A method for recovering straightening bars Agt of high ductility cold-rolled ribbed steel bars

By heat treatment and insulation treatment of straightened cold-rolled ribbed steel bars at 472℃~488℃, the problem of Agt failure in the steel bar welded net was solved, and performance indicators that meet national standards were achieved.

CN117488053BActive Publication Date: 2024-11-01山东高速新材料科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311388767.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-25
Publication Date
2024-11-01
Estimated Expiration
2043-10-25

AI Technical Summary

Technical Problem

During the production process of steel bar welding mesh, the quality inspection samples taken from straightened cold-rolled ribbed steel bars often have the problem of unqualified total elongation (Agt) of maximum force (Agt), which hinders the normal production of steel bar welding mesh. .

Method used

The straightened high-ductile cold-rolled ribbed steel bars are placed in a heat treatment furnace for heat treatment, and the temperature is raised to 472℃~488℃, and the heat is kept for 3 hours. Then, it is cooled to normal temperature with the furnace. The trolley-type resistor furnace is used to provide the furnace temperature uniformity. It is ±10℃, and the temperature control accuracy is ±1℃.

Benefits of technology

Through heat treatment, the microstructure of the steel bars is changed, the grain size is refined, so that the Agt performance indicators meet the national standard requirements, and the problem of unqualified performance is solved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117488053B_ABST
    Figure CN117488053B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for recovering the straightened steel bar Agt of high ductility cold-rolled ribbed steel bars, wherein the straightened high ductility cold-rolled ribbed steel bars are placed in a heat treatment furnace for heat treatment, first heated to 472°C to 488°C, then kept warm for 3 hours, and then cooled to room temperature with the furnace. The steel bars obtained by the treatment method of the present technical solution are used for welding to make steel bar welded mesh, and the Agt performance index of the steel bar test sample can meet the national standard requirements, solving the practical problems faced in production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of steel bar processing for reinforced concrete, and in particular relates to a method for recovering a straightening bar Agt of a high-ductility cold-rolled ribbed steel bar. Background Art

[0002] The national standard GB / T 1499.3-2022 Steel for reinforced concrete Part 3 Welded steel mesh defines welded steel mesh and stipulates that the steel bars used should be: CRB550 cold-rolled ribbed steel bars and CRB600H high-ductility cold-rolled ribbed steel bars in accordance with the national standard GB / T13788; hot-rolled round steel bars in accordance with the national standard GB / T1499.1; and ribbed steel bars in accordance with the national standard BG / T1499.2. The national standard GB / T 1799.3-2022 also gives clear provisions for the performance requirements of welded steel mesh, requiring that the mechanical and process properties of welded mesh steel bars should comply with the provisions of the corresponding grades of steel bars in the corresponding standards, and the inspected samples should be cut from the finished mesh.

[0003] When cold-rolled ribbed steel bars with a diameter of less than 14 mm are used to make steel welded mesh, the raw materials used are generally coiled steel bars, which are easy to store and transport. Before welding the steel mesh, the coiled steel bars need to be straightened, and then the straightened steel bars are cut into longitudinal and transverse steel bars that meet the construction requirements, and then the longitudinal and transverse steel bars are arranged at a certain distance and welded at right angles to each other into a mesh.

[0004] The problem faced by the inventors is that the relevant properties of the purchased coiled steel bars are in compliance with the national standard GB / T13788, but when the quality inspection samples taken from the welded steel mesh are inspected for performance, the maximum force total elongation (Agt) often fails to meet the standards. This problem not only troubles the inventors, but also hinders the normal production of steel mesh. Summary of the invention

[0005] The technical problem to be solved by the present invention is to make up for the deficiencies of the prior art and provide a method for recovering the straightening bars Agt of high-ductility cold-rolled ribbed steel bars.

[0006] To solve the above technical problems, the technical solution of the present invention is:

[0007] A method for recovering straightened bars Agt of high-ductility cold-rolled ribbed steel bars comprises placing the straightened high-ductility cold-rolled ribbed steel bars in a heat treatment furnace for heat treatment, first heating the temperature to 472°C to 488°C, then keeping the temperature for 3 hours, and then cooling the steel bars to room temperature along with the furnace.

[0008] Furthermore, the temperature uniformity of the heat treatment furnace is ±10°C, and the temperature control accuracy is ±1°C.

[0009] Furthermore, the heat treatment furnace is a resistance furnace.

[0010] The beneficial effects that can be achieved by the present invention are as follows: by subjecting the straightened cold-rolled ribbed steel bars to a heat treatment of "raising the temperature to 472°C to 488°C, keeping the temperature for 3 hours, and then cooling to room temperature with the furnace", the state of lattice distortion in the microstructure of the steel bars is changed, the grain size is refined, so that the Agt performance index meets the national standard requirements, and the practical problems encountered in production are solved. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] Figure 1 It is the metallographic structure of cold-rolled ribbed steel bars in coil state.

[0012] Figure 2 It is the metallographic structure of cold-rolled ribbed steel bars after straightening.

[0013] Figure 3 It is the metallographic structure of cold rolled ribbed steel bars after heat treatment. DETAILED DESCRIPTION

[0014] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments.

[0015] A method for recovering straightening bars Agt of high-ductility cold-rolled ribbed steel bars comprises the following steps:

[0016] S1: Straighten the coiled cold-rolled ribbed steel bars by mechanical straightening. The diameter of the cold-rolled ribbed steel bars is 10 mm, which conforms to the CRB600H high ductility cold-rolled ribbed steel bars specified in the national standard GB / T13788. The relevant performance indicators are shown in Table 1 below:

[0017]

[0018] S2: Cut the straightened cold-rolled ribbed steel bars into steel bar segments that meet the construction size requirements.

[0019] S3: Place the steel bar segment in a heat treatment furnace for heat treatment: The heat treatment furnace specifically adopts a trolley-type resistance furnace with a furnace temperature uniformity of ±10°C and a temperature control accuracy of ±1°C; first heat it to 480±8°C, then keep it warm for 3h, and then cool it to room temperature along with the furnace.

[0020] The cold-rolled ribbed steel bars obtained by the above pretreatment method are arranged so that the longitudinal steel bars and the transverse steel bars are arranged at a certain interval and at right angles to each other, and all the intersections are welded together by resistance welding to form a steel welded mesh.

[0021]

[0022] It can be seen from the above that the maximum total elongation (Agt) after heat treatment is not less than 5.0, which meets the national standard requirements.

[0023] The microstructures of the cold-rolled ribbed steel bars in coiled state, the cold-rolled ribbed steel bars after straightening, and the cold-rolled ribbed steel bars after heat treatment were examined using a metallographic microscope. The magnification under the metallographic microscope was 500×, and the organizational morphologies were as follows: Figure 1 , Figure 2 , Figure 3 shown.

[0024] After the coiled steel bars are straightened, they are cold deformed, and the metallographic structure is ferrite + pearlite. Compared with before straightening, slip and dislocation occur between the grains, the shape of the grains changes, there are elongation and flattening phenomena, and there is longitudinal fiberization. The lattice distortion increases the slip resistance, and the plastic deformation resistance of the metal increases, that is, the strength and hardness are slightly improved, and the plasticity and toughness are significantly reduced, which makes the Agt performance index decrease and produces work hardening phenomenon.

[0025] The metallographic structure of the steel bar after heat treatment is ferrite + pearlite structure. Compared with the steel bar after straightening and before heat treatment, the optical microstructure has not changed significantly, reorganization has occurred between the grains, the grain shape has changed, there is a recovery phenomenon, and the grain size has been refined, so that the Agt performance indicators meet the national standard requirements.

Claims

1. A method for recovering straightening bars Agt of high ductility cold-rolled ribbed steel bars, characterized by: The straightened high ductility cold-rolled ribbed steel bars are placed in a heat treatment furnace for heat treatment, first heated to 472°C to 488°C, then kept warm for 3 hours, and then cooled to room temperature along with the furnace; The temperature uniformity of the heat treatment furnace is ±10°C, and the temperature control accuracy is ±1°C; The heat treatment furnace is a resistance furnace.