least covering the first region;
[0135] Step B5: A patterned photoresist layer is formed on the electroplating seed layer. The photoresist layer includes a first portion located in the first region and a second portion located in the second region. The second portion covers the bonding pad, and the first portion has an opening that exposes the electroplating seed layer.
[0136] Step B6: Electroplating a second metal layer inside the opening;
[0137] Step B7: Remove the portion of the electroplated seed layer located in the first region and the first portion of the photoresist layer, leaving the second portion covering the bonding pad;
[0138] Step B8: Form at least one film layer on the second metal layer, the film layer being cured under baking;
[0139] Step B9: Remove the second portion of the photoresist layer to expose the bonding pad.
[0140] The method for preparing the driving substrate in this application embodiment involves forming a second metal layer on an exposed electroplating seed layer after the step of forming bonding pads, using a patterned photoresist layer as a shield. The photoresist layer covering the bonding pads is then retained to reduce the risk of the bonding pads being oxidized in subsequent high-temperature processes. The high-temperature process can be a film layer process that requires baking and curing, or a reflow soldering process in component assembly.
[0141] Optionally, the fabrication method of the driving substrate will be described below.
[0142] In step B1, please refer to Figure 1 A substrate 11 is provided, the substrate 11 includes a first region 11a and a second region 11b disposed on one side of the first region 11a.
[0143] The first region 11a is used for the display area of the corresponding display panel or the light-emitting area of the backlight substrate. The second region 11b is a bonding area, used for bonding and connecting with external devices; the external devices can be flip-chip films, flexible circuit boards, transistors, or chips, etc.
[0144] Optionally, the substrate 11 can be made of glass, sapphire, or a PCB substrate. The thickness of the substrate 11 can be, but is not limited to, 0.4 mm, 0.5 mm, or 0.7 mm.
[0145] In step B2, please refer to Figure 2 A patterned first metal layer 12 is formed on the substrate 11. The first metal layer 12 includes bonding pads 121 disposed in the second region 11b.
[0146] It should be noted that the first metal layer 12 also includes a signal component 122 disposed in the first region 11a. The signal component may be a gate, a scan line, a common electrode line, or other signal traces.
[0147] Optionally, the first metal layer 12 can be formed by vapor deposition or by electroplating.
[0148] Optionally, the first metal layer 12 may be formed using a metal element selected from chromium (Cr), copper (Cu), aluminum (Al), gold (Au), silver (Ag), zinc (Zn), molybdenum (Mo), tantalum (Ta), titanium (Ti), tungsten (W), manganese (Mn), nickel (Ni), iron (Fe), and cobalt (Co), an alloy with any of the above metal elements as its composition, or an alloy combining any of the above metal elements. Furthermore, the first metal layer 12 may have a single-layer structure or a stacked structure of two or more layers.
[0149] Optionally, bonding pads 121 may be disposed on the long side and / or short side of the substrate 11. The width of bonding pads 121 is, but is not limited to, 50 mm, and the number is, but is not limited to, 8 or 12. The thickness of bonding pads 121 is, but is not limited to, 5 mm or 10 mm.
[0150] In step B3, please refer to Figure 3 An insulating layer 13 is formed on the first metal layer 12. The insulating layer 13 covers the first metal layer 12 and exposes the bonding pad 121.
[0151] Optionally, the insulating layer 13 may be formed of a plurality of inorganic layers stacked in an alternating manner. For example, the insulating layer 13 may be formed as a bilayer by stacking inorganic layers comprising at least one of silicon oxide, silicon nitride, silicon oxynitride, aluminum oxide, magnesium oxide, and titanium oxide, or as a multilayer by alternating stacking inorganic layers comprising at least one of silicon oxide, silicon nitride, silicon oxynitride, aluminum oxide, magnesium oxide, and titanium oxide. However, this disclosure is not limited thereto, and the insulating layer 13 may be formed as a single inorganic layer comprising the aforementioned insulating material.
[0152] In step B4, please refer to Figure 4 An electroplating seed layer 14 is formed on the insulating layer 13. The electroplating seed layer 14 at least covers the first region 11a.
[0153] Optionally, the electroplating seed layer 14 covers only the first region 11a.
[0154] Optionally, the material of the electroplated seed layer 14 can be silver, copper, nickel-chromium alloy, etc.
[0155] In step B5, please refer to Figure 5 A patterned photoresist layer 15 is formed on the electroplating seed layer 14. The photoresist layer 15 includes a first portion 151 located in a first region 11a and a second portion 152 located in a second region 11b. The second portion 152 covers the bonding pad 121. An opening k1 is provided on the first portion 151 to expose the electroplating seed layer 14.
[0156] The first part 151 of the photoresist layer 15 is disposed on the electroplating seed layer 14, and the second part 152 of the photoresist layer 15 directly covers the bonding pad 121.
[0157] Optionally, step B5 includes the following steps:
[0158] Step B51: Form a photoresist material layer on the electroplated seed layer 14;
[0159] Step B52: Expose the photoresist material layer;
[0160] Step B53: Develop the photoresist material layer to form an opening k1 of the exposed electroplating seed layer 14 in the first region 11a;
[0161] Step B54: Bake the photoresist material layer to form a patterned photoresist layer 15. The adhesion of the first portion 151 of the photoresist layer 15 is less than the adhesion of the second portion 152 of the photoresist layer 15.
[0162] Optionally, the thickness of the photoresist material layer is greater than or equal to 8 micrometers, such as 8 micrometers, 9 micrometers, 10 micrometers, 12 micrometers, or 15 micrometers. The material of the photoresist material layer can be ordinary photoresist or electroplated photoresist.
[0163] It should be noted that adhesion refers to the adhesive force of the first feature to the second feature. It can be obtained through aging separation test or peel separation test. For example, the longer the aging time required to separate the first feature and the second feature, the stronger the adhesion of the first feature; or, the greater the pulling force required to pull the first feature away from the second feature to achieve separation, the stronger the adhesion of the first feature.
[0164] Since the adhesion of the first portion 151 is less than that of the second portion 152, when the photoresist layer 15 is peeled off, the first portion 151 will be peeled off first, while the remaining second portion 152 will be retained to protect the bonding pad 121. The step of making the adhesion of the first portion 151 less than that of the second portion 152 can be reflected in at least one of steps B51, B52 and B54.
[0165] For example, in step B52, a first light beam is used to expose the portion of the photoresist material layer located in the first region 11a. A second light beam is used to expose the portion of the photoresist material layer located in the second region 11b. The illumination intensity of the first light beam is less than the illumination intensity of the second light beam, and / or, the illumination time of the first light beam is less than the illumination time of the second light beam.
[0166] The photoresist layer 15 is cured to different degrees by varying the light intensity and / or the light exposure time. That is, by increasing the light intensity and / or the light exposure time of the photoresist material layer in the second region 11b, the adhesion of the second part 152 is made greater than that of the first part 151, which increases the difficulty of peeling off the second part 152 and thus preserves the second part 152.
[0167] Optionally, the photoresist material layer is a negative photoresist.
[0168] Of course, in some embodiments, the photoresist material layer can also be a positive photoresist.
[0169] Optionally, in some embodiments, the illumination intensity and / or amount of light on the photoresist layer located in the second region 11b can be increased by improving the photomask. For example:
[0170] A mask template is provided, the mask template including a plurality of first cutouts and a second cutout;
[0171] The photoresist material layer is blocked by the mask template. The first cutout corresponds to the first region, and the second cutout corresponds to the second region. The second cutout exposes all areas where the bonding pads are located, so that the light intensity transmitted through the second cutout is greater than the light intensity transmitted through the first cutout.
[0172] This means that the portion of the photomask corresponding to the second region 11b (binding area) is completely hollowed out to increase the exposure and thus accelerate the curing speed of the photoresist material layer on the second region 11b.
[0173] Optionally, in some embodiments, in step B54, the baking temperature and / or baking time for the portion of the photoresist layer corresponding to the second region 11b may be increased to improve the curing degree of the photoresist layer on the second region 11b. The higher the curing degree, the stronger the adhesion of the photoresist layer.
[0174] For example, baking the photoresist layer can reduce the curing rate of the first part of the photoresist layer to be less than that of the second part of the photoresist layer.
[0175] It should be explained that when the second region is fully baked, the higher the hardness of the photoresist layer, the higher its curing rate.
[0176] Optionally, at a first set temperature, the portion of the photoresist material layer corresponding to the first region is baked; at a second set temperature, the portion of the photoresist material layer corresponding to the second region is baked, wherein the first set temperature is lower than the second set temperature.
[0177] And / or, for a first set duration, the portion of the photoresist material layer corresponding to the first region is baked; for a second set duration, the portion of the photoresist material layer corresponding to the second region is baked, wherein the first set duration is shorter than the second set duration.
[0178] Optionally, in some embodiments, two photoresist materials with different solid contents can be selected in step B51, so that the adhesion of the two photoresist materials after curing is different.
[0179] Optionally, step B51 includes: forming a first photoresist layer on the portion of the electroplating seed layer 14 corresponding to the first region 11a; and forming a second photoresist layer on the portion of the electroplating seed layer 14 corresponding to the second region 11b. The solid content of the first photoresist layer is less than the solid content of the second photoresist layer.
[0180] Since the solid content of the second photoresist layer is greater than that of the first photoresist layer, the adhesion of the second portion 152 formed by the second photoresist layer is greater than that of the first portion 151 formed by the first photoresist layer.
[0181] In step B6, please refer to Figure 6 A second metal layer 16 is electroplated inside the opening k1.
[0182] In step B7, please refer to Figure 7 Remove the portion of the electroplated seed layer 14 located in the first region 11a and the first portion 151 of the photoresist layer 15, leaving the second portion 152 to cover the bonding pad 121.
[0183] Optionally, a stripping solution is used to peel off the photoresist layer 15. Since the adhesion of the first part 151 is less than that of the second part 152, the first part 151 is peeled off first under the action of the stripping solution. After the first part 151 is peeled off, the stripping of the photoresist layer 15 is stopped, and the second part 152 can be retained to continue to cover the bonding pad 121.
[0184] In step B8, please refer to Figure 8 At least one film layer 17 is formed on the second metal layer 16. The film layer 17 is cured by baking.
[0185] Because the bonding pad 121 is covered by the second portion 152 of the photoresist layer 15, the risk of the bonding pad 121 coming into contact with air is reduced. When the film layer 17 is in the baking state, the arrangement of the second portion 152 of the photoresist layer 15 reduces the risk of the bonding pad 121 being oxidized. It also reduces the risk of the bonding pad 121 being contaminated by electroplating and etching solutions.
[0186] Alternatively, film layer 17 can be a reflective layer made of white oil, which can be formed by thermosetting. Film layer 17 can also be a protective layer, which can also be formed by thermosetting. Alternatively, film layer 17 can be an active layer, which requires high-temperature crystallization.
[0187] In step B9, please refer to Figure 9 Remove the second part 152 of the photoresist layer 15 to expose the bonding pad 121.
[0188] Optionally, a cleaning solution is used to remove the second portion 152 of the photoresist layer 15 and to clean the bonding pad 121. Using a cleaning solution to remove the photoresist layer 15 and clean the bonding pad 121 simultaneously saves process steps.
[0189] Optionally, the cleaning solution can be a liquid such as alcohol that can dissolve phenolic resin.
[0190] Please refer to Figure 10 In some embodiments, the method for preparing the driving substrate differs from the method for preparing the driving substrate in the above embodiments in steps B4, B5, and B9.
[0191] Step B4, forming an electroplating seed layer on the insulating layer, includes the steps of: forming a patterned electroplating seed layer 14 on the insulating layer 13, the electroplating seed layer 14 covering the first region 11a and the second region 11b.
[0192] Step B5, forming a patterned photoresist layer 15 on the electroplating seed layer 14, includes the steps of: forming a patterned photoresist layer 15 on the electroplating seed layer 14, wherein the photoresist layer 15 is disposed on the electroplating seed layer 14.
[0193] Step B9, removing the second portion 152 of the photoresist layer 15 to expose the bonding pad 121, includes the steps of: removing the second portion 152 of the photoresist layer 15 and the electroplated seed layer 14 corresponding to the second region 11b, and exposing the bonding pad 121.
[0194] The second part 152 of the photoresist layer 15 is stripped using a stripping solution, and the remaining electroplating seed layer 14 is removed using a wet etching process.
[0195] In this embodiment, after step B7, the step of cleaning the bonding pad is further included. The bonding pad can be cleaned with a cleaning solution.
[0196] This application also relates to another method for preparing a driving substrate, which includes the following steps:
[0197] Step B101: Provide a substrate, the substrate including a first region and a second region disposed on one side of the first region;
[0198] Step B102: A patterned first metal layer is formed on the substrate, the first metal layer including bonding pads disposed in the second region;
[0199] Step B103: An insulating layer is formed on the first metal layer, the insulating layer covering the first metal layer and exposing the bonding pad;
[0200] Step B104: Form a patterned second metal layer on the portion of the insulating layer corresponding to the first region;
[0201] Step B105: A patterned photoresist layer is formed on the second metal layer, the photoresist layer comprising a first portion located in the first region and a second portion located in the second region, the second portion covering the bonding pad;
[0202] Step B106: Remove the first portion of the photoresist layer, leaving the second portion covering the bonding pad;
[0203] Step B107: Form at least one film layer on the second metal layer, the film layer being cured under baking;
[0204] Step B108: Remove the second portion of the photoresist layer to expose the bonding pad.
[0205] The method for preparing the driving substrate in this application embodiment adds a patterned photoresist layer as a shield after the step of forming a patterned second metal layer, and retains the photoresist layer covering the bonding pad area to reduce the risk of the bonding pad being oxidized in the subsequent high-temperature process. The high-temperature process can be a film layer process that requires baking and curing, or a reflow soldering process in the assembly process.
[0206] Optionally, the fabrication method of the driving substrate will be described below.
[0207] Step B101 is the same as step B1, step B102 is the same as step B2, and step B103 is the same as step B3. Therefore, steps B101, B102, and B103 will not be described here. Please refer to the description of steps B1, B2, and B3 for details.
[0208] In step B104, please refer to Figure 11 A patterned second metal layer 16 is formed on the portion of the insulating layer 13 corresponding to the first region 11a.
[0209] Optionally, the patterned second metal layer 16 can be formed by electroplating or by photolithography; there is no limitation, as long as a patterned second metal layer 16 can be formed. This embodiment uses electroplating to form the patterned second metal layer 16 as an example for explanation, but it is not limited to this.
[0210] Please refer to Figure 11 Step B104 includes the following steps:
[0211] Step B1041: An electroplating seed layer 14 is formed on the insulating layer 13, the electroplating seed layer 14 at least covering the first region 11a; for example, the electroplating seed layer 14 may only cover the first region 11a, or the electroplating seed layer 14 may cover the first region 11a and the second region 11b.
[0212] Optionally, the material of the electroplated seed layer 14 can be silver, copper, nickel-chromium alloy, etc.
[0213] Step B1042: A patterned photoresist layer PR is formed on the electroplating seed layer 14. The photoresist layer PR covers the first region 11a and the second region 11b. The photoresist layer PR has an opening k1 exposed in the portion corresponding to the first region 11a.
[0214] Step B1043: Electroplating a second metal layer 16 inside the opening k1;
[0215] Step B1044: Remove the photoresist layer PR and remove the portion of the electroplating seed layer 14 that overlaps with the photoresist layer PR to expose the bonding pad 121.
[0216] Optionally, all photoresist layers PR are removed using a stripping solution, followed by wet etching to remove the exposed portion of the electroplating seed layer 14, in order to form a patterned second metal layer 16 and exposed bonding pads 121.
[0217] In step B105, please refer to Figure 12 A patterned photoresist layer 15 is formed on the second metal layer 16. The photoresist layer 15 includes a first portion 151 located in the first region 11a and a second portion 152 located in the second region 11b. The second portion 152 covers the bonding pad 121.
[0218] Optionally, step B105 includes the following steps:
[0219] Step B1051: A photoresist material layer is formed on the second metal layer 16;
[0220] Step B1052: Expose the photoresist material layer;
[0221] Step B1053: Develop the photoresist material layer;
[0222] Step B1054: Bake the photoresist material layer to form a patterned photoresist layer 15, wherein the adhesion of the first part 151 of the photoresist layer 15 is less than the adhesion of the second part 152 of the photoresist layer 15.
[0223] Optionally, the thickness of the photoresist material layer is greater than or equal to 8 micrometers, such as 8 micrometers, 9 micrometers, 10 micrometers, 12 micrometers, or 15 micrometers. The material of the photoresist material layer can be ordinary photoresist or electroplated photoresist.
[0224] It should be noted that adhesion refers to the adhesive force of the first feature to the second feature. It can be obtained through aging separation test or peel separation test. For example, the longer the aging time required to separate the first feature and the second feature, the stronger the adhesion of the first feature; or, the greater the pulling force required to pull the first feature away from the second feature to achieve separation, the stronger the adhesion of the first feature.
[0225] Since the adhesion of the first portion 151 is less than that of the second portion 152, when the photoresist layer 15 is peeled off, the first portion 151 will be peeled off first, while the remaining second portion 152 will be retained to protect the bonding pad 121. The step of making the adhesion of the first portion 151 less than that of the second portion 152 can be reflected in at least one of steps B1051, B1052 and B1054.
[0226] For example, in step B1052, a first light beam is used to expose the portion of the photoresist material layer located in the first region 11a. A second light beam is used to expose the portion of the photoresist material layer located in the second region 11b. The illumination intensity of the first light beam is less than the illumination intensity of the second light beam, and / or, the illumination time of the first light beam is less than the illumination time of the second light beam.
[0227] The photoresist layer 15 is cured to different degrees by varying the light intensity and / or the light exposure time. That is, by increasing the light intensity and / or the light exposure time of the photoresist material layer in the second region 11b, the adhesion of the second part 152 is made greater than that of the first part 151, which increases the difficulty of peeling off the second part 152 and thus preserves the second part 152.
[0228] Optionally, the photoresist material layer is a negative photoresist.
[0229] Of course, in some embodiments, the photoresist material layer can also be a positive photoresist.
[0230] Optionally, in some embodiments, the illumination intensity and / or amount of light on the photoresist layer located in the second region 11b can be increased by improving the photomask. For example:
[0231] A mask template is provided, the mask template including a plurality of first cutouts and a second cutout;
[0232] The photoresist material layer is blocked by the mask template. The first cutout corresponds to the first region, and the second cutout corresponds to the second region. The second cutout exposes all areas where the bonding pads are located, so that the light intensity transmitted through the second cutout is greater than the light intensity transmitted through the first cutout.
[0233] This means that the portion of the photomask corresponding to the second region 11b (binding area) is completely hollowed out to increase the exposure and thus accelerate the curing speed of the photoresist material layer on the second region 11b.
[0234] Optionally, in some embodiments, in step B1054, the baking temperature and / or baking time for the portion of the photoresist layer corresponding to the second region 11b may be increased to improve the curing degree of the photoresist layer on the second region 11b. The higher the curing degree, the stronger the adhesion of the photoresist layer.
[0235] For example, baking the photoresist layer can reduce the curing rate of the first part of the photoresist layer to be less than that of the second part of the photoresist layer.
[0236] It should be explained that when the second region is fully baked, the higher the hardness of the photoresist layer, the higher its curing rate.
[0237] Optionally, at a first set temperature, the portion of the photoresist material layer corresponding to the first region is baked; at a second set temperature, the portion of the photoresist material layer corresponding to the second region is baked, wherein the first set temperature is lower than the second set temperature.
[0238] And / or, for a first set duration, the portion of the photoresist material layer corresponding to the first region is baked; for a second set duration, the portion of the photoresist material layer corresponding to the second region is baked, wherein the first set duration is shorter than the second set duration.
[0239] Optionally, in some embodiments, two photoresist materials with different solid contents can be selected in step B51, so that the adhesion of the two photoresist materials after curing is different.
[0240] Optionally, step B1051 includes: forming a first photoresist layer on the portion of the electroplating seed layer 14 corresponding to the first region 11a; and forming a second photoresist layer on the portion of the electroplating seed layer 14 corresponding to the second region 11b. The solid content of the first photoresist layer is less than the solid content of the second photoresist layer.
[0241] Since the solid content of the second photoresist layer is greater than that of the first photoresist layer, the adhesion of the second portion 152 formed by the second photoresist layer is greater than that of the first portion 151 formed by the first photoresist layer.
[0242] In step B106, please refer to Figure 13 Remove the first part 151 of the photoresist layer 15, and retain the second part 152 to cover the bonding pad;
[0243] In step B107, please refer to Figure 14At least one film layer 17 is formed on the second metal layer 16, and the film layer 17 is cured by baking.
[0244] Because the bonding pad 121 is covered by the second portion 152 of the photoresist layer 15, the risk of the bonding pad 121 coming into contact with air is reduced. When the film layer 17 is in the baking state, the arrangement of the second portion 152 of the photoresist layer 15 reduces the risk of the bonding pad 121 being oxidized. It also reduces the risk of the bonding pad 121 being contaminated by electroplating and etching solutions.
[0245] In step B108, please refer to Figure 15 Remove the second part 152 of the photoresist layer 15 to expose the bonding pad 121.
[0246] Optionally, a cleaning solution is used to remove the second portion 152 of the photoresist layer 15 and to clean the bonding pad 121. Using a cleaning solution to remove both the photoresist layer 15 and the bonding pad 121 simultaneously saves process steps. Optionally, the cleaning solution can be a liquid such as alcohol that can dissolve phenolic resin.
[0247] Accordingly, this application also provides a method for fabricating a light-emitting diode substrate, which includes the following steps:
[0248] Step B21: Provide a substrate, the substrate including a first region and a second region disposed on one side of the first region;
[0249] Step B22: A patterned first metal layer is formed on the substrate, the first metal layer including bonding pads disposed in the second region;
[0250] Step B23: An insulating layer is formed on the first metal layer, the insulating layer covering the first metal layer and exposing the bonding pad;
[0251] Step B24: Form an electroplating seed layer on the insulating layer, the electroplating seed layer at least covering the first region;
[0252] Step B25: A patterned photoresist layer is formed on the electroplating seed layer. The photoresist layer includes a first portion located in the first region and a second portion located in the second region. The second portion covers the bonding pad, and the first portion has an opening that exposes the electroplating seed layer.
[0253] Step B26: Electroplating a second metal layer inside the opening;
[0254] Step B27: Remove the portion of the electroplated seed layer located in the first region and the first portion of the photoresist layer, leaving the second portion covering the bonding pad;
[0255] Step B28: Form a multilayer film on the second metal layer to form a driving circuit structure layer, the driving circuit structure layer including a thin film transistor;
[0256] Step B29: Deploy light-emitting diode devices on the drive circuit structure layer by reflow soldering;
[0257] Step B210: Remove the second portion of the photoresist layer to expose the bonding pad.
[0258] The method for fabricating a light-emitting diode substrate according to the present application embodiment involves forming a second metal layer on an exposed electroplating seed layer after the step of forming bonding pads, using a patterned photoresist layer as a shield, and then retaining the photoresist layer covering the bonding pads to reduce the risk of the bonding pads being oxidized in subsequent high-temperature processes. The high-temperature processes can be film layer processes that require baking and curing, or reflow soldering processes in component assembly.
[0259] The basic fabrication method for this light-emitting diode, compared to the aforementioned method for fabricating the driving substrate, includes an additional step B29: setting the light-emitting diode device on the driving circuit structure layer using reflow soldering. That is, the second part of step "removing the photoresist layer" is performed after reflow soldering to better protect the bonding pads.
[0260] It should be noted that steps B21 to B27 are the same as steps B1 to B7 in any of the above embodiments. For details, please refer to the description of steps B1 to B7 in the above embodiments, which will not be repeated here.
[0261] In step B28, please refer to Figure 16 A multilayer film layer 17 is formed on the second metal layer 16 to form a driving circuit structure layer, the driving circuit structure layer including a thin film transistor.
[0262] The driving circuit structure layer includes a signal component 122 of a first metal layer 12, an insulating layer 13, an electroplating seed layer 14, a second metal layer 16, and a multilayer film layer 17.
[0263] The thin-film transistor can be a top-gate, bottom-gate, or dual-gate thin-film transistor.
[0264] In step B29, please refer to Figure 17 The light-emitting diode device El is set on the drive circuit structure layer by reflow soldering.
[0265] Since reflow soldering is performed in a high-temperature environment, when the drive circuit structure layer and the light-emitting diode device E1 are reflow soldered, the second part 152 of the photoresist layer 15 protects the bonding pad 121, thereby reducing the risk of the bonding pad 121 being oxidized.
[0266] Optionally, the spacing between the light-emitting diode devices E1 can be, but is not limited to, 2 mm and 4 mm.
[0267] In step B210, please refer to Figure 18 Remove the second part 152 of the photoresist layer 15 to expose the bonding pad 121.
[0268] Optionally, a cleaning solution is used to remove the second portion 152 of the photoresist layer 15 and to clean the bonding pad 121. Using a cleaning solution to remove the photoresist layer 15 and clean the bonding pad 121 simultaneously saves process steps.
[0269] Optionally, the cleaning solution can be a liquid such as alcohol that can dissolve phenolic resin.
[0270] The method for preparing the driving substrate and the light-emitting diode substrate in this application embodiment involves forming a second metal layer on the exposed electroplating seed layer after the step of forming bonding pads, using a patterned photoresist layer as a shield, and then retaining the photoresist layer covering the bonding pads to reduce the risk of the bonding pads being oxidized in subsequent high-temperature processes. The high-temperature process can be a film layer process that requires baking and curing, or a reflow soldering process in component assembly.
[0271] The above provides a detailed description of the preparation method of a driving substrate and a light-emitting diode substrate provided in the embodiments of this application. Specific examples have been used to illustrate the principles and implementation methods of this application. The description of the above embodiments is only for the purpose of helping to understand the method and core ideas of this application. At the same time, for those skilled in the art, there will be changes in the specific implementation methods and application scope based on the ideas of this application. Therefore, the content of this specification should not be construed as a limitation of this application.
Claims
1. A method for fabricating a driving substrate, characterized in that, Includes the following steps: A substrate is provided, the substrate including a first region and a second region disposed on one side of the first region; A patterned first metal layer is formed on the substrate, the first metal layer including bonding pads disposed in the second region; An insulating layer is formed on the first metal layer, the insulating layer covering the first metal layer, and the insulating layer exposing the bonding pad; An electroplating seed layer is formed on the insulating layer, the electroplating seed layer at least covering the first region; A patterned photoresist layer is formed on the electroplating seed layer. The photoresist layer includes a first portion located in the first region and a second portion located in the second region. The second portion covers the bonding pad. An opening is provided on the first portion to expose the electroplating seed layer. A second metal layer is electroplated inside the opening; Remove the portion of the electroplated seed layer located in the first region and the first portion of the photoresist layer, leaving the second portion covering the bonding pad; At least one film layer is formed on the second metal layer, and the film layer is cured under baking. Remove the second portion of the photoresist layer to expose the bonding pad.
2. The method for preparing the driving substrate according to claim 1, characterized in that, Forming a patterned photoresist layer on the electroplated seed layer includes the following steps: A photoresist layer is formed on the electroplated seed layer; Expose the photoresist material layer; The photoresist material layer is developed to form an opening in the first region that exposes the electroplating seed layer; The photoresist material layer is baked to form a patterned photoresist layer, wherein the adhesion of the first part of the photoresist layer is less than the adhesion of the second part of the photoresist layer.
3. The method for preparing the driving substrate according to claim 2, characterized in that, Exposure of the photoresist material layer includes the following steps: A first light beam is used to expose the portion of the photoresist material layer located in the first region, and a second light beam is used to expose the portion of the photoresist material layer located in the second region. The light intensity of the first light beam is less than the light intensity of the second light beam, and / or the illumination time of the first light beam is less than the illumination time of the second light beam.
4. The method for preparing the driving substrate according to claim 2 or 3, characterized in that, Exposure of the photoresist material layer includes the following steps: A mask template is provided, the mask template including a plurality of first cutouts and a second cutout; The photoresist material layer is blocked by the mask template. The first cutout corresponds to the first region, and the second cutout corresponds to the second region. The second cutout exposes all areas where the bonding pads are located, so that the light intensity transmitted through the second cutout is greater than the light intensity transmitted through the first cutout.
5. The method for preparing the driving substrate according to claim 2 or 3, characterized in that, Baking the photoresist material layer includes the following steps: At a first set temperature, the portion of the photoresist material layer corresponding to the first region is baked; At a second set temperature, the portion of the photoresist layer corresponding to the second region is baked, where the first set temperature is lower than the second set temperature, so that the curing rate of the first portion of the photoresist layer is less than the curing rate of the second portion of the photoresist layer.
6. The method for preparing the driving substrate according to claim 2 or 3, characterized in that, Forming a photoresist material layer on the electroplated seed layer includes the following steps: A first photoresist layer is formed on the portion of the electroplated seed layer corresponding to the first region; A second photoresist layer is formed on the portion of the electroplated seed layer corresponding to the second region, wherein the solid content of the first photoresist layer is less than the solid content of the second photoresist layer.
7. The method for preparing the driving substrate according to any one of claims 1-3, characterized in that, Forming an electroplating seed layer on the insulating layer includes the steps of: forming a patterned electroplating seed layer on the insulating layer, wherein the electroplating seed layer only covers the first region; Forming a patterned photoresist layer on the electroplating seed layer includes the steps of: forming a patterned photoresist layer on the electroplating seed layer, wherein a first portion of the photoresist layer is disposed on the electroplating seed layer, and a second portion of the photoresist layer directly covers the bonding pad; Removing the second portion of the photoresist layer to expose the bonding pad includes the steps of: removing the second portion of the photoresist layer with a cleaning solution and cleaning the bonding pad.
8. The method for preparing a driving substrate according to any one of claims 1-3, characterized in that, Forming an electroplating seed layer on the insulating layer includes the steps of: forming a patterned electroplating seed layer on the insulating layer, the electroplating seed layer covering the first region and the second region; Forming a patterned photoresist layer on the electroplating seed layer includes the steps of: forming a patterned photoresist layer on the electroplating seed layer, wherein the photoresist layer is disposed on the electroplating seed layer; Removing the second portion of the photoresist layer to expose the bonding pad includes the steps of: removing the second portion of the photoresist layer and the electroplated seed layer corresponding to the second region, and exposing the bonding pad.
9. A method for fabricating a driving substrate, characterized in that, Includes the following steps: A substrate is provided, the substrate including a first region and a second region disposed on one side of the first region; A patterned first metal layer is formed on the substrate, the first metal layer including bonding pads disposed in the second region; An insulating layer is formed on the first metal layer, the insulating layer covering the first metal layer, and the insulating layer exposing the bonding pad; A patterned second metal layer is formed on the portion of the insulating layer corresponding to the first region; A patterned photoresist layer is formed on the second metal layer, the photoresist layer comprising a first portion located in the first region and a second portion located in the second region, the second portion covering the bonding pad; Remove the first portion of the photoresist layer, leaving the second portion covering the bonding pad; At least one film layer is formed on the second metal layer, and the film layer is cured under baking. Remove the second portion of the photoresist layer to expose the bonding pad.
10. A method for fabricating a light-emitting diode substrate, characterized in that, Includes the following steps: A substrate is provided, the substrate including a first region and a second region disposed on one side of the first region; A patterned first metal layer is formed on the substrate, the first metal layer including bonding pads disposed in the second region; An insulating layer is formed on the first metal layer, the insulating layer covering the first metal layer, and the insulating layer exposing the bonding pad; An electroplating seed layer is formed on the insulating layer, the electroplating seed layer at least covering the first region; A patterned photoresist layer is formed on the electroplating seed layer. The photoresist layer includes a first portion located in the first region and a second portion located in the second region. The second portion covers the bonding pad. An opening is provided on the first portion to expose the electroplating seed layer. A second metal layer is electroplated inside the opening; Remove the portion of the electroplated seed layer located in the first region and the first portion of the photoresist layer, leaving the second portion covering the bonding pad; Multiple film layers are formed on the second metal layer to form a driving circuit structure layer, the driving circuit structure layer including thin film transistors; Light-emitting diode devices are disposed on the drive circuit structure layer by reflow soldering. Remove the second portion of the photoresist layer to expose the bonding pad.
Citation Information
Patent Citations
Preparation method of TFE structure of novel OLED device
CN115148943A
Method for fabricating liquid crystal display device
KR1020020057088A