Resin composition, resin sheet, multilayer printed circuit board, and semiconductor device

By combining specific maleimide compounds and photocuring initiators, the problems of poor light transmittance and insufficient developability in existing technologies have been solved, enabling the manufacture of high-precision, high-density printed circuit boards and semiconductor devices with excellent photocurability and alkaline developability.

CN117500850BActive Publication Date: 2026-11-10MITSUBISHI GAS CHEM CO INC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202280042795.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-06-15
Filing Date
2022-06-14
Publication Date
2026-11-10
Estimated Expiration
2042-06-14

AI Technical Summary

Technical Problem

In the prior art, when using bismaleimide compounds as curing resins, the light transmittance is poor, which means that light cannot fully reach the photocuring initiator, resulting in low reactivity. Furthermore, heat curing is required before development, making it impossible to manufacture high-density printed circuit boards with high-precision resist patterns.

Method used

By employing a specific combination of maleimide compounds and photocuring initiators, including maleimide compounds and oxime ester compounds containing specific structural units, with an absorbance of 2.0 or higher, and in conjunction with compounds containing carboxyl groups, it is used for photocuring of 365nm i-rays in the exposure process and for alkaline development in the development process, forming a high-precision resist pattern.

Benefits of technology

It achieves excellent photocurability for 365nm i-rays in the exposure process and excellent alkaline developability in the development process, enabling the manufacture of high-precision, high-density printed circuit boards and semiconductor devices, and possesses excellent photocurability, alkaline developability, and thermal stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117500850B_ABST
    Figure CN117500850B_ABST
Patent Text Reader

Abstract

The present invention provides a resin composition and a resin sheet having excellent photocurability for active energy rays including i-rays of wavelength 365 nm in an exposure step, and being capable of imparting excellent alkali developability in a development step, at the time of manufacturing a multilayer printed circuit board, and a high-density printed circuit board and a semiconductor device having a high-fineness resist pattern by using them. The resin composition of the present invention comprises a maleimide compound (A) comprising a structural unit represented by the following formula (1) and maleimide groups at both terminals of a molecular chain, and a photocuring initiator (B) having an absorbance of 2.0 or more at wavelength 365 nm (i-rays).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to resin compositions, resin sheets, multilayer printed circuit boards, and semiconductor devices. Background Technology

[0002] Due to the miniaturization and high density of multilayer printed circuit boards (PCBs), research is actively underway to reduce the thickness of the laminates used in multilayer PCBs. Along with this thinning, there is also a demand for thinner insulating layers, leading to the search for resin sheets that do not contain glass cloth. Regarding the resin compositions used as insulating layers, thermosetting resins are the mainstream choice, and the openings used to create conductivity between insulating layers are typically achieved through laser processing.

[0003] On the other hand, laser-processed openings have the following problems: the more holes a high-density substrate has, the longer the processing time becomes. Therefore, in recent years, there has been a demand for resin sheets that use a resin composition that can cure the exposed areas (exposure process) and remove the unexposed areas (development process) by irradiation with light or the like, thereby enabling opening processing to be performed in one step through the exposure and development processes.

[0004] As an exposure method, a method using a mercury lamp as the light source and exposing the material through a photomask is employed, requiring materials that can be appropriately exposed under the mercury lamp's light source. This mercury lamp-based exposure method uses a mixture of g-rays (gamma rays with a wavelength of 436 nm, h-rays with a wavelength of 405 nm, and i-rays with a wavelength of 365 nm), and a generally applicable photocuring initiator can be selected. Furthermore, in recent years, to obtain more refined patterns, exposure methods using i-rays (wavelength 365 nm), which have less color difference compared to gamma rays, have been introduced.

[0005] As a developing method, alkaline development was used to obtain highly detailed patterns.

[0006] Patent Document 1 describes a resin composition comprising a bismaleimide compound (curable resin) and a photoradical polymerization initiator (curing agent) as a photosensitive resin composition used in laminates and resin sheets.

[0007] Existing technical documents

[0008] Patent documents

[0009] Patent Document 1: WO2018 / 56466A1 Summary of the Invention

[0010] The problem the invention aims to solve

[0011] However, Patent Document 1 uses a bismaleimide compound as the curing resin. Maleimide compounds typically have poor light transmittance, so if they are included, light cannot sufficiently reach the photocuring initiator, making it difficult for the initiator to generate free radicals, resulting in very low reactivity. Furthermore, Patent Document 1 makes no mention of a light source capable of irradiating with active energy rays containing 365nm (i-rays). Moreover, in Patent Document 1, when using active energy rays containing 365nm i-rays for photocuring, the low i-ray transmittance of the maleimide compound leads to low curing degree. Therefore, Patent Document 1 cures the maleimide compound by additional heating before development; however, due to the accompanying heating, a high-precision resist pattern cannot be obtained. Additionally, the resin composition described in Patent Document 1 originally has insufficient alkaline developability, leaving unexposed resin composition after development. Therefore, from this perspective, Patent Document 1 also fails to produce a high-precision resist pattern and cannot be used to manufacture high-density printed circuit boards.

[0012] The present invention was made in view of the problems of the prior art, and provides resin compositions and resin sheets that have excellent photocurability to active energy rays including i-rays with a wavelength of 365 nm in the exposure process during the fabrication of multilayer printed circuit boards, and can impart excellent alkaline developability in the development process, as well as high-density printed circuit boards and semiconductor devices with high-fine resist patterns by using them.

[0013] Solution for solving the problem

[0014] The inventors conducted in-depth research and found that resin compositions and resin sheets containing specific maleimide compounds (A) and specific photocuring initiators (B) exhibit excellent photocurability to active energy rays containing i-rays with a wavelength of 365 nm during the exposure process of manufacturing multilayer printed circuit boards, and can impart excellent alkaline developability during the development process. By using them, high-density printed circuit boards and semiconductor devices with fine resist patterns can be obtained, thereby completing the present invention.

[0015] That is, the present invention includes the following contents.

[0016] [1] A resin composition comprising a maleimide compound (A) and a photocurable initiator (B), wherein the maleimide compound (A) comprises a structural unit as shown in formula (1) and maleimide groups located at both ends of the molecular chain, and the photocurable initiator (B) has an absorbance of 2.0 or more at a wavelength of 365 nm (i-ray).

[0017]

[0018] (In formula (1), R1 represents a straight-chain or branched alkylene group having 1 to 16 carbon atoms, or a straight-chain or branched alkenyl group having 2 to 16 carbon atoms. R2 represents a straight-chain or branched alkylene group having 1 to 16 carbon atoms, or a straight-chain or branched alkenyl group having 2 to 16 carbon atoms. R3 each independently represents a hydrogen atom, a straight-chain or branched alkyl group having 1 to 16 carbon atoms, or a straight-chain or branched alkenyl group having 2 to 16 carbon atoms. n1 each independently represents an integer from 1 to 10.)

[0019] [2] The resin composition according to [1], wherein the aforementioned photocuring initiator (B) comprises an oxime ester compound.

[0020] [3] The resin composition according to [1] or [2], wherein the aforementioned photocuring initiator (B) comprises the photocuring initiator (B1) shown in formula (2) below and / or the photocuring initiator (B2) shown in formula (3) below.

[0021]

[0022] (In formula (2), R4 represents acetyl or benzoyl. R5 represents phenyl or naphthyl, optionally with a substituent. R6 represents a hydrogen atom, or an alkyl group having 1 to 16 carbon atoms, either straight-chain or branched. R7 each independently represents a hydrogen atom, or an alkyl group having 1 to 6 carbon atoms, either straight-chain or branched. n2 each independently represents an integer from 1 to 5.)

[0023]

[0024] In formula (3), R8 represents an aryl group with 6 to 24 carbon atoms that may be substituted, or a heteroaryl group with 3 to 24 carbon atoms that may be substituted. R9 represents an acetyl group or a benzoyl group. 10 Represents a hydrogen atom, or an alkyl group having 1 to 16 carbon atoms (optionally with substituents) in a straight or branched form. X represents an oxygen atom or a sulfur atom.

[0025] [4] The resin composition according to any one of [1] to [3] further comprises: a compound (C) containing one or more carboxyl groups.

[0026] [5] The resin composition according to [4], wherein the aforementioned compound (C) containing one or more carboxyl groups comprises the compound shown in the following formula (4).

[0027]

[0028] (In equation (4), R) 11Each of these independently represents a group or hydrogen atom as shown in formula (5) below. R 12 Each alkyl group independently represents a hydrogen atom or a straight-chain or branched alkyl group having 1 to 6 carbon atoms. At least one R is present. 11 The group is represented by the formula (5) below.

[0029]

[0030] (In equation (5), -* represents an atomic bond.)

[0031] [6] The resin composition according to any one of [1] to [5] further comprises at least one maleimide compound (D) selected from the group consisting of the compound shown in formula (6), the compound shown in formula (7), the compound shown in formula (8), the compound shown in formula (9), the compound shown in formula (10), and the compound shown in formula (11).

[0032]

[0033] (In equation (6), R) 13 R 14 and R 15 Each can independently represent a hydrogen atom, or optionally a straight-chain or branched alkyl group having 1 to 8 carbon atoms and substituents.

[0034]

[0035] (In equation (7), R) 16 R 17 and R 18 Each group independently represents a hydrogen atom, a hydroxyl group, or an alkyl group with 1 to 6 carbon atoms that may be substituented, either straight-chain or branched. n2 represents an integer from 1 to 10.

[0036]

[0037] (In equation (8), R) 19 Each can independently represent a hydrogen atom, a methyl group, or an ethyl group. R 20 Each can independently represent a hydrogen atom or a methyl group.

[0038]

[0039] (In equation (9), R) 21 Each can independently represent a hydrogen atom or a methyl group. n3 represents an integer from 1 to 10.

[0040]

[0041] (In equation (10), R)22 Each can independently represent a hydrogen atom, a methyl group, or an ethyl group.

[0042]

[0043] (In equation (11), R) 23 Each can independently represent a hydrogen atom or a methyl group. n4 represents an integer from 1 to 10.

[0044] [7] A resin sheet having a support and a resin layer disposed on one or both sides of the support, the resin layer comprising any one of [1] to [6].

[0045] [8] The resin sheet according to [7], wherein the thickness of the aforementioned resin layer is 1 to 50 μm.

[0046] [9] A multilayer printed circuit board having an insulating layer and a conductor layer formed on one or both sides of the insulating layer, wherein the insulating layer comprises any one of [1] to [6].

[0047]

[10] A semiconductor device comprising any one of the resin compositions described in [1] to [6].

[0048] The effects of the invention

[0049] According to the present invention, a high-density printed circuit board and semiconductor device can be provided that exhibits excellent photocurability to active energy rays containing i-rays with a wavelength of 365 nm in the exposure process of manufacturing multilayer printed circuit boards and can impart excellent alkaline developability in the development process, thereby having a high-precision resist pattern. Attached Figure Description

[0050] Figure 1 It is the photocuring initiator (B1A) obtained in Synthesis Example 1. 1 1H-NMR spectrum.

[0051] Figure 2 It is the photocuring initiator (B2A) obtained in Synthesis Example 2. 1 1H-NMR spectrum.

[0052] Figure 3 It is an amyl acid compound (MA-TMDA) 1 1H-NMR spectrum.

[0053] Figure 4 It is a maleimide compound (TMDM) 1 1H-NMR spectrum.

[0054] Figure 5It is the compound (C1) obtained in Synthesis Example 4. 1 1H-NMR spectrum. Detailed Implementation

[0055] Hereinafter, a method for carrying out the present invention (hereinafter referred to as "this embodiment") will be described in detail. This embodiment is merely an example for illustrating the present invention and is not intended to limit the invention to its contents. The present invention can be implemented with appropriate modifications within the scope of its spirit.

[0056] It should be noted that "(meth)acrylic acid" in this specification refers to both "acrylic acid" and its corresponding "methacrylic acid". Furthermore, in this specification, "resin solids" or "resin solids in the resin composition" refers to the components in the resin composition other than photocuring initiator (B), photocuring initiator (b), compounds containing one or more carboxyl groups (C), additives, solvents, and fillers, unless otherwise specified. "100 parts by weight of resin solids" means that the total amount of components in the resin composition other than photocuring initiator (B), photocuring initiator (b), compounds containing one or more carboxyl groups (C), additives, solvents, and fillers is 100 parts by weight.

[0057] In this specification, Mw represents the mass-average molecular weight, Mn represents the number-average molecular weight, and Mw / Mn represents the molecular weight distribution. Mw, Mn, and Mw / Mn can be determined by gel permeation chromatography (GPC) using polystyrene standards.

[0058] [Resin Composition]

[0059] The resin composition of this embodiment comprises a maleimide compound (A) (also referred to as component (A) or bismaleimide compound (A)) and a photocurable initiator (B) (also referred to as component (B) or initiator (B)). The maleimide compound (A) comprises the structural unit shown in formula (1) and maleimide groups located at both ends of the molecular chain. The photocurable initiator (B) has an absorbance of 2.0 or higher at a wavelength of 365 nm (i-rays). The resin composition of this embodiment, comprising compound (A) and compound (B), is suitable for fabricating multilayer printed circuit boards. By using the resin composition, excellent photocurability is achieved for active energy rays containing i-rays at a wavelength of 365 nm during the exposure process of fabricating multilayer printed circuit boards, and excellent alkaline developability is imparted during the development process.

[0060] [Bismaleimide compound (A)]

[0061] The resin composition of this embodiment contains a maleimide compound (A), which contains the structural unit shown in formula (1) and maleimide groups located at both ends of the molecular chain.

[0062]

[0063] In formula (1), R1 represents a straight-chain or branched alkylene group having 1 to 16 carbon atoms, or a straight-chain or branched alkenyl group having 2 to 16 carbon atoms. R2 represents a straight-chain or branched alkylene group having 1 to 16 carbon atoms, or a straight-chain or branched alkenyl group having 2 to 16 carbon atoms. R3 independently represents a hydrogen atom, a straight-chain or branched alkyl group having 1 to 16 carbon atoms, or a straight-chain or branched alkenyl group having 2 to 16 carbon atoms. n1 independently represents an integer from 1 to 10.

[0064] The inventors speculate that the resin composition exhibits excellent photocurability to active energy rays (light rays) containing i-rays with a wavelength of 365 nm by including both the photocuring initiator (B) described later and the bismaleimide compound (A) for the following reasons.

[0065] Typically, maleimide compounds have poor light transmittance. Therefore, if a resin composition contains maleimide compounds, light cannot sufficiently reach the photocuring initiator dispersed in the resin composition, making it difficult for the photocuring initiator to generate free radicals. Consequently, photoradical reactions of maleimide compounds are usually difficult to occur, and even if free radical polymerization and dimerization reactions of maleimide monomers occur, their reactivity is very low.

[0066] However, the bismaleimide compound (A) has the structural unit shown in formula (1), namely the alicyclic skeleton, and therefore exhibits excellent light transmittance. When a chloroform solution containing 1% by mass of the bismaleimide compound (A) is prepared, and the transmittance of the chloroform solution containing 1% by mass of the bismaleimide compound (A) is measured using active energy rays containing a wavelength of 365 nm (i-rays), the transmittance is 5% or more, demonstrating very excellent light transmittance. From the viewpoint of exhibiting even better light transmittance, the transmittance at a wavelength of 365 nm (i-rays) is preferably 8% or more, more preferably 10% or more. The upper limit of the transmittance at a wavelength of 365 nm (i-rays) is, for example, 99.9% or less.

[0067] On the other hand, photocuring initiators typically exhibit a tendency to decrease absorbance when exposed to active energy rays containing wavelengths of 365 nm (i-rays). Therefore, conventional photocuring initiators do not absorb this light, and polymerization will not occur unless a photocuring initiator capable of appropriately absorbing this light and generating free radicals is used. In this regard, when measuring the absorbance of a chloroform solution containing 0.01% by mass of photocuring initiator (B), the photocuring initiator (B) showed an absorbance of over 2.0 for light at a wavelength of 365 nm (i-rays), indicating a very high absorbance.

[0068] In summary, by using a bismaleimide compound (A) to ensure sufficient light reaches the photocuring initiator, and by using a photocuring initiator (B) capable of generating free radicals by absorbing active energy rays containing a wavelength of 365 nm (i-rays), a photoradical reaction of maleimide can also occur effectively in a composition containing a large amount of bismaleimide compound (A). Therefore, by using bismaleimide compound (A), photocuring initiator (B), a compound (C) containing one or more carboxyl groups (hereinafter referred to as component (C) or compound (C)), and a maleimide compound (D) (hereinafter referred to as component (D) or compound (D)), and using active energy rays containing a wavelength of 365 nm (i-rays), photocuring can occur, and printed circuit boards with high-density and high-fine wiring formation (patterning) can be suitable for manufacturing.

[0069] Furthermore, maleimide compounds typically have extremely low water solubility and are not reactive with the alkaline components in alkaline developers, making it difficult to achieve alkaline developability. However, the resin composition, by containing a bismaleimide compound (A), exhibits excellent photocurability and very good alkaline developability. The reason for this is not yet certain, but the inventors speculate as follows.

[0070] That is, bismaleimide compound (A) has a relatively long chain and a flexible structure, and therefore does not have a structure that would allow it to interact with the alkaline components in the alkaline developer. Therefore, bismaleimide compound (A) can dissolve in the alkaline developer while retaining the structure of other components such as compound (C), for example, as it dissolves in the alkaline developer. Therefore, it is speculated that even if the alkaline developer flows into the unexposed portion (resin composition) during the developing process, bismaleimide compound (A) will not prevent it from reacting with the alkaline components in the alkaline developer, and the resin composition will exhibit excellent alkaline developability.

[0071] Therefore, the resin composition of this embodiment exhibits excellent photocurability to active energy rays including 365nm (i-rays) during the exposure process of manufacturing multilayer printed circuit boards, and can impart excellent alkaline developability during the development process. Thus, high-density printed circuit boards and semiconductor devices with highly fine resist patterns can be obtained. Furthermore, the resulting cured product also exhibits excellent heat resistance, insulation reliability, and thermal stability. Therefore, according to this embodiment, protective films and insulating layers in multilayer printed circuit boards and semiconductor devices can be suitably formed.

[0072] The bismaleimide compound (A) is not particularly limited as long as it achieves the effects of the present invention. From the viewpoint of obtaining a suitable viscosity and being able to suppress the increase of viscosity of the varnish, the mass-average molecular weight is preferably 100 to 5000, more preferably 300 to 4500.

[0073] Next, the structure of the bismaleimide compound (A) will be described.

[0074] In formula (1) of the bismaleimide compound (A), R1 represents a straight-chain or branched alkylene group having 1 to 16 carbon atoms, or a straight-chain or branched alkenyl group having 2 to 16 carbon atoms. From the viewpoint of obtaining a more suitable viscosity and further suppressing the increase in viscosity of the varnish, a straight-chain or branched alkylene group is preferred as R1, and a straight-chain alkylene group is more preferred.

[0075] From the viewpoint that a more suitable viscosity can be obtained and the viscosity increase of the varnish can be further suppressed, the number of carbon atoms in the alkylene group is preferably 2 to 14, and more preferably 4 to 12.

[0076] Examples of linear or branched alkylene compounds include methylene, ethylene, propylene, 2,2-dimethylpropylene, butylene, pentylene, hexylene, heptylene, octylene, nonylene, decylene, dodecylene, undecylene, tridecylene, tetradecylene, pentadecylene, hexadecylene, neopentylene, dimethylbutylene, methylhexylene, ethylhexylene, dimethylhexylene, trimethylhexylene, methylheptylene, dimethylheptylene, trimethylheptylene, tetramethylheptylene, ethylheptylene, methyloctylene, methylnonylene, methyldecylene, methyl dodecylene, methyl undecylene, methyl tridecylene, methyl tetradecylene, and methyl pentadecylene.

[0077] From the viewpoint that a more suitable viscosity can be obtained and the viscosity increase of the varnish can be further suppressed, the number of carbon atoms in the subalkenyl group is preferably 2 to 14, more preferably 4 to 12.

[0078] Examples of straight-chain or branched alkenyl groups include vinylidene, 1-methylvinylidene, allylidene, propenylidene, isopropenylidene, 1-butenylidene, 2-butenylidene, 1-pentenylidene, 2-pentenylidene, isopentylidene, cyclopentenylidene, cyclohexenylidene, and dicyclopentadienylidene.

[0079] In formula (1), R2 represents a linear or branched alkylene group having 1 to 16 carbon atoms, or a linear or branched alkenyl group having 2 to 16 carbon atoms. From the viewpoint that a more suitable viscosity can be obtained and the viscosity increase of the varnish can be further suppressed, a linear or branched alkylene group is preferred as R2, and a linear alkylene group is more preferred.

[0080] From the viewpoint that a more suitable viscosity can be obtained and the viscosity increase of the varnish can be further suppressed, the number of carbon atoms in the alkylene group is preferably 2 to 14, and more preferably 4 to 12.

[0081] As a linear or branched alkylene group, refer to R1 mentioned above.

[0082] From the viewpoint that a more suitable viscosity can be obtained and the viscosity increase of the varnish can be further suppressed, the number of carbon atoms in the subalkenyl group is preferably 2 to 14, more preferably 4 to 12.

[0083] As a linear or branched alkenyl group, refer to R1 mentioned above.

[0084] In formula (1), R1 and R2 can be the same or different, but from the viewpoint that it is easier to synthesize bismaleimide compound (A), it is preferred to be the same.

[0085] In formula (1), each of R3 independently represents a hydrogen atom, a straight-chain or branched alkyl group having 1 to 16 carbon atoms, or a straight-chain or branched alkenyl group having 2 to 16 carbon atoms. From the viewpoint of obtaining a more suitable viscosity and being able to further suppress the increase in viscosity of the varnish, it is preferable that each of R3 is a hydrogen atom or a straight-chain or branched alkyl group having 1 to 16 carbon atoms, more preferably that 1 to 5 of the R3 groups (R3) are straight-chain or branched alkyl groups having 1 to 16 carbon atoms, and the remaining groups (R3) are hydrogen atoms, and even more preferably that 1 to 3 of the R3 groups (R3) are straight-chain or branched alkyl groups having 1 to 16 carbon atoms, and the remaining groups (R3) are hydrogen atoms.

[0086] From the viewpoint that a more suitable viscosity can be obtained and the viscosity increase of the varnish can be further suppressed, the number of carbon atoms of the alkyl group is preferably 2 to 14, more preferably 4 to 12.

[0087] Examples of linear or branched alkyl groups include methyl, ethyl, n-propyl, isopropyl, 1-ethylpropyl, n-butyl, 2-butyl, isobutyl, tert-butyl, n-pentyl, 2-pentyl, tert-pentyl, 2-methylbutyl, 3-methylbutyl, 2,2-dimethylpropyl, n-hexyl, 2-hexyl, 3-hexyl, n-heptyl, n-octyl, 2-methylpentyl, 3-methylpentyl, 4-methylpentyl, 2-methylpent-3-yl, and n-nonyl.

[0088] From the viewpoint that a more suitable viscosity can be obtained and the viscosity increase of the varnish can be further suppressed, the number of carbon atoms in the alkenyl group is preferably 2 to 14, more preferably 4 to 12.

[0089] Examples of alkenyl groups that can be straight-chain or branched include vinyl, allyl, 4-pentenyl, isopropenyl, isopentenyl, 2-heptenyl, 2-octenyl, and 2-nonenyl.

[0090] In equation (1), n1 independently represents integers from 1 to 10.

[0091] The bismaleimide compound (A) has maleimide groups at both ends of its molecular chain. "Both ends" refers to the two ends of the molecular chain of the bismaleimide compound (A). For example, in the case where the structural unit shown in formula (1) is located at the end of the molecular chain of the bismaleimide compound (A), it means that a maleimide group is present at the end of the molecular chain of R1, or at the end of the molecular chain on the N atom of the maleimide ring, or at both ends. The bismaleimide compound (A) may also have maleimide groups at positions other than the two ends of the molecular chain.

[0092] The maleimide group is represented by formula (12), where the N atom is bonded to the molecular chain of the bismaleimide compound (A). Furthermore, the maleimide groups bonded to the bismaleimide compound (A) may be all the same or different, but preferably the maleimide groups at both ends of the molecular chain are the same.

[0093]

[0094] In equation (12), R 24 Each R independently represents a hydrogen atom or a straight-chain or branched alkyl group having 1 to 4 carbon atoms. From the viewpoint of more suitable photocuring, two Rs are preferred. 24 All are hydrogen atoms.

[0095] From the viewpoint that the number of carbon atoms in the alkyl group is more suitable for photocuring, it is preferably 1 to 3, and more preferably 1 to 2.

[0096] As for straight-chain or branched alkyl groups, refer to R3 above.

[0097] Examples of such bismaleimide compounds (A) include maleimide compounds represented by formula (13). They can be used alone or in combination of two or more.

[0098]

[0099] In equation (13), a represents an integer from 1 to 10. From the viewpoint of obtaining a more suitable viscosity and further controlling the viscosity rise of the varnish, a is preferably an integer from 1 to 6.

[0100] Bismaleimide compound (A) can also be commercially available. Examples of commercially available products include MIZ-001 (trade name, containing maleimide compound of formula (13)) manufactured by Nippon Kayaku Co., Ltd.

[0101] From the viewpoint that a cured product with bismaleimide compound as the main component can be obtained, that photocurability can be further improved, and that better heat resistance and thermal stability can be obtained, the content of bismaleimide compound (A) in the resin composition is preferably 10 to 90 parts by mass, more preferably 30 to 80 parts by mass, and even more preferably 40 to 70 parts by mass in 100 parts by mass of resin solids in the resin composition.

[0102] Furthermore, when the resin composition contains bismaleimide compound (A) and maleimide compound (D) other than bismaleimide compound (A), from the viewpoint that a cured product with bismaleimide compound as the main component can be obtained, that photocurability can be further improved, and that better heat resistance and thermal stability can be obtained, the content of bismaleimide compound (A) is preferably 10 to 90 parts by mass relative to 100 parts by mass of the total of bismaleimide compound (A) and maleimide compound (D), more preferably 30 to 80 parts by mass, and even more preferably 40 to 70 parts by mass. As the maleimide compound (D), it is preferred to include at least one of the compounds selected from the group consisting of the compound shown in (6), the compound shown in (7), the compound shown in (8), the compound shown in (9), the compound shown in (10), and the compound shown in (11), more preferably including at least one of the compounds selected from the group consisting of the compound shown in (6), the compound shown in (7), and the compound shown in (8), further preferably including at least one of the compounds selected from the group consisting of the compound shown in (6) and the compound shown in (7), and even more preferably including the compound shown in (7).

[0103] When the resin composition contains bismaleimide compound (A) and initiator (B), and also contains compounds (C) and (D), from the perspective of imparting better alkali developability and exhibiting better curability due to the uninhibited photocuring initiator in the resin composition, the content of bismaleimide compound (A) relative to 100 parts by mass of the total of bismaleimide compound (A), initiator (B), compound (C) and compound (D) is preferably 10 to 85 parts by mass, more preferably 15 to 80 parts by mass, further preferably 40 to 75 parts by mass, and even more preferably 45 to 70 parts by mass.

[0104] Bismaleimide compound (A) can be used alone or in appropriate combinations of two or more.

[0105] (Method for manufacturing bismaleimide compound (A))

[0106] The bismaleimide compound (A) can be manufactured by known methods. For example, 1,2,4,5-cyclohexanetetracarboxylic acid dianhydride, a monomer containing a diamine such as a dimerizing diamine, and maleic anhydride are subjected to an addition polymerization reaction at a temperature typically around 80–250°C, preferably around 100–200°C, for typically 0.5–50 hours, preferably 1–20 hours, to obtain an addition polymer. Then, the addition polymer is subjected to an imidization reaction, i.e., a dehydration and ring-closing reaction, at a temperature typically around 60–120°C, preferably around 80–100°C, for typically 0.1–2 hours, preferably 0.1–0.5 hours, to obtain the bismaleimide compound (A).

[0107] Dimeric diamines are obtained, for example, by the reductive amination reaction of dimer acids. The amination reaction can be carried out by known methods, such as reduction using ammonia and a catalyst (e.g., the method described in Japanese Patent Application Publication No. 9-12712). Dimeric acids refer to diacids obtained by dimerizing unsaturated fatty acids through intermolecular polymerization reactions. While dependent on synthesis and purification conditions, they typically include small amounts of monomeric acids, trimer acids, etc., in addition to dimer acids. The resulting molecule may retain intramolecular double bonds; however, in this embodiment, substances that reduce intramolecular double bonds to become saturated diacids through hydrogenation reactions are also included within the category of dimer acids. Dimeric acids are obtained by polymerizing unsaturated fatty acids, for example, using Lewis acids and Brønsted acids as catalysts. Dimeric acids can be manufactured by known methods (e.g., the method described in Japanese Patent Application Publication No. 9-12712). Examples of unsaturated fatty acids include crotonic acid, myristoleic acid, palmitoleic acid, oleic acid, transoleic acid, vaccenic acid, gadooleic acid, eicosapentaenoic acid, erucic acid, nervonic acid, linoleic acid, pinolenic acid, tung oil acid, meadacid, dihyo-γ-linolenic acid, eicosatrienoic acid, stearidonicacid, arachidonic acid, eicosatetraenoic acid, adrenal acid, 5Z,8Z,10E,12E,14Z-eicosapentaenoic acid, osbond acid, clupatanodonic acid, docosahexaenoic acid, and nisinic acid. Unsaturated fatty acids typically have 4 to 24 carbon atoms, preferably 14 to 20.

[0108] In the manufacture of the bismaleimide compound (A), it is preferable to first dissolve or disperse the monomer containing the diamine in an organic solvent in a slurry under an inactive atmosphere such as argon or nitrogen to prepare a monomer solution containing the diamine. Furthermore, 1,2,4,5-cyclohexanetetracarboxylic dianhydride is preferably added to the above-mentioned monomer solution containing the diamine after being dissolved or dispersed in an organic solvent in a slurry or in a solid state.

[0109] By adjusting the molar amounts of 1,2,4,5-cyclohexanetetracarboxylic dianhydride and the total molar amounts of the monomer containing the diamine and the maleimide compound, any bismaleimide compound (A) can be obtained.

[0110] In addition polymerization and imidization reactions, a variety of known solvents can be used. Examples of solvents include amides such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methyl-2-pyrrolidone; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, and isophorone; esters such as γ-butyrolactone, γ-valerolactone, δ-valerolactone, γ-caprolactone, ε-caprolactone, α-methyl-γ-butyrolactone, ethyl lactate, methyl acetate, ethyl acetate, and butyl acetate; and aliphatic alcohols with 1 to 10 carbon atoms such as methanol, ethanol, and propanol. Phenolic solvents containing aromatic groups, such as phenol and cresol; alcohols containing aromatic groups, such as benzyl alcohol; diols, such as ethylene glycol and propylene glycol, or diol ethers of these diols with methanol, ethanol, butanol, hexanol, octanol, benzyl alcohol, phenol, and cresol, or esters of these diol ethers; cyclic ethers, such as dioxane and tetrahydrofuran; carbonates, such as ethylene carbonate and propylene carbonate; aliphatic hydrocarbons and aromatic hydrocarbons, such as toluene and xylene; and aprotic polar solvents, such as dimethyl sulfoxide. One of these solvents may be used alone or in combination of two or more, as needed.

[0111] Furthermore, a catalyst is preferably used in the imidization reaction. Examples of catalysts include tertiary amines and dehydration catalysts. Heterocyclic tertiary amines are preferred, such as pyridine, methylpyridine, quinoline, and isoquinoline. Examples of dehydration catalysts include acetic anhydride, propionic anhydride, n-butyric anhydride, benzoic anhydride, and trifluoroacetic anhydride.

[0112] Regarding the amount of catalyst added, it is preferred that, for example, the imidizing agent is set to about 0.5 to 5.0 molar equivalents relative to the amide group, and the dehydration catalyst is set to 0.5 to 10.0 molar equivalents relative to the amide group.

[0113] After the imidization reaction is complete, the solution can be used as a solution of bismaleimide compound (A), or a poor solvent can be added to the reaction solvent to form a solid substance of bismaleimide compound (A). Examples of poor solvents include water, methanol, ethanol, 2-propanol, ethylene glycol, triethylene glycol, 2-butanol, 2-pentanol, 2-hexanol, cyclopentanol, cyclohexanol, phenol, and tert-butanol.

[0114] [Photocuring Initiator (B)]

[0115] The resin composition of this embodiment includes a photocurable initiator (B) (also referred to as component (B) or initiator (B)), wherein the photocurable initiator (B) has an absorbance of 2.0 or higher at a wavelength of 365 nm (i-rays). The photocurable initiator (B) is not particularly limited as long as the absorbance at a wavelength of 365 nm (i-rays) is 2.0 or higher, and substances generally known in the field of photocurable resin compositions can be used. The photocurable initiator (B) is used to photocur with a bismaleimide compound (A) and, as needed, compounds (C) and (D), using an active energy ray (light) containing a wavelength of 365 nm (i-rays). One photocurable initiator (B) can be used alone or two or more can be used in appropriate mixtures.

[0116] A chloroform solution containing 0.01% by mass of photocurable initiator (B) was prepared. When the absorbance of the chloroform solution containing 0.01% by mass of photocurable initiator (B) was measured using active energy rays with a wavelength of 365 nm (i-rays), the absorbance was 2.0 or higher, indicating that the photocurable initiator (B) exhibited very high absorbance. By using this photocurable initiator (B), the free radical reaction of the bismaleimide compound (A) can be effectively induced, enabling photocuring and the manufacture of printed circuit boards with high-density and high-fine wiring formation (patterning). It should be noted that, from the perspective of obtaining a resin composition with superior photocurability, the absorbance at a wavelength of 365 nm (i-rays) is preferably 2.5 or higher, more preferably 3.0 or higher, and even more preferably 3.5 or higher. The upper limit of the absorbance at a wavelength of 365 nm (i-rays) is, for example, 99.9 or lower.

[0117] From the viewpoint of enabling the resin composition to be photocured more fully without hindering the photocuring reaction and to make the exposed portion more insoluble in terms of alkali developability, the content of photocuring initiator (B) in 100 parts by weight of the resin solids in the resin composition is preferably 0.1 to 50 parts by weight, more preferably 0.2 to 30 parts by weight, and even more preferably 0.3 to 10 parts by weight.

[0118] Furthermore, when the resin composition contains both bismaleimide compound (A) and compounds (C) and (D), from the viewpoint of enabling the resin composition to be photocured more fully without hindering the photocuring reaction and to make the exposed portion more insoluble in terms of alkali developability, the content of photocuring initiator (B) is preferably 0.1 to 20 parts by mass relative to a total of 100 parts by mass of bismaleimide compound (A), initiator (B), compound (C), and compound (D), more preferably 0.15 to 15 parts by mass, further preferably 0.2 to 13 parts by mass, and even more preferably 0.5 to 10 parts by mass.

[0119] From the viewpoint of high sensitivity to i-rays, oxime esters are preferred as photocuring initiators (B). Furthermore, from the viewpoint of even higher sensitivity to i-rays and better solvent solubility, photocuring initiators (B1) shown in formula (2) and / or photocuring initiators (B2) shown in formula (3) are more preferred as oxime esters.

[0120] The inventors speculate that by including both the photocurable initiator (B1) of formula (2) and the photocurable initiator (B2) of formula (3) along with the bismaleimide compound (A), the resin composition exhibits superior photocurability to active energy rays (light rays) containing i-rays with a wavelength of 365 nm due to the following reasons: The photocurable initiator (B1) of formula (2) and the photocurable initiator (B2) of formula (3) have superior compatibility with the bismaleimide compound (A). Furthermore, the photocurable initiators (B1) and (B2) have higher absorbance to active energy rays containing i-rays with a wavelength of 365 nm, thus making it easier to generate active free radicals by absorbing i-rays. Therefore, it can be speculated that during the exposure process, by irradiating with active energy rays containing i-rays, active free radicals are rapidly generated by the photocurable initiators (B1) and (B2), which rapidly initiate a reaction with the bismaleimide compound (A), thus exhibiting superior photocurability.

[0121] Therefore, the resin composition exhibits superior photocurability to active energy rays including 365nm (i-rays) during the exposure process of manufacturing multilayer printed circuit boards, and can impart superior alkaline developability during the development process. Thus, high-density printed circuit boards and semiconductor devices with finer resist patterns can be obtained. Furthermore, the resulting cured product also exhibits superior heat resistance, insulation reliability, and thermal stability. Therefore, according to this embodiment, protective films and insulating layers in multilayer printed circuit boards and semiconductor devices can be more suitable for formation.

[0122] Next, the photocuring initiator (B1) shown in formula (2) and the photocuring initiator (B2) shown in formula (3) will be described.

[0123] (The photocuring initiator (B1) shown in formula (2))

[0124] The photocuring initiator (B1) shown in formula (2) is the following compound.

[0125]

[0126] In formula (2), R4 represents acetyl or benzoyl. Acetyl is preferred for its higher sensitivity relative to i-rays.

[0127] R5 represents a phenyl or naphthyl group optionally having a substituent. Examples of such groups include phenyl or naphthyl groups having substituents such as hydrogen atoms, alkyl groups having 1 to 4 carbon atoms, trifluoromethyl, tetrafluoropropoxy, pentafluoropropoxy, hexafluoropropoxy, halogen atoms such as fluorine, chlorine, bromine, and iodine atoms, nitro, cyano, carbamoyl, aminosulfonyl, and alkoxy groups having 1 to 4 carbon atoms. Among these, tetrafluoropropoxyphenyl, pentafluoropropoxyphenyl, and hexafluoropropoxyphenyl are preferred for reasons of higher sensitivity relative to i-rays, and tetrafluoropropoxyphenyl is more preferred.

[0128] R6 represents a hydrogen atom, or optionally a straight-chain or branched alkyl group having 1 to 16 carbon atoms with substituents. Examples of straight-chain or branched alkyl groups having 1 to 16 carbon atoms with substituents include methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl, tert-butyl, n-pentyl, 1-ethylpropyl, 2,2-dimethylpropyl, cyclopentyl, hexyl, 5-ethylhexyl, 6-methylheptyl, and octyl. Among these, 5-ethylhexyl, 6-methylheptyl, and octyl are preferred for their better compatibility with bismaleimide compound (A), and 5-ethylhexyl is more preferred.

[0129] R7 can be a hydrogen atom or an alkyl group having 1 to 6 carbon atoms that is either straight-chain or branched. For example, R6 in formula (2) can be considered as an alkyl group having 1 to 6 carbon atoms that is either straight-chain or branched. Methyl, ethyl, propyl, and isopropyl are preferred for reasons of better solvent solubility, with methyl being more preferred.

[0130] n2 independently represents integers from 1 to 5.

[0131] It should be noted that the photocuring initiator (B1) shown in formula (2) can be an initiator with NO bond as (E) body, an initiator with NO bond as (Z) body, or a mixture of an initiator with NO bond as (E) body and an initiator with NO bond as (Z) body.

[0132] As the photocuring initiator (B1) shown in formula (2), the photocuring initiator shown in formula (14) is further preferred because it has higher sensitivity to i-rays and better solvent solubility.

[0133]

[0134] It should be noted that the photocuring initiator shown in formula (14) can be an initiator with NO bond as (E) body, an initiator with NO bond as (Z) body, or a mixture of an initiator with NO bond as (E) body and an initiator with NO bond as (Z) body.

[0135] (Manufacturing method of photocuring initiator (B1))

[0136] The photocuring initiator (B1) can be manufactured by known methods without particular limitation, such as the method described in Japanese Patent Publication No. 2014-500852.

[0137] The obtained photocuring initiator (B1) can be identified using known methods such as NMR (nuclear magnetic resonance analysis). The purity of the photocuring initiator (B1) can be analyzed using methods such as GPC, liquid chromatography, and IR spectroscopy. Volatile components such as byproducts and residual solvents in the photocuring initiator (B1) can be quantitatively analyzed using methods such as GPC and gas chromatography. If halogen atoms remain in the photocuring initiator (B1), the residual halogen compound can be identified using methods such as liquid chromatography-mass spectrometry, or quantitatively determined by potentiometric titration with silver nitrate solution or by decomposition via combustion followed by ion chromatography.

[0138] (The photocuring initiator (B2) shown in formula (3))

[0139] The photocuring initiator (B2) shown in formula (3) is the following compound.

[0140]

[0141] In formula (3), R8 represents an aryl group having 6 to 24 carbon atoms with optional substituents, or a heteroaryl group having 3 to 24 carbon atoms with optional substituents. Examples of aryl groups having 6 to 24 carbon atoms with optional substituents include phenyl, naphthyl, biphenyl, terphenyl, phenanthrene, and anthracene groups having hydrogen atoms, alkyl groups having 1 to 4 carbon atoms, halogen atoms such as trifluoromethyl, tetrafluoropropoxy, fluorine, chlorine, bromine, and iodine atoms, nitro, cyano, carbamoyl, aminosulfonyl, and alkoxy groups having 1 to 4 carbon atoms. Examples of heteroaryl groups with 3 to 24 carbon atoms that may have optional substituents include pyrrole, furanyl, benzofuranyl, thiophene, pyrazolyl, imidazolyl, oxazolyl, isoxazolyl, thiazolyl, isothiazolyl, triazolyl, pyridinyl, quinolinyl, isoquinolinyl, indolyl, benzofuranyl, benzothiophene, benzotriazolyl, and benzimidazolyl. Among these, benzofuranyl and benzothiophene are preferred for their higher sensitivity relative to i-rays, and benzofuranyl is more preferred.

[0142] R9 represents acetyl or benzoyl. Acetyl is preferred for its higher sensitivity relative to i-rays.

[0143] R 10 The alkyl group represents a hydrogen atom or, optionally, a straight-chain or branched alkyl group having 1 to 16 carbon atoms with substituents. Examples of straight-chain or branched alkyl groups having 1 to 16 carbon atoms with substituents include methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl, tert-butyl, n-pentyl, 1-ethylpropyl, 2,2-dimethylpropyl, cyclopentyl, isopentyl, hexyl, 5-ethylhexyl, and heptyl. Among these, isopentyl, hexyl, and 5-ethylhexyl are preferred for their better compatibility with the bismaleimide compound (A), and isopentyl is more preferred.

[0144] X represents an oxygen atom or a sulfur atom. Sulfur atoms are preferred because they have higher sensitivity relative to i-rays.

[0145] It should be noted that the photocuring initiator (B2) shown in formula (3) can be an initiator with NO bond as (E) body, an initiator with NO bond as (Z) body, or a mixture of an initiator with NO bond as (E) body and an initiator with NO bond as (Z) body.

[0146] As the photocuring initiator (B2) shown in formula (3), the photocuring initiator shown in formula (15) is further preferred because it has higher sensitivity to i-rays and better solvent solubility.

[0147]

[0148] It should be noted that the photocuring initiator shown in formula (15) can be an initiator with NO bond as (E) body, an initiator with NO bond as (Z) body, or a mixture of an initiator with NO bond as (E) body and an initiator with NO bond as (Z) body.

[0149] (Manufacturing method of photocuring initiator (B2))

[0150] The photocuring initiator (B2) can be manufactured by known methods without particular limitation, such as the method described in Japanese Patent Publication No. 2016-531926.

[0151] The obtained photocuring initiator (B2) can be identified using known methods such as NMR (nuclear magnetic resonance analysis). The purity of the photocuring initiator (B2) can be analyzed using methods such as GPC, liquid chromatography, and IR spectroscopy. Volatile components such as byproducts and residual solvents in the photocuring initiator (B2) can be quantitatively analyzed using methods such as GPC and gas chromatography. If halogen atoms remain in the photocuring initiator (B2), the residual halogen compounds can be identified using methods such as liquid chromatography-mass spectrometry, or quantitatively determined by potentiometric titration with silver nitrate solution or by decomposition via combustion followed by ion chromatography.

[0152] (Other photocuring initiators (b))

[0153] The resin composition of this embodiment can contain a known photocuring initiator (b) other than the photocuring initiator (B) as long as it achieves the effects of the present invention. Examples of photocuring initiators (b) include benzoin derivatives such as benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin propyl ether, and benzoin isobutyl ether; organic peroxides such as benzoyl peroxide, lauroyl peroxide, acetyl peroxide, p-chlorobenzoyl peroxide, and di-tert-butyl disperoxy phthalate; acylphosphine oxides such as 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, benzoyl-diphenylphosphine oxide, and bisbenzoyl-phenylphosphine oxide; and acetophenone, 2,2-diethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, 1,1-dichloroacetophenone, 2-hydroxy-2-methyl-phenylpropane-1-one, diethoxyacetophenone, 1-hydroxycyclohexylphenyl ketone, 2-methyl-1-phenylacetophenone, etc. Acetophenones such as -[4-(methylthio)phenyl]-2-morpholinopropane-1-one and 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1; anthraquinones such as 2-ethylanthraquinone, 2-tert-butylanthraquinone, 2-chloroanthraquinone and 2-pentylanthraquinone; thioxanones such as 2,4-diethylthioxanone, 2-isopropylthioxanone and 2-chlorothioxanone; acetophenone dimethyl ketal and benzoyl dimethyl ketal. Ketals such as ketones; benzophenones such as benzoyl-4'-methyldiphenyl sulfide and 4,4'-dimethylaminobenzophenone; free radical photoinitiators such as 1-[4-(phenylthio)phenyl]-1,2-octanedione-2-(O-benzoyl oxime)] and 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3-yl]-acetone-1-(O-acetyl oxime);

[0154] Diazonium salts of Lewis acids such as p-methoxyphenyldiazonium fluorophosphonate and N,N-diethylaminophenyldiazonium hexafluorophosphonate; iodonium salts of Lewis acids such as diphenyliodonium hexafluorophosphonate and diphenyliodonium hexafluoroantimonate; sulfonium salts of Lewis acids such as triphenylsulfonium hexafluorophosphonate and triphenylsulfonium hexafluoroantimonate; phosphonium salts of Lewis acids such as triphenylphosphonium hexafluoroantimonate; other halides; triazine initiators; borate initiators; and other cationic photopolymerization initiators such as photoacid generators.

[0155] These photocuring initiators (b) can be used alone or in appropriate combinations of two or more.

[0156] Photocuring initiators (b) can also be commercially available products, such as IGM Resins BV's Omnirad 369 (trade name), IGM Resins BV's Omnirad 819 (trade name), IGM Resins BV's Omnirad 819DW (trade name), IGM Resins BV's Omnirad 907 (trade name), IGM Resins BV's Omnirad TPO (trade name), IGM Resins BV's Omnirad TPO-G (trade name), IGM Resins BV's Omnirad 784 (trade name), BASF Japan's Irgacure OXE01 (trade name) and BASF Japan's Irgacure OXE02 (trade name), etc.

[0157] As the photocuring initiator (b), acylphosphine oxides are preferred because they are more compatible with bismaleimide compounds (A) and photocuring initiators (B).

[0158] As an acylphosphine oxide, the compound shown in formula (16) is more preferred.

[0159]

[0160] In equation (16), R 25 Each of the substituents or phenyl groups represented independently by formula (17) is preferred. 25 One or more of them are substituents as shown in formula (17).

[0161]

[0162] In equation (17), R 26 Each can independently represent a hydrogen atom or a methyl group. In formula (17), -* indicates a direct connection to R in formula (16). 25 The atomic bonds of phosphorus atoms (P). Preferably R 26 One or more of them are methyl, more preferably all of them are methyl.

[0163] Examples of compounds represented by formula (16) include acylphosphine oxides such as 2,4,6-trimethylbenzoyl-diphenylphosphine oxide and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide. Among these, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide is preferred due to its better compatibility with bismaleimide compound (A) and photocuring initiator (B) and its superior solvent solubility. These compounds can be used alone or in appropriate mixtures of two or more.

[0164] When the resin composition contains a photocuring initiator (b), from the viewpoint of enabling the resin composition to be photocured more fully without hindering the photocuring reaction and making the exposed portion more insoluble in terms of alkali developability, the content of the photocuring initiator (b) is preferably 0.05 to 20 parts by mass of the resin solids in the resin composition, more preferably 0.1 to 15 parts by mass, further preferably 0.2 to 10 parts by mass, and even more preferably 0.3 to 7.0 parts by mass.

[0165] When the resin composition contains a photocuring initiator (b), from the viewpoint of enabling the resin composition to be photocured more fully without hindering the photocuring reaction and making the exposed portion more insoluble in terms of alkali developability, the total content of the photocuring initiator (B) and the photocuring initiator (b) is preferably 0.2 to 50 parts by mass of 100 parts by mass of the resin solids in the resin composition, more preferably 1.0 to 30 parts by mass, and even more preferably 1.5 to 10 parts by mass.

[0166] When the resin composition contains a photocuring initiator (b), from the viewpoint of enabling the resin composition to undergo photocuring more fully without hindering the photocuring reaction and ensuring that the exposed portion is more fully insoluble in terms of alkali developability, the content of the photocuring initiator (B) is preferably 30 to 99 parts by mass relative to a total of 100 parts by mass of the photocuring initiator (B) and the photocuring initiator (b), more preferably 40 to 95 parts by mass, and even more preferably 50 to 90 parts by mass. Furthermore, the content of the photocuring initiator (b) is preferably 1.0 to 70 parts by mass relative to a total of 100 parts by mass of the photocuring initiator (B) and the photocuring initiator (b), more preferably 5.0 to 60 parts by mass, and even more preferably 10 to 50 parts by mass.

[0167] [Compounds containing one or more carboxyl groups (C)]

[0168] The resin composition of this embodiment preferably further comprises a compound (C) containing one or more carboxyl groups. There are no particular limitations on the compound (C) as long as it contains one or more carboxyl groups. The carboxyl group can be a salt such as a sodium salt or a potassium salt, and if it contains two or more carboxyl groups within the molecule, it can be an acid anhydride formed by their linkage to each other. Compound (C) can be used alone or in a suitable mixture of two or more.

[0169] In this embodiment, during the exposure process of manufacturing a multilayer printed circuit board, by using a resin composition that includes a bismaleimide compound (A), an initiator (B), a compound (C), and a maleimide compound (D) mixed as needed (described later), a cured product can be obtained more effectively without hindering the photocuring reaction. Furthermore, during the development process, a resin composition that includes a bismaleimide compound (A), an initiator (B), a compound (C), and a maleimide compound (D) mixed as needed (described later) can be obtained, which imparts superior alkaline developability to the resin composition in the unexposed areas after exposure. The reasons for this are not yet certain, but the inventors speculate as follows.

[0170] In other words, during the exposure process of manufacturing multilayer printed circuit boards, compound (C) does not possess functional groups that participate in the photocuring reaction during the exposure process and does not hinder the photocuring reaction. Bismaleimide compound (A) does not possess a framework that hinders light transmittance and exhibits excellent light transmittance. Therefore, even when bismaleimide compound (A) and initiator (B) are present along with compound (C) and compound (D) mixed as needed, photopolymerization will still occur, resulting in a more suitable cured product.

[0171] Furthermore, compound (C) can be present in the resin composition of the unexposed portion. Therefore, during the developing process, if the alkaline developer flows into the unexposed portion, the alkaline component in the alkaline developer and the carboxyl group in compound (C) can more readily form a salt, further improving water solubility. Thus, superior alkaline developability can be obtained.

[0172] When preparing an N-methylpyrrolidone solution containing 1% by mass of compound (C), and measuring the transmittance of the N-methylpyrrolidone solution containing 1% by mass of compound (C) using active energy rays containing a wavelength of 365 nm (i-rays), the transmittance is preferably 5% or more. This compound (C) exhibits very excellent light transmittance. When using this compound (C), even when using active energy rays containing a wavelength of 365 nm (i-rays), the photoradical reaction of maleimide is effectively induced when manufacturing printed circuit boards with high-density and high-fine wiring formation (patterns). From the perspective of obtaining a resin composition with better photocurability, the transmittance at a wavelength of 365 nm (i-rays) is preferably in the range of 8% or more, 10% or more, 20% or more, 30% or more, and 40% or more, respectively. The upper limit of the transmittance at a wavelength of 365 nm (i-rays) is, for example, 99.9% or less, and can be 100% or less.

[0173] In this embodiment, from the viewpoint of obtaining better alkaline developability, it is preferable to include carboxyl groups in the molecule of compound (C) in integers from 2 to 20.

[0174] From the viewpoint of further improving developability, the molecular weight of compound (C) is preferably 50 to 10,000, more preferably 100 to 8,000, even more preferably 130 to 6,000, and even more preferably 150 to 5,000.

[0175] From the viewpoint of further improving developability, the mass-average molecular weight of compound (C) is preferably 50 to 10,000, more preferably 100 to 8,000, and even more preferably 150 to 5,000.

[0176] In the resin composition, from the perspective of imparting better alkali developability and enabling the resin composition to exhibit good curability without hindering the photocuring reaction, the content of compound (C) relative to 100 parts by weight of the resin solids in the resin composition is preferably 0.1 to 30 parts by weight, more preferably 0.5 to 20 parts by weight, even more preferably 1.0 to 15 parts by weight, even more preferably 1.5 to 10 parts by weight, and even more preferably 2.0 to 10 parts by weight.

[0177] When the resin composition contains both bismaleimide compound (A) and initiator (B) and compound (D), from the perspective of imparting better alkali developability and enabling the resin composition to exhibit good curability without hindering the photocuring reaction, the content of compound (C) is preferably 0.1 to 20 parts by mass relative to the total of 100 parts by mass of compound (A), initiator (B), compound (C) and compound (D), more preferably 0.5 to 15 parts by mass, further preferably 1.0 to 10 parts by mass, and even more preferably 2.0 to 9.0 parts by mass.

[0178] Examples of compounds (C) include formic acid, aliphatic compounds containing one or more carboxyl groups, aromatic compounds containing one or more carboxyl groups, heteroatom compounds containing one or more carboxyl groups, and anhydrides. These compounds (C) may be used alone or in appropriate combinations of two or more.

[0179] (Aliphatic compounds containing one or more carboxyl groups)

[0180] Examples of aliphatic compounds containing one or more carboxyl groups include chain-like aliphatic monocarboxylic acids, alicyclic monocarboxylic acids, chain-like aliphatic polycarboxylic acids, and alicyclic polycarboxylic acids. These compounds may contain hydrogen atoms and substituents such as alkyl, alkoxy, aryloxy, aryl, aminoalkyl, hydroxyl, amino, and carboxylalkyl groups within the molecule. Furthermore, when these compounds contain two or more carboxyl groups within the molecule, they can be acid anhydrides formed by their interconnection. When these compounds contain carboxylalkyl groups within the molecule, they can be acid anhydrides formed by the interconnection of carboxylalkyl and carboxyl groups. When these compounds contain two or more carboxylalkyl groups within the molecule, they can be acid anhydrides formed by their interconnection.

[0181] Examples of alkyl groups include methyl, ethyl, n-propyl, isopropyl, butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, n-hexyl, n-heptyl, and n-octyl.

[0182] Examples of alkoxy groups include methoxy, ethoxy, propoxy, isopropoxy, n-butoxy, isobutoxy, tert-butoxy, n-hexyloxy, and 2-methylpropoxy.

[0183] Examples of aryloxy groups include phenoxy and p-tolyloxy.

[0184] Examples of aryl groups include phenyl, tolyl, benzyl, methylbenzyl, xylyl, mesitylene, naphthyl, and anthracene.

[0185] Examples of aminoalkyl groups include aminomethyl, aminoethyl, aminopropyl, aminodimethyl, aminodiethyl, aminodipropyl, aminobutyl, aminohexyl, and aminononyl.

[0186] Examples of carboxyl alkyl groups include carboxymethyl, carboxyethyl, carboxypropyl, carboxybutyl, carboxyhexyl, and carboxynonyl.

[0187] As chain-like aliphatic monocarboxylic acids, examples include saturated fatty acids such as acetic acid, propionic acid, isobutyric acid, butyric acid, isovaleric acid, valeric acid, hexanoic acid, lactic acid, succinic acid, octanoic acid, nonanoic acid, decanoic acid, dodecanoic acid, tetradecanoic acid, hexadecanoic acid, heptadecanoic acid, and octadecanoic acid, as well as unsaturated fatty acids such as oleic acid, transoleic acid, erucic acid, nervonic acid, linolenic acid, stearidonic acid, eicosapentaenoic acid, linoleic acid, and linolenic acid.

[0188] Examples of alicyclic monocarboxylic acids include monocyclic carboxylic acids such as cyclopropane carboxylic acid, cyclopropene carboxylic acid, cyclobutane carboxylic acid, cyclobutene carboxylic acid, cyclopentane carboxylic acid, cyclopentene carboxylic acid, cyclohexane carboxylic acid, cyclohexene carboxylic acid, cycloheptane carboxylic acid, cycloheptene carboxylic acid, cyclooctane carboxylic acid, and cyclooctene carboxylic acid; and polycyclic or bridged alicyclic carboxylic acids such as norbornene carboxylic acid, tricyclic decane carboxylic acid, tetracyclic dodecane carboxylic acid, adamantane carboxylic acid, methyl adamantane carboxylic acid, ethyl adamantane carboxylic acid, and butyl adamantane carboxylic acid.

[0189] As chain-like aliphatic polycarboxylic acids, examples include carboxylic acids obtained by further adding one or more carboxyl groups to chain-like aliphatic monocarboxylic acids. Examples include malonic acid, octanoic acid, azelaic acid, sebacic acid, dodecanoic acid, tetradecanoic acid, hexadecanoic acid, heptadecanoic acid, and octadecanoic acid.

[0190] As alicyclic polycarboxylic acids, examples include carboxylic acids obtained by adding one or more carboxyl groups to an alicyclic monocarboxylic acid. Examples include monocyclic carboxylic acids such as cyclopropane dicarboxylic acid, cyclopropane dicarboxylic acid, cyclopropane tricarboxylic acid, cyclopropane tricarboxylic acid, cyclobutane dicarboxylic acid, cyclobutene dicarboxylic acid, cyclobutane tricarboxylic acid, cyclobutene tricarboxylic acid, cyclobutane tetracarboxylic acid, cyclobutene tetracarboxylic acid, cyclopentane dicarboxylic acid, cyclopentene dicarboxylic acid, cyclopentane tricarboxylic acid, cyclopentane tetracarboxylic acid, cyclopentene tetracarboxylic acid, cyclopentane pentacarboxylic acid, cyclopentene pentacarboxylic acid, cyclohexane dicarboxylic acid, cyclohexene dicarboxylic acid, cyclohexene tricarboxylic acid, cyclohexane tetracarboxylic acid, cyclohexene tetracarboxylic acid, cyclohexane pentacarboxylic acid, cyclohexene pentacarboxylic acid, cyclohexane hexacarboxylic acid, cyclohexene hexacarboxylic acid, cycloheptane dicarboxylic acid, cycloheptene dicarboxylic acid, cyclooctane dicarboxylic acid, and cyclooctene dicarboxylic acid, as well as polycyclic or bridged alicyclic dicarboxylic acids such as norbornane dicarboxylic acid and adamantane dicarboxylic acid.

[0191] (Aromatic compounds containing one or more carboxyl groups)

[0192] Examples of parent skeletons for aromatic compounds containing one or more carboxyl groups include benzoic acid, phenylene acetic acid, salicylic acid, phthalic acid, trimellitic acid, pyromellitic acid, pentacarboxybenzene, hexacarboxybenzene, naphtholic acid, naphthalene dicarboxylic acid, naphthalene tricarboxylic acid, naphthalene tetracarboxylic acid, anthracene carboxylic acid, anthracene dicarboxylic acid, anthracene tricarboxylic acid, anthracene tetracarboxylic acid, and anthracene pentacarboxylic acid. Aromatic compounds may have, for example, hydrogen atoms and substituents such as alkyl, alkoxy, aryloxy, aryl, aminoalkyl, hydroxyl, amino, and carboxylalkyl groups on the aromatic ring of these parent skeletons. Furthermore, when these compounds have two or more carboxyl groups within their molecule, they can be anhydrides formed by their interconnection. When these compounds have carboxylalkyl groups within their molecule, they can be anhydrides formed by the interconnection of carboxylalkyl and carboxyl groups. When these compounds have two or more carboxylalkyl groups within their molecule, they can be anhydrides formed by their interconnection. For these substituents, refer to the foregoing.

[0193] (Heteroatom compounds containing one or more carboxyl groups)

[0194] Examples of heteroatom compounds containing one or more carboxyl groups as parent skeletons include compounds containing one or more carboxyl groups on heterocycles such as furan, thiophene, pyrrole, imidazole, pyran, pyridine, pyrimidine, pyrazine, pyrrolidine, piperidine, piperazine, morpholine, indole, purine, quinoline, isoquinoline, quinine ring, chromene, thiathracene, phenothiazine, phenoxazine, oxanthracene, acridine, phenothiazine, and carbazole. Heteroatom compounds may have, for example, hydrogen atoms and substituents such as alkyl, alkoxy, aryloxy, aryl, aminoalkyl, hydroxyl, amino, and carboxylalkyl groups on these parent skeletons. Furthermore, when these compounds have two or more carboxyl groups within their molecule, they can be anhydrides formed by their interconnection. When these compounds have carboxylalkyl groups within their molecule, they can be anhydrides formed by the interconnection of carboxylalkyl and carboxyl groups. When these compounds have two or more carboxylalkyl groups within their molecule, they can be anhydrides formed by their interconnection. For these substituents, refer to the foregoing.

[0195] As for compound (C), the compound containing formula (4) is preferred because it has better compatibility with bismaleimide compound (A), can quickly and more suitably form salts with the alkaline components in alkaline developer, and has further improved water solubility.

[0196]

[0197] In equation (4), R 11 Each group or hydrogen atom represented independently by formula (5) is represented by R. 12 Each alkyl group independently represents a hydrogen atom or a straight-chain or branched alkyl group having 1 to 6 carbon atoms. At least one R is present. 11 The group is shown in formula (5).

[0198]

[0199] In equation (5), -* indicates a direct connection to R in equation (4). 11 The atomic bonds of the oxygen atom (O).

[0200] In equation (4), from the perspective of imparting superior alkali developability, R 11 Preferably, it contains two or more groups represented by formula (5), more preferably three or more, and even more preferably R 11 All are groups represented by Formula (5). Regarding the groups represented by Formula (5), if the carbonyl group is positioned at position 1 relative to the cyclohexane ring, and a carboxyl group is bonded at position 2 relative to that carbonyl group, then the other carboxyl group can be bonded to any of the 3 to 6 positions of the cyclohexane ring. In addition, the compound represented by Formula (4) exists in cis, trans, and mixtures of cis and trans forms because the structure of the carbonyl group bonded to the cyclohexane ring and the two carboxyl groups in the groups represented by Formula (5) has a stereostructure. That is, the compound represented by Formula (4) can be a single isomer or a mixture containing two or more isomers.

[0201] In equation (4), regarding R 11 From the perspective of imparting superior alkali developability, R is preferred. 11 At least one of the groups is a group represented by formula (18). That is, preferably, in the group represented by formula (18), the stereostructure of the carbonyl group bonded at position 1 of the cyclohexane ring and the carboxyl group at position 2 is cis-isomorphic. For the other carboxyl group, its stereostructure can be either cis-isomorphic or trans-isomorphic. For R 11 From the perspective of imparting further superior alkali developability, it is preferable to include two or more groups represented by formula (18), more preferably three or more, and even more preferably R 11 All are groups represented by formula (18). Regarding R 11 It is not clear whether at least one of the groups in the resin composition is a group represented by formula (18) that imparts superior alkaline developability, but the inventors speculate as follows. That is, if the carbonyl group bonded at position 1 and the carboxyl group bonded at position 2 are cis-forms, the carboxyl group at position 2 in the resin composition can more easily form a salt stereostructure with the alkaline component in the alkaline developer. Therefore, it is speculated that this is because the water solubility is further improved, which further promotes the inflow of the alkaline developer into the resin composition.

[0202]

[0203] In equation (18), -* indicates a direct connection to R in equation (4). 11 The oxygen atom (O) is connected by an atomic bond.

[0204] In equation (4), R 12 Each can independently represent a hydrogen atom or a straight-chain or branched alkyl group having 1 to 6 carbon atoms.

[0205] Examples of alkyl groups that are straight-chain or branched and have 1 to 6 carbon atoms include methyl, ethyl, n-propyl, isopropyl, n-butyl, 2-butyl, isobutyl, tert-butyl, n-pentyl, 2-pentyl, tert-pentyl, 2-methylbutyl, 3-methylbutyl, 2,2-dimethylpropyl, n-hexyl, 2-hexyl, 3-hexyl, 2-methylpentyl, 3-methylpentyl, 4-methylpentyl, and 2-methylpentan-3-yl.

[0206] As R 12 From the viewpoint of exhibiting good solubility in solvents, it is preferred to be a straight-chain alkyl group having 1 to 6 carbon atoms, more preferably methyl, ethyl, n-propyl, 2-butyl, isobutyl, tert-butyl and n-pentyl, and even more preferably methyl, ethyl and n-propyl.

[0207] From the viewpoint that it can impart better alkaline development properties and thus exhibit good solubility in solvents, the compound shown in formula (4) is preferably the compound shown in formula (19) and the compound shown in formula (20), and more preferably the compound shown in formula (20).

[0208]

[0209]

[0210] In the resin composition, from the perspective of being able to impart better alkali developability and enabling the resin composition to exhibit better curability without hindering the photocuring reaction, the content of the compound shown in formula (4) relative to the total 100 parts by mass of compound (C) is preferably 10 to 100 parts by mass, more preferably 30 to 99 parts by mass, further preferably 50 to 95 parts by mass, even more preferably 60 to 90 parts by mass, and even more preferably 80 to 90 parts by mass.

[0211] [Method for manufacturing the compound shown in formula (4)]

[0212] The compound shown in formula (4) can be manufactured by known methods, for example, by a step involving esterification of the alcohol compound shown in formula (21) with the anhydride (cyclohexane-1,2,4-tricarboxylic acid-1,2-anhydride) shown in formula (22). It should be noted that the anhydride shown in formula (22) has a stereostructure due to the two carbonyl groups and one carboxyl group bonded to the cyclohexane ring, and therefore exists in cis, trans, and mixtures of cis and trans isomers. That is, the anhydride shown in formula (22) can be a single isomer or a mixture containing two or more isomers.

[0213]

[0214] In equation (21), R 27 Each can independently represent a hydrogen atom or a straight-chain or branched alkyl group having 1 to 6 carbon atoms.

[0215] As a straight-chain or branched alkyl group having 1 to 6 carbon atoms, including its preferred form, refer to R in the aforementioned formula (4). 12 .

[0216]

[0217] Examples of alcohol compounds represented by formula (22) include, for example, bis(trimethylolethane), bis(trimethylolpropane), bis(trimethylolbutane), bis(trimethylolpentane), 2,2'-(oxybis(methylene))bis(propane-1,3-diol), 2,2'-(oxybis(methylene))bis(2-methylpropane-1,3-diol) and 2-((2,2-bis(hydroxymethyl)butoxy)methyl)-2-methylpropane-1,3-diol.

[0218] When using the compound shown in formula (4) to manufacture a cured product as the anhydride represented by formula (22), it is preferable to include the anhydride represented by formula (23) (cis-,cis-cyclohexane-1,2,4-tricarboxylic acid-1,2-anhydride) from the viewpoint of imparting better alkali developability. That is, in the anhydride represented by formula (23), if the carbonyl group is positioned at positions 1 and 2 relative to the cyclohexane ring, the stereostructure of the carbonyl group bonded to position 4 relative to the carbonyl group and the two carbonyl groups is preferably cis-form.

[0219]

[0220] Esterification reactions can be carried out in solvents or under solvent-free conditions. There are no particular limitations on the solvent, as long as it does not react with alcohols or acid anhydrides.

[0221] Examples of such solvents include halogenated solvents such as dichloromethane, chloroform, dichloroethane, and chlorobenzene; aprotic polar solvents such as dimethylformamide, dimethylacetamide, dimethyl sulfoxide, tetrahydrofuran, dioxane, and acetonitrile; ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclopentanone, and cyclohexanone; cellosolve solvents such as 2-ethoxyethanol and propylene glycol monomethyl ether; aliphatic alcohol solvents such as methanol, ethanol, propanol, isopropanol, and butanol; phenol solvents containing aromatic groups such as phenol and cresol; ester solvents such as ethyl lactate, methyl acetate, ethyl acetate, butyl acetate, isoamyl acetate, methyl methoxypropionate, methyl hydroxyisobutyrate, γ-butyrolactone, and propylene glycol monomethyl ether acetate; and aromatic hydrocarbon solvents such as toluene and xylene. These solvents can be used alone or in combination of two or more.

[0222] Among them, from the viewpoint of being able to more fully dissolve alcohol compounds and acid anhydrides, halogenated solvents, aprotic polar solvents, ketone solvents, and ester solvents are preferred.

[0223] Dichloromethane is preferred as a halogen-containing solvent. Dimethylacetamide is preferred as an aprotic polar solvent. Methyl ethyl ketone is preferred as a ketone solvent. Propylene glycol monomethyl ether is preferred as a cellosol solvent. Butyl acetate, γ-butyrolactone, and propylene glycol monomethyl ether acetate are preferred as ester solvents.

[0224] When using solvent, the amount used is typically 20 to 2000 parts by mass relative to the total 100 parts by mass of the alcohol and acid anhydride.

[0225] Esterification can occur with or without a catalyst.

[0226] When a catalyst is used, examples of catalysts include acidic compounds such as hydrochloric acid, sulfuric acid, methanesulfonic acid, trifluoromethanesulfonic acid, p-toluenesulfonic acid, nitric acid, trifluoroacetic acid, and trichloroacetic acid; metal hydroxides such as sodium hydroxide, potassium hydroxide, calcium hydroxide, and magnesium hydroxide; amine compounds such as triethylamine, tripropylamine, diisopropylethylamine, and tributylamine; aliphatic amines with aromatic rings such as aniline, N-methylaniline, N,N-dimethylaniline, and benzylamine; and pyridine, 4-dimethylaminopyridine, 1,8-diazabicyclo[5.4.0]undec-7-ene, imidazole, etc. Heterocyclic compounds such as azoles, triazoles, and tetraazoles; quaternary ammonium salts such as tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, trimethylethylammonium hydroxide, trimethylpropylammonium hydroxide, trimethylbutylammonium hydroxide, trimethylhexadecylammonium hydroxide, trioctylmethylammonium hydroxide, tetramethylammonium chloride, tetramethylammonium bromide, tetramethylammonium iodide, tetramethylammonium acetate, and trioctylmethylammonium acetate; orthotitanic acids such as tetraethyl orthotitanic acid and tetramethyl orthotitanic acid; and metal soaps such as tin octoate, cobalt octoate, zinc octoate, manganese octoate, calcium octoate, sodium octoate, and potassium octoate. These catalysts can be used alone or in appropriate mixtures of two or more. From the viewpoint of better reactivity, amine compounds, aliphatic amines with aromatic rings, and heterocyclic compounds are preferred, with triethylamine and 4-dimethylaminopyridine being more preferred. Furthermore, the amount of catalyst used is typically 0.0001 to 1000 parts by mass relative to 1 part by mass of the alcohol compound.

[0227] Regarding methods of adding catalysts, examples include: adding them directly to alcohol compounds and / or acid anhydrides; and adding a solution of the catalyst, which is dissolved in a soluble solvent, to alcohol compounds, acid anhydrides, and / or solvents containing them.

[0228] When esterification is carried out using a catalyst, the reaction temperature is not particularly limited by the amount of catalyst or the solvent used, and is typically -20 to 150°C. Furthermore, the reaction time is not particularly limited, and is typically 0.5 to 100 hours. The reaction can be completed in one stage or in two or more stages.

[0229] In this embodiment, the alcohol compound represented by formula (21) and the acid anhydride represented by formula (22) are relatively highly reactive, and therefore esterification can occur even without a catalyst. As the acid anhydride represented by formula (22), it is preferable to include the acid anhydride represented by formula (23) to enhance its reactivity with the alcohol compound. In this specification, "without a catalyst" means that no catalyst is added or only a very small amount is added to facilitate the esterification reaction. Specifically, this means that in the reaction, the catalyst content is 50 ppm or less relative to 1 part by mass of the alcohol compound represented by formula (22). Furthermore, the catalyst content that facilitates the esterification reaction is preferably 0 ppm.

[0230] When esterification is carried out without a catalyst, halogenated solvents, ketone solvents, and ester solvents are preferred from the viewpoint of being able to fully dissolve the alcohol compound and the acid anhydride, and also to dissolve the compound shown in formula (4) more fully. Furthermore, halogenated solvents and ester solvents are more preferred from the viewpoint of exhibiting better solubility and further suppressing the hydrolysis of the acid anhydride. Moreover, ester solvents are further preferred from the viewpoint of enabling the alcohol compound to react better with the acid anhydride, further suppressing the hydrolysis of the acid anhydride, and reducing environmental impact. As a halogenated solvent, dichloromethane is preferred from the viewpoint of exhibiting better solubility. As a ketone solvent, methyl ethyl ketone is preferred from the viewpoint of exhibiting better solubility. As an ester solvent, butyl acetate, γ-butyrolactone, and propylene glycol monomethyl ether acetate are preferred from the viewpoint of exhibiting better solubility.

[0231] By using this solvent under catalyst-free conditions, the steps of separating the compound of formula (4) from the reaction mixture described later, as well as the purification steps, can be eliminated. It should be noted that the reaction temperature and reaction time are as described later.

[0232] The rationale for this is not yet certain, but the inventors speculate as follows: By using halogen-containing solvents, ketone solvents, and ester solvents, the hydrolysis of the acid anhydride shown in formula (22) can be more appropriately suppressed, further suppressing side reactions other than the target esterification reaction. Therefore, it is speculated that impurities are less likely to be generated, and the target product with high purity can be obtained.

[0233] In addition, regarding the amount of solvent used, it is usually 20 to 2000 parts by mass relative to the total 100 parts by mass of alcohol compound and acid anhydride. From the perspective of further reducing the environmental impact, it is preferably 20 to 1000 parts by mass, and more preferably 20 to 500 parts by mass.

[0234] When esterification is carried out without a catalyst, the reaction temperature of esterification can be appropriately set according to the solvent used, typically from -20 to 150°C, and more preferably from 0 to 150°C, and even more preferably from 20 to 120°C, for better esterification.

[0235] When esterification is carried out without a catalyst, the reaction time is typically 0.5 to 100 hours. From the perspective of suppressing side reactions and ensuring better esterification, a reaction time of 0.5 to 80 hours, and even more preferably 0.5 to 50 hours, is preferred. It should be noted that the reaction can be completed in one stage or in two or more stages.

[0236] When using an ester solvent, the alcohol compound can be more fully esterified with the acid anhydride under catalyst-free conditions. This reduces the cost of catalysts, eliminates the need for catalyst removal, minimizes the generation of impurities, and yields compounds with relatively high purity. Therefore, under these manufacturing conditions, the steps of separating the compound of formula (4) from the reaction mixture and the purification step, described later, can also be omitted. It should be noted that the reaction temperature and reaction time are as described above.

[0237] The rationale for this is still uncertain, but the inventors speculate as follows: That is, the ester solvent can further suppress the hydrolysis of the acid anhydride shown in formula (22), and can further suppress side reactions other than the target esterification reaction. Therefore, it is speculated that impurities are less likely to form compared to other solvents, resulting in a target product with higher purity.

[0238] Regarding the method for separating the target compound from the reaction mixture containing the compound shown in formula (4), if the target compound precipitates from the reaction solvent, separation can be performed by filtration or centrifugation. Alternatively, if the target compound is dissolved in the reaction solvent, precipitation can be achieved by distilling off the solvent under reduced pressure, adding a suitable unsuitable solvent to the reaction mixture, or discharging the reaction mixture into an unsuitable solvent, followed by filtration or centrifugation. It should be noted that unsuitable solvents include hydrocarbons such as hexane, heptane, cyclohexane, toluene, and xylene. One of these solvents can be used alone, or two or more can be used in appropriate combinations.

[0239] If further purification of the isolated compound is required, well-known methods can be used. Examples of such methods include distillation, recrystallization, column chromatography, sludge treatment, and activated carbon treatment.

[0240] The compound represented by formula (4) can be identified by known methods such as NMR (nuclear magnetic resonance analysis). The purity of the compound can be analyzed by, for example, GPC, liquid chromatography, and IR spectroscopy. Volatile components such as byproducts and residual solvents in the compound can be quantitatively analyzed by, for example, GPC and gas chromatography. Residual halides in the compound can be identified by, for example, liquid chromatography-mass spectrometry, or quantitatively determined by ion chromatography after potentiometric titration with silver nitrate solution or decomposition based on combustion.

[0241] Furthermore, in this embodiment, from the viewpoint of imparting more superior alkaline developability to the resin composition, the anhydride comprising a fully hydrogenated aromatic polycarboxylic acid and / or a partially hydrogenated aromatic polycarboxylic acid is more preferred as compound (C). From the viewpoint of imparting more superior alkaline developability to the resin composition, it is further preferred that these compounds be used in conjunction with the compound shown in formula (4).

[0242] Anhydrides of aromatic polycarboxylic acids, both complete and partial hydrides, include, for example, 1,2,4-cyclohexanetricarboxylic acid-1,2-anhydride and 1,2,4,5-cyclohexanetetracarboxylic acid dianhydride; 1,2,3-benzenetricarboxylic acid, 1,2,4-naphthalenetricarboxylic acid, 3,3',4,4'-benzophenonetetracarboxylic acid, 2,2',3,3'-benzophenonetetracarboxylic acid, 2,3,3',4'-benzophenonetetracarboxylic acid, 3,3 Anhydrides of the fully hydrogenated or partially hydrogenated forms of ',4,4'-biphenyltetracarboxylic acid, 2,2',3,3'-biphenyltetracarboxylic acid, 2,3,3',4'-biphenyltetracarboxylic acid, 4,4'-oxobisphthalic acid, diphenylmethanetetracarboxylic acid, 1,2,5,6-naphthalenetetracarboxylic acid, 2,3,6,7-naphthalenetetracarboxylic acid, 3,4,9,10-perylenetetracarboxylic acid, anthracenetetracarboxylic acid, 4,4'-(hexafluoroisopropylidene)diphthalic acid, phenylpentacarboxylic acid, and phenylhexacarboxylic acid.

[0243] Regarding the anhydrides of fully hydrides and partially hydrides of aromatic polycarboxylic acids, from the viewpoint of imparting superior alkali developability and better compatibility with compounds of formula (4) when used with them, alicyclic structures such as monocyclic cycloalkanes (e.g., cyclopentane and cyclohexane), monocyclic cycloolefins (e.g., cyclopropylene and cyclohexene), bicyclic alkanes (e.g., dicyclic undecane and decahydronaphthalene), and bicyclic alkenes (e.g., norbornene and norbornadiene) are preferred, and monocyclic cycloalkanes or monocyclic cycloolefins are even more preferred. Examples of such preferred anhydrides include, for instance, 1,2,4-cyclohexanetricarboxylic acid-1,2-anhydride and 1,2,4,5-cyclohexanetetracarboxylic acid dianhydride. From the viewpoint of being able to impart better alkali developability and having better compatibility with the compound shown in formula (4) when used with the compound shown in formula (4), 1,2,4-cyclohexanetricarboxylic acid-1,2-anhydride is further preferred, and cis,cis-1,2,4-cyclohexanetricarboxylic acid-1,2-anhydride is further preferred.

[0244] In the resin composition, from the perspective of imparting better alkali developability and enabling the resin composition to exhibit better curability without hindering the photocuring reaction, the total content of the anhydrides of the fully hydrogenated and partially hydrogenated aromatic polycarboxylic acids is preferably 0.05 to 40 parts by mass relative to a total of 100 parts by mass of compound (C), more preferably 0.1 to 35 parts by mass, further preferably 1.0 to 30 parts by mass, even more preferably 5.0 to 25 parts by mass, and still more preferably 10 to 20 parts by mass.

[0245] [Maleimide compound (D)]

[0246] The resin composition of this embodiment preferably further comprises at least one maleimide compound (D) selected from the group consisting of the compound shown in formula (6), the compound shown in formula (7), the compound shown in formula (8), the compound shown in formula (9), the compound shown in formula (10), and the compound shown in formula (11).

[0247] As mentioned above, maleimide compounds typically exhibit very low photoradical reactivity. However, bismaleimide compound (A) possesses excellent light transmittance, as described above. Therefore, even when the resin composition contains maleimide compound (D), by using bismaleimide compound (A) together with an initiator (B) and a compound (C) as needed, light sufficiently reaches the photocuring initiator under active energy rays containing a wavelength of 365 nm (i-rays), appropriately initiating a free radical reaction using the free radicals generated by the photocuring initiator, effectively induced by the photoradical reaction of maleimide, thus enabling its photocuring.

[0248] The resin compositions containing maleimide compound (D) also exhibit excellent alkali developability and photocurability. Furthermore, the resulting cured products demonstrate superior heat resistance, insulation reliability, and thermal stability, thus enabling the suitable formation of protective films and insulating layers.

[0249] As a maleimide compound (D), from the viewpoint of exhibiting better curability, superior heat resistance and thermal stability, better solubility in solvents, low melting point, low water absorption, and better compatibility with other resins, it is preferable to include at least one of the compounds selected from the group consisting of the compound shown in formula (6), the compound shown in formula (7), and the compound shown in formula (8), more preferably including at least one of the group consisting of the compound shown in formula (6) and the compound shown in formula (7), and even more preferably including the compound shown in formula (7).

[0250] Next, the compounds shown in formula (6) to formula (11) contained in maleimide compound (D) will be described.

[0251] (The compound shown in formula (6))

[0252] The compound shown in formula (6) is the following compound.

[0253]

[0254] In equation (6), R 13 R 14 and R 15 Each can independently represent a hydrogen atom, or an alkyl group having 1 to 8 carbon atoms with optional substituents, either straight-chain or branched.

[0255] Examples of linear or branched alkyl groups having 1 to 8 carbon atoms and optionally containing substituents include methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl, tert-butyl, n-pentyl, 1-ethylpropyl, 2,2-dimethylpropyl, cyclopentyl, hexyl, and heptyl. The hydrogen atoms in these alkyl groups may optionally be substituted with halogen atoms such as fluorine and chlorine atoms, or with cyano groups. From the viewpoint of superior photocurability, heat resistance, and thermal stability, as well as good solubility in solvents, low melting point, low water absorption, and good compatibility with other resins, methyl, ethyl, isopropyl, and tert-butyl are preferred, more preferably methyl, ethyl, and isopropyl, and even more preferably methyl.

[0256] From the viewpoint of exhibiting superior photocurability, heat resistance and thermal stability, solubility in solvents, low melting point, low water absorption, and compatibility with other resins, the compound shown in formula (6) is even more preferred. The compound shown in formula (24) (also referred to as TMDM in this embodiment) is preferred.

[0257]

[0258] (The compound shown in formula (7))

[0259] The compound shown in formula (7) is the following compound.

[0260]

[0261] In equation (7), R 16 R 17 and R 18 Each of the following can independently represent a hydrogen atom, a hydroxyl group, or an alkyl group with 1 to 6 carbon atoms that may have a substituent. n2 represents an integer from 1 to 10.

[0262] As a straight-chain or branched alkyl group having 1 to 6 carbon atoms, R can be referred to in the aforementioned formula (4). 12 As an alkyl group, from the viewpoint of exhibiting better solubility in solvents, low melting point, low water absorption, and better compatibility with other resins, methyl, ethyl, n-propyl, and isopropyl are preferred, with methyl being more preferred.

[0263] Additionally, R 16 R 17 and R 18 From the viewpoint of exhibiting superior solubility in solvents, R is preferred. 16 and R 18 It is a straight-chain or branched alkyl group having 1 to 6 carbon atoms, and R 17It consists of hydrogen atoms. It should be noted that the preferred alkyl group is as described above.

[0264] From the viewpoint that it has better solubility in solvents, can obtain a more suitable viscosity, and can further control the viscosity rise of the varnish, n2 is preferably an integer from 1 to 10, and more preferably an integer from 1 to 6.

[0265] As the compound shown in formula (7), commercially available products can be used, such as the compound shown in formula (25) (BCPH01 (trade name, Mw / Mn = 1.0 to 1.8) and BCPH13 (trade name, Mw / Mn = 1.0 to 1.6) manufactured by Kunei Chemical Industry Co., Ltd.) and the compound shown in formula (26) (BMCX426 (trade name) manufactured by Kunei Chemical Industry Co., Ltd.).

[0266]

[0267] In equation (25), n 21 It is an integer from 1 to 5.

[0268]

[0269] In equation (26), n 22 It is an integer from 1 to 10.

[0270] (The compound shown in formula (8))

[0271] The compound shown in formula (8) is the following compound.

[0272]

[0273] In equation (8), R 19 Each can independently represent a hydrogen atom, a methyl group, or an ethyl group; R 20 Each can be used independently to represent a hydrogen atom or a methyl group.

[0274] As R 19 From the viewpoint of exhibiting better solubility in solvents, low melting point, low water absorption, and better compatibility with other resins, methyl or ethyl resins are preferred.

[0275] As R 20 From the viewpoint of exhibiting better solubility in solvents, low melting point, low water absorption, and better compatibility with other resins, hydrogen atoms are preferred.

[0276] As the maleimide compound shown in formula (8), commercially available products can be used, such as BMI-70 (trade name) manufactured by KI Chemical Co., Ltd., as shown in formula (27).

[0277]

[0278] (The compound shown in formula (9))

[0279] The compound shown in formula (9) is the following compound.

[0280]

[0281] In equation (9), R 21 Each can independently represent a hydrogen atom or a methyl group. n3 represents an integer from 1 to 10.

[0282] As the maleimide compound shown in formula (9), commercially available products can be used, such as MIR-3000 (trade name) manufactured by Nippon Kayaku Co., Ltd., as shown in formula (28).

[0283]

[0284] In equation (28), n 31 It is an integer from 1 to 10.

[0285] (The compound shown in formula (10))

[0286] The compound represented by formula (10) is the following compound.

[0287]

[0288] In equation (10), R 22 Each can independently represent a hydrogen atom, a methyl group, or an ethyl group.

[0289] As R 22 From the viewpoint of exhibiting better solubility in solvents, low melting point, low water absorption, and better compatibility with other resins, methyl or ethyl resins are preferred.

[0290] As the maleimide compound shown in formula (10), commercially available products can be used, such as BMI-80 (trade name) manufactured by KI Chemical Co., Ltd., as shown in formula (29).

[0291]

[0292] (The compound shown in formula (11))

[0293] The compound shown in formula (11) is the following compound.

[0294]

[0295] In equation (11), R 23 Each can independently represent a hydrogen atom or a methyl group. n4 represents an integer from 1 to 10.

[0296] As R 23 From the viewpoint of exhibiting better solubility in solvents, low melting point, low water absorption, and better compatibility with other resins, hydrogen atoms are preferred.

[0297] From the viewpoint that n4 has better solubility in solvents, can obtain a more suitable viscosity, and can further control the increase in viscosity of the varnish, it is more preferable to be an integer from 1 to 5.

[0298] As the maleimide compound shown in formula (11), commercially available products can be used, such as BMI-2300 (trade name) manufactured by Yamato Chemical Industries Co., Ltd., as shown in formula (30).

[0299]

[0300] In equation (30), n 41 It is an integer from 1 to 5.

[0301] From the viewpoint of obtaining better heat resistance and thermal stability, the total content of maleimide compound (D) in the resin composition preferably includes 10 to 90 parts by mass of 100 parts by mass of the resin solids in the resin composition, more preferably 20 to 70 parts by mass, and even more preferably 30 to 60 parts by mass.

[0302] Furthermore, from the viewpoint of obtaining better heat resistance and thermal stability, the total content of maleimide compound (D) in the resin composition preferably includes 10 to 90 parts by mass relative to a total of 100 parts by mass of bismaleimide compound (A) and maleimide compound (D), more preferably 20 to 70 parts by mass, and even more preferably 30 to 60 parts by mass.

[0303] When the resin composition contains bismaleimide compound (A) and initiator (B), as well as compounds (C) and (D), from the viewpoint of obtaining better heat resistance and thermal stability, the content of maleimide compound (D) is preferably 10 to 85 parts by mass relative to a total of 100 parts by mass of bismaleimide compound (A), initiator (B), compound (C), and compound (D), more preferably 15 to 80 parts by mass, further preferably 20 to 45 parts by mass, and even more preferably 25 to 44 parts by mass.

[0304] [Other maleimide compounds]

[0305] The resin composition of this embodiment may further comprise other maleimide compounds different from bismaleimide compound (A) and maleimide compound (D). Such other maleimide compounds are not particularly limited as long as they are compounds having one or more maleimide groups in their molecules. Other maleimide compounds include, for example, N-phenylmaleimide, N-cyclohexylmaleimide, N-hydroxyphenylmaleimide, N-anilinephenylmaleimide, N-carboxyphenylmaleimide, N-(4-carboxy-3-hydroxyphenyl)maleimide, 6-maleimide hexanoic acid, 4-maleimide butyric acid, bis(4-maleimidephenyl)methane, 2,2-bis(4-(4-maleimidephenoxy)-phenyl)propane, 4,4-diphenylmethane bismaleimide, bis(3,5-dimethyl-4-maleimidephenyl)methane, bis(3-ethylhexyl)propane, etc. 5-methyl-4-maleimide phenyl)methane, bis(3,5-diethyl-4-maleimide phenyl)methane, phenylmethane maleimide, o-phenylene bismaleimide, m-phenylene bismaleimide, p-phenylene bismaleimide, o-phenylene bisciconimide, m-phenylene bisciconimide, p-phenylene bisciconimide, 2,2-bis(4-(4-maleimide phenoxy)-phenyl)propane, 3,3-dimethyl-5,5-diethyl-4,4-diphenylmethane bismaleimide, 4-methyl-1,3-phenylene bismaleimide, 1,2-bismaleimide Imine ethane, 1,4-bismaleimide butane, 1,5-bismaleimide pentane, 1,5-bismaleimide-2-methylpentane, 1,6-bismaleimide hexane, 1,6-bismaleimide-(2,2,4-trimethyl)hexane, 1,8-bismaleimide-3,6-dioxaoctane, 1,11-bismaleimide-3,6,9-trioxaundecane, 1,3-bis(maleimidemethyl)cyclohexane, 1,4-bis(maleimidemethyl)cyclohexane, 4,4-diphenyl ether bismaleimide, 4,4-diphenyl sulfone bismaleimide, 1,3-bis... (3-maleimide phenoxy)benzene, 1,3-bis(4-maleimide phenoxy)benzene, 4,4-diphenylmethane bisciconimide, 2,2-bis[4-(4-ciconimide phenoxy)phenyl]propane, bis(3,5-dimethyl-4-ciconimide phenyl)methane, bis(3-ethyl-5-methyl-4-ciconimide phenyl)methane, bis(3,5-diethyl-4-ciconimide phenyl)methane, polyphenylmethane maleimide, fluorescein-5-maleimide, and prepolymers of these maleimide compounds, as well as prepolymers of maleimide compounds and amine compounds, etc. These maleimide compounds can be used alone or in appropriate mixtures of two or more.

[0306] As for other maleimide compounds, compounds with excellent light transmittance are preferred.

[0307] When other maleimide compounds are included in the resin composition, the total content of the other maleimide compounds is usually about 0.01 to 40 parts by weight per 100 parts by weight of the resin solids in the resin composition.

[0308] [Filling material]

[0309] In the resin composition of this embodiment, a filler material can be used to further improve various properties such as coating properties and heat resistance. As a filler material, it is preferable to have insulating properties and not impede the transmittance to various active energy rays used for photocuring, and more preferably to have transmittance to active energy rays including wavelengths of 365 nm (i-rays).

[0310] Examples of filler materials include silica (such as natural silica, fused silica, amorphous silica, and hollow silica), aluminum compounds (such as boehmite, aluminum hydroxide, aluminum oxide, and aluminum nitride), boron compounds (such as boron nitride), magnesium compounds (such as magnesium oxide and magnesium hydroxide), calcium compounds (such as calcium carbonate), molybdenum compounds (such as molybdenum oxide and zinc molybdate), barium compounds (such as barium sulfate and barium silicate), talc (such as natural talc and calcined talc), mica, glass (such as short-fiber glass, spherical glass, micronized glass, E glass, T glass, and D glass), silicone powder, fluoropolymer fillers, urethane resin fillers, (meth)acrylic resin fillers, polyethylene fillers, styrene-butadiene rubber, and silicone rubber. These fillers can be used alone or in appropriate combinations of two or more.

[0311] Among these, preferably one or more are selected from the group consisting of silica, boehmite, barium sulfate, organosilicon powder, fluoropolymer filler, urethane resin filler, (meth)acrylic resin filler, polyethylene filler, styrene-butadiene rubber, and organosilicon rubber.

[0312] These filler materials can be surface-treated with silane coupling agents, etc., as described later.

[0313] From the viewpoint of further improving the heat resistance of the cured product and obtaining better coating properties, silica is preferred, and fused silica is more preferred. Specific examples of silica include SFP-130MC (trade name) manufactured by Denka, SC2050-MB (trade name), SC1050-MLE (trade name), YA010C-MFN (trade name), and YA050C-MJA (trade name) manufactured by Admatechs.

[0314] The particle size of the filler material is not particularly limited, but from the viewpoint of further improving the ultraviolet light transmittance of the resin composition, it is generally 0.005 to 10 μm, preferably 0.01 to 1.0 μm.

[0315] In resin compositions, from the viewpoint of improving the light transmittance of the resin composition and the heat resistance of the cured product, the content of filler material is generally preferably 300 parts by mass or less, more preferably 200 parts by mass or less, and even more preferably 100 parts by mass or less, relative to 100 parts by mass of the resin solids in the resin composition. It should be noted that, when filler material is included, from the viewpoint of obtaining effects that further improve coating properties, heat resistance, and other characteristics, the lower limit value is generally 1 part by mass relative to 100 parts by mass of the resin solids in the resin composition.

[0316] [Silane coupling agents and wetting and dispersing agents]

[0317] In the resin composition of this embodiment, in order to further improve the dispersibility of the filler material and the adhesion strength between the polymer and / or the resin and the filler material, a combination of silane coupling agent and / or wetting and dispersing agent may be used.

[0318] As for these silane coupling agents, there are no particular limitations, mainly those commonly used in the surface treatment of inorganic materials. Examples include 3-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, 3-aminopropyldimethoxymethylsilane, 3-aminopropyldiethoxymethylsilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminopropyldimethoxymethylsilane, N-(2-aminoethyl)-3-aminopropyldiethoxymethylsilane, N-phenyl-3-aminopropyltrimethoxysilane, N-phenyl-3-aminopropyltriethoxysilane, [3-(6-aminohexylamino)propyl]trimethoxysilane, and [3-(N,N [-dimethylamino)-propyl]trimethoxysilane and other aminosilane series; γ-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropyldimethoxymethylsilane, 3-glycidoxypropyldiethoxymethylsilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane and [8-(glycidoxy)-n-octyl]trimethoxysilane and other epoxysilane series; vinyltris(2-methoxyethoxy)silane, vinyltrimethoxysilane, vinyltriethoxysilane, dimethoxymethylvinylsilane, diethoxymethylvinylsilane, trimethoxy(7-octen-1-yl)silane and trimethoxy... 4-Vinylphenyl)silanes and other vinylsilanes; 3-methacryloyloxypropyltrimethoxysilane, 3-methacryloyloxypropyltriethoxysilane, 3-methacryloyloxypropyldimethoxymethylsilane, 3-methacryloyloxypropyldiethoxymethylsilane and other methacryloylsilanes; 3-acryloyloxypropyltrimethoxysilane and 3-acryloyloxypropyltriethoxysilane and other acryloylsilanes; 3-isocyanopropyltrimethoxysilane and 3-isocyanopropyltriethoxysilane and other isocyanate silanes; tri-(trimethoxysilylpropyl)isocyanurate and other isocyanurate silanes; 3-mercaptopropyltrimethoxysilane The silane coupling agents include mercaptosilanes such as 3-mercaptopropyldimethoxymethylsilane; ureosilanes such as 3-ureopropyltriethoxysilane; styrylsilanes such as p-styryltrimethoxysilane; cationic silanes such as N-β-(N-vinylbenzylaminoethyl-γ-aminopropyltrimethoxysilane hydrochloride); acid anhydride systems such as [3-(trimethoxysilyl)propyl]succinic anhydride; phenylsilanes such as phenyltrimethoxysilane, phenyltriethoxysilane, dimethoxymethylphenylsilane, diethoxymethylphenylsilane, and p-tolyltrimethoxysilane; and arylsilanes such as trimethoxy(1-naphthyl)silane. These silane coupling agents can be used alone or in appropriate combinations of two or more.

[0319] In resin compositions, the content of silane coupling agent is typically 0.1 to 10 parts by weight relative to 100 parts by weight of the solid resin component in the resin composition.

[0320] As a wetting and dispersing agent, there are no particular limitations as long as it is a dispersing stabilizer used in coating applications. Specific examples include BYK Japan's DISPERBYK (registered trademark)-110, 111, 118, 180, 161, BYK (registered trademark)-W996, W9010, and W903 (trade names). These wetting and dispersing agents can be used alone or in appropriate combinations of two or more.

[0321] In resin compositions, the content of wetting and dispersing agents is typically 0.1 to 10 parts by weight relative to 100 parts by weight of the resin solids in the resin composition.

[0322] [Cyanate ester compounds, phenolic resins, oxetane resins, benzoxazine compounds, epoxy resins, and other compounds]

[0323] In this embodiment, as long as the effects of the present invention are achieved, various compounds and resins, excluding bismaleimide compound (A), photocuring initiator (B), compound (C), maleimide compound (D), and other maleimide compounds, such as cyanate ester compounds, phenolic resins, oxetane resins, benzoxazine compounds, epoxy resins, and other compounds, can be used based on the flame retardancy, heat resistance, and thermal expansion characteristics of the cured product. Furthermore, regarding these compounds and resins, it is preferable that the resin composition undergoes photocuring by exposure to active energy rays containing a wavelength of 365 nm (i-rays).

[0324] These compounds and resins can be used alone or in appropriate combinations of two or more.

[0325] <Cyanate compounds>

[0326] As a cyanate compound, there are no particular limitations as long as it is a resin having an aromatic moiety that is substituted by at least one cyanooxy group (cyanate group) within the molecule.

[0327] Examples of compounds can be listed, such as those shown in formula (31).

[0328]

[0329] In formula (31), Ar1 represents a benzene ring, a naphthalene ring, or a group consisting of two benzene rings bonded by a single bond. Multiple Ar1 groups may be identical or different. Ra independently represents a hydrogen atom, an alkyl group with 1 to 6 carbon atoms, an alkenyl group with 2 to 6 carbon atoms, an aryl group with 6 to 12 carbon atoms, an alkoxy group with 1 to 4 carbon atoms, or a group consisting of an alkyl group with 1 to 6 carbon atoms bonded to an aryl group with 6 to 12 carbon atoms. The aromatic ring in Ra may optionally have substituents, and the substituents in Ar1 and Ra may be in any position. p represents the number of cyanoxy groups bonded to Ar1, each being an integer from 1 to 3. q represents the number of Ra groups bonded to Ar1, which is 4-p when Ar1 is a benzene ring, 6-p when Ar1 is a naphthalene ring, and 8-p when Ar1 is a group consisting of two benzene rings bonded by a single bond. t represents the average number of repetitions, an integer from 0 to 50, and the cyanate ester compound may be a mixture of compounds with different t values. In the presence of multiple X's, each X independently represents a single bond, a divalent organic group with 1 to 50 carbon atoms (with hydrogen atoms optionally replaced by heteroatoms), a divalent organic group with 1 to 10 nitrogen atoms (e.g., -NRN-, where R represents an organic group), a carbonyl group (-CO-), a carboxyl group (-C(=O)O-), a carbonyl dioxy group (-OC(=O)O-), a sulfonyl group (-SO2-), a divalent sulfur atom, or a divalent oxygen atom.

[0330] The alkyl group in Ra of formula (31) can have either a straight or branched chain structure, or a cyclic structure (such as cycloalkyl).

[0331] In addition, the hydrogen atoms in the alkyl group in formula (31) and the aryl group in Ra can be optionally replaced by halogen atoms such as fluorine and chlorine atoms, alkoxy groups such as methoxy and phenoxy groups, or cyano groups.

[0332] Specific examples of alkyl groups include methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl, tert-butyl, n-pentyl, 1-ethylpropyl, 2,2-dimethylpropyl, cyclopentyl, hexyl, cyclohexyl, and trifluoromethyl.

[0333] Specific examples of alkenyl groups include vinyl, (methyl)allyl, isopropenyl, 1-propenyl, 2-butenyl, 3-butenyl, 1,3-butadienyl, 2-methyl-2-propenyl, 2-pentenyl, and 2-hexenyl.

[0334] Specific examples of aryl groups include phenyl, xylyl, mesitylene, naphthyl, phenoxyphenyl, ethylphenyl, o-fluorophenyl, m-fluorophenyl, p-fluorophenyl, dichlorophenyl, dicyanophenyl, trifluorophenyl, methoxyphenyl, and o-tolyl, m-tolyl, or p-tolyl.

[0335] Examples of alkoxy groups include methoxy, ethoxy, propoxy, isopropoxy, n-butoxy, isobutoxy, and tert-butoxy.

[0336] Specific examples of divalent organic groups with 1 to 50 carbon atoms in X of formula (31) include methylene, ethylene, trimethylene, cyclopentylene, cyclohexylene, trimethylcyclohexylene, biphenylmethylene, dimethylmethylene-phenylene-dimethylmethylene, fluorenediyl, and phthalidediyl. The hydrogen atoms in the divalent organic group may be optionally replaced by halogen atoms such as fluorine and chlorine atoms, alkoxy groups such as methoxy and phenoxy groups, and cyano groups.

[0337] Examples of divalent organic groups with nitrogen number 1 to 10 in X of formula (31) include imino and polyimide groups.

[0338] In addition, as an organic group of X in formula (31), examples include groups having the structure shown in formula (32) or groups having the structure shown in formula (33).

[0339]

[0340] In formula (32), Ar2 represents phenyldiyl, naphthyl, or biphenyldiyl, and these can be the same or different from each other when u is an integer of 2 or more. Rb, Rc, Rf, and Rg each independently represent a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an aryl group having 6 to 12 carbon atoms, a trifluoromethyl group, or an aryl group having at least one phenolic hydroxyl group. Rd and Re each independently select from any one of a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an aryl group having 6 to 12 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, or a hydroxyl group. u represents an integer from 0 to 5.

[0341]

[0342] In formula (33), Ar3 represents phenyldiyl, naphthyl, or biphenyldiyl, which may be the same or different from each other when v is an integer of 2 or more. Ri and Rj each independently represent a hydrogen atom, an alkyl group with 1 to 6 carbon atoms, an aryl group with 6 to 12 carbon atoms, a benzyl group, an alkoxy group with 1 to 4 carbon atoms, a hydroxyl group, a trifluoromethyl group, or an aryl group substituted with at least one cyanoxy group. v represents an integer of 0 to 5, or may be a mixture of compounds with different v.

[0343] Furthermore, as X in formula (31), divalent groups can be listed as shown in the following formula.

[0344] -O- -S-

[0345] Here, z represents an integer from 4 to 7. Rk independently represents either a hydrogen atom or an alkyl group with 1 to 6 carbon atoms.

[0346] As specific examples of Ar2 in formula (32) and Ar3 in formula (33), examples include phenyldiyl groups with two carbon atoms as shown in formula (32) or two oxygen atoms as shown in formula (33) bonded to the 1,4 or 1,3 positions; biphenyldiyl groups with two carbon atoms or two oxygen atoms bonded to the 4,4', 2,4', 2,2', 2,3', 3,3' or 3,4' positions; and naphthyl groups with two carbon atoms or two oxygen atoms bonded to the 2,6, 1,5, 1,6, 1,8, 1,3, 1,4 or 2,7 positions.

[0347] The alkyl and aryl groups in Rb, Rc, Rd, Re, Rf and Rg in formula (32) and Ri and Rj in formula (33) have the same meaning as in formula (31).

[0348] Specific examples of cyanooxy-substituted aromatic compounds represented by formula (31) include cyanooxybenzene, 1-cyanooxy-2-methylbenzene, 1-cyanooxy-3-methylbenzene, 1-cyanooxy-4-methylbenzene, 1-cyanooxy-2-methoxybenzene, 1-cyanooxy-3-methoxybenzene, 1-cyanooxy-4-methoxybenzene, 1-cyanooxy-2,3-dimethylbenzene, 1-cyanooxy-2,4-dimethylbenzene, 1-cyanooxy-2,5-dimethylbenzene, 1-cyanooxy-2,6-dimethylbenzene, 1-cyanooxy-3,4-dimethylbenzene, 1-cyanooxy-3,5-dimethylbenzene, cyanooxy-2,6-dimethylbenzene, 1-cyanooxy-3,4-dimethylbenzene, 1-cyanooxy-3,5-dimethylbenzene, cyanooxyethylbenzene, cyanooxybutylbenzene, cyanooxyoctylbenzene, cyanooxynonylbenzene, and 2-(4-cyanooxyphenyl)-2-phenylpropane. Alkane (cyanate ester of 4-α-cumylphenol), 1-cyanooxy-4-cyclohexylbenzene, 1-cyanooxy-4-vinylbenzene, 1-cyanooxy-2-chlorobenzene, 1-cyanooxy-3-chlorobenzene, 1-cyanooxy-2,6-dichlorobenzene, 1-cyanooxy-2-methyl-3-chlorobenzene, cyanooxynitrobenzene, 1-cyanooxy-4-nitro-2-ethylbenzene, 1-cyanooxy-2-methoxy-4-allylbenzene (cyanate ester of eugenol), methyl (4-cyanooxyphenyl) sulfide, 1-cyanooxy-3-trifluoromethylbenzene, 4-cyanooxybiphenyl, 1-cyanooxy-2-acetylbenzene, 1-cyanooxy-4-acetylbenzene, 4-cyanooxybenzaldehyde, methyl 4-cyanooxybenzoate, phenyl 4-cyanooxybenzoate, 1-cyanooxy 4-Acetaminophen, 4-Cyanoxybenzophenone, 1-Cyanoxy-2,6-di-tert-butylbenzene, 1,2-Dicyanoxybenzene, 1,3-Dicyanoxybenzene, 1,4-Dicyanoxybenzene, 1,4-Dicyanoxy-2-tert-butylbenzene, 1,4-Dicyanoxy-2,4-Dimethylbenzene, 1,4-Dicyanoxy-2,3,4-Dimethylbenzene, 1,3-Dicyanoxy-2,4,6-Trimethylbenzene, 1,3-Dicyanoxy-5-Methylbenzene, 1-Cyanoxynaphthalene, 2-Cyanoxynaphthalene, 1-Cyanoxy-4-methoxynaphthalene, 2-Cyanoxy-6-methoxynaphthalene, 2-Cyanoxy-7-methoxynaphthalene, 2,2'-Dicyanoxy-1,1'-Binaphthalene, 1,3-Dicyanoxynaphthalene, 1,4-Dicyanoxynaphthalene 1,5-Dicyanoxynaphthalene, 1,6-Dicyanoxynaphthalene, 1,7-Dicyanoxynaphthalene, 2,3-Dicyanoxynaphthalene, 2,6-Dicyanoxynaphthalene, 2,7-Dicyanoxynaphthalene, 2,2'-Dicyanoxybiphenyl, 4,4'-Dicyanoxybiphenyl, 4,4'-Dicyanoxyoctafluorobiphenyl, 2,4'-Dicyanoxydiphenylmethane, 4,4'-Dicyanoxydiphenylmethane, bis(4-cyanoxy-3,5-dimethylphenyl)methane, 1,1-bis(4-cyanoxyphenyl)ethane, 1,1-bis(4-cyanoxyphenyl)propane, 2,2-bis(4-cyanoxyphenyl)propane, 2,2-bis(4-cyanoxy-3-methylphenyl)propane, 2,2-bis(2-cyanoxy-5-biphenyl)propane, 2,2-Bis(4-cyanoxyphenyl)hexafluoropropane, 2,2-bis(4-cyanoxy-3,5-dimethylphenyl)propane, 1,1-bis(4-cyanoxyphenyl)butane, 1,1-bis(4-cyanoxyphenyl)isobutane, 1,1-bis(4-cyanoxyphenyl)pentane, 1,1-bis(4-cyanoxyphenyl)-3-methylbutane, 1,1-bis(4-cyanoxyphenyl)-2-methylbutane, 1,1-bis(4-cyanoxyphenyl)-2,2-dimethylpropane, 2,2-bis(4-cyanoxyphenyl)butane, 2,2-bis(4-cyanoxyphenyl)pentane, 2,2-bis(4-cyanoxyphenyl)hexane, 2,2-bis(4-cyanoxyphenyl)-3-methylbutane, 2,2-bis(4-cyanoxyphenyl)hexane 4-Methylpentane, 2,2-bis(4-cyanoxyphenyl)-3,3-dimethylbutane, 3,3-bis(4-cyanoxyphenyl)hexane, 3,3-bis(4-cyanoxyphenyl)heptane, 3,3-bis(4-cyanoxyphenyl)octane, 3,3-bis(4-cyanoxyphenyl)-2-methylpentane, 3,3-bis(4-cyanoxyphenyl)-2-methylhexane, 3,3-bis(4-cyanoxyphenyl)-2,2-dimethylpentane, 4,4-bis(4-cyanoxyphenyl)-3-methylheptane, 3,3-bis(4-cyanoxyphenyl)-2-methylheptane, 3,3-bis(4-cyanoxyphenyl)-2,2-dimethylhexane, 3,3-bis(4-cyanoxyphenyl)-2,4-dimethylhexane, 3 3-bis(4-cyanoxyphenyl)-2,2,4-trimethylpentane, 2,2-bis(4-cyanoxyphenyl)-1,1,1,3,3,3-hexafluoropropane, bis(4-cyanoxyphenyl)phenylmethane, 1,1-bis(4-cyanoxyphenyl)-1-phenylethane, bis(4-cyanoxyphenyl)biphenylmethane, 1,1-bis(4-cyanoxyphenyl)cyclopentane, 1,1-bis(4-cyanoxyphenyl)cyclohexane, 2,2-bis(4-cyanoxy-3-isopropylphenyl)propane, 1,1-bis(3-cyclohexyl-4-cyanoxyphenyl)cyclohexane, bis(4-cyanoxyphenyl)diphenylmethane, bis(4-cyanoxyphenyl)-2,2-dichloroethylene, 1,3-bis[2-(4-cyanoxyphenyl)-2- [Propyl]benzene, 1,4-bis[2-(4-cyanoxyphenyl)-2-propyl]benzene, 1,1-bis(4-cyanoxyphenyl)-3,3,5-trimethylcyclohexane, 4-[bis(4-cyanoxyphenyl)methyl]biphenyl, 4,4-dicyanoxybenzophenone, 1,3-bis(4-cyanoxyphenyl)-2-propen-1-one, bis(4-cyanoxyphenyl) ether, bis(4-cyanoxyphenyl) sulfide, bis(4-cyanoxyphenyl) sulfone, 4-cyanoxybenzoic acid-4-cyanoxyphenyl ester (4-cyanoxyphenyl-4-cyanoxybenzoate), bis-(4-cyanoxyphenyl) carbonate, 1,3-bis(4-cyanoxyphenyl)adamantane, 1,3-bis(4-cyanoxyphenyl)-5,7-dimethyladamantane, 3,3-Bis(4-cyanoxyphenyl)isobenzofuran-1(3H)-one (cyanate ester of phenolphthalein), 3,3-bis(4-cyanoxy-3-methylphenyl)isobenzofuran-1(3H)-one (cyanate ester of o-cresolphthalein), 9,9'-bis(4-cyanoxyphenyl)fluorene, 9,9-bis(4-cyanoxy-3-methylphenyl)fluorene, 9,9-bis(2-cyanoxy-5-biphenyl)fluorene, tris(4-cyanoxyphenyl)methane, 1,1,1-tris(4-cyanoxyphenyl)methane α,α,α'-tris(4-cyanooxyphenyl)ethane, 1,1,3-tris(4-cyanooxyphenyl)propane, α,α,α'-tris(4-cyanooxyphenyl)-1-ethyl-4-isopropylbenzene, 1,1,2,2-tetra(4-cyanooxyphenyl)ethane, tetra(4-cyanooxyphenyl)methane, 2,4,6-tris(N-methyl-4-cyanooxyaniline)-1,3,5-triazine, 2,4-bis(N-methyl-4-cyanooxyaniline)-6-(N-methylaniline)- 1,3,5-Triazine, bis(N-4-cyanoxy-2-methylphenyl)-4,4'-oxophthalimide, bis(N-3-cyanoxy-4-methylphenyl)-4,4'-oxophthalimide, bis(N-4-cyanoxyphenyl)-4,4'-oxophthalimide, bis(N-4-cyanoxy-2-methylphenyl)-4,4'-(hexafluoroisopropyl)diphthalimide, tris(3,5-dimethyl-4-cyanoxy) Benzyl isocyanurate, 2-phenyl-3,3-bis(4-cyanoxyphenyl)benzo[C]pyrrolidone, 2-(4-methylphenyl)-3,3-bis(4-cyanoxyphenyl)benzo[C]pyrrolidone, 2-phenyl-3,3-bis(4-cyanoxyphenyl)benzo[C]pyrrolidone, 1-methyl-3,3-bis(4-cyanoxyphenyl)indololin-2-one and 2-phenyl-3,3-bis(4-cyanoxyphenyl)indololin-2-one.

[0349] These cyanate compounds can be used alone or in appropriate combinations of two or more.

[0350] Other specific examples of the cyanate ester compounds shown in formula (31) include: phenol-formaldehyde varnish resins and cresol-formaldehyde varnish resins (substances obtained by reacting phenol, alkyl-substituted phenol, or halogen-substituted phenol with formaldehyde compounds such as formaldehyde or paraformaldehyde in an acidic solution using known methods), triphenol-formaldehyde varnish resins (substances obtained by reacting hydroxybenzaldehyde with phenol in the presence of an acidic catalyst), and fluorene-formaldehyde varnish resins (substances obtained by reacting fluorene ketone compounds with 9,9-bis(hydroxyaryl)fluorenes in an acidic solution). Substances obtained by reacting in the presence of an acidic catalyst), phenolic aralkyl resins, cresol aralkyl resins, naphthol aralkyl resins, and biphenyl aralkyl resins (substances obtained by reacting a dihalomethyl compound as shown in Ar4-(CH2Y)2 (Ar4 represents phenyl, Y represents a halogen atom. The same applies hereinafter in this paragraph) with a phenolic compound using a known method, either in the presence or without a catalyst; bis(alkoxymethyl) compounds as shown in Ar4-(CH2OR)2 (R represents alkyl). Substances obtained by reacting a bis(hydroxymethyl) compound with a phenolic compound in the presence of an acidic catalyst; or substances obtained by reacting a bis(hydroxymethyl) compound, such as Ar4-(CH2OH)2, with a phenolic compound in the presence of an acidic catalyst; or substances obtained by condensing an aromatic aldehyde compound with an aralkyl compound and a phenolic compound; phenol-modified xyleneformaldehyde resin (substance obtained by reacting xyleneformaldehyde resin with a phenolic compound in the presence of an acidic catalyst using a known method); modified naphthaldehyde resin (substance obtained by reacting naphthaldehyde resin with a hydroxyl-substituted aromatic compound in the presence of an acidic catalyst using a known method); phenol-modified dicyclopentadiene resin or phenolic resin having a polynaphthalene ether structure (substance obtained by dehydrating and condensing a polyhydroxynaphthalene compound having two or more phenolic hydroxyl groups in one molecule in the presence of an alkaline catalyst using a known method); and other phenolic resins obtained by cyanate esterification using the same methods as described above, as well as their prepolymers. These cyanate ester compounds can be used alone or in appropriate combinations of two or more.

[0351] There are no particular limitations on the method for producing these cyanate ester compounds, and known methods can be used. Specific examples include purchasing or synthesizing hydroxyl-containing compounds with a desired skeleton and modifying the hydroxyl groups using known methods to induce cyanate esterification. Methods for inducing cyanate esterification of hydroxyl groups include, for example, those described in Ian Hamerton, "Chemistry and Technology of Cyanate Ester Resins," Blackie Academic & Professional.

[0352] Cured products using these cyanate compounds exhibit superior properties such as glass transition temperature, low thermal expansion, and coating adhesion.

[0353] In the resin composition, the content of the cyanate ester compound is 0.01 to 40 parts by weight relative to 100 parts by weight of the resin solids in the resin composition.

[0354] Phenolic resin

[0355] As for phenolic resins, any phenolic resin having two or more hydroxyl groups in one molecule can use commonly known substances. Examples of phenolic resins include bisphenol A type phenolic resin, bisphenol E type phenolic resin, bisphenol F type phenolic resin, bisphenol S type phenolic resin, phenolic varnish resin, bisphenol A phenolic varnish type phenolic resin, glycidyl ester type phenolic resin, aralkyl phenolic varnish type phenolic resin, biphenyl aralkyl type phenolic resin, cresol phenolic varnish type phenolic resin, polyfunctional phenolic resin, naphthol resin, naphthol phenolic varnish resin, polyfunctional naphthol resin, anthracene type phenolic resin, naphthalene skeleton modified phenolic varnish type phenolic resin, phenol aralkyl type phenolic resin, naphthol aralkyl type phenolic resin, dicyclopentadiene type phenolic resin, biphenyl type phenolic resin, alicyclic phenolic resin, polyol type phenolic resin, phosphorus-containing phenolic resin, phenolic resin containing polymerizable unsaturated hydrocarbon groups, and hydroxyl-containing organosilicon resins. These phenolic resins can be used alone or in appropriate mixtures of two or more.

[0356] In the resin composition, the content of phenolic resin is 0.01 to 40 parts by weight relative to 100 parts by weight of the solid resin component in the resin composition.

[0357] <Oxycyclobutane resin>

[0358] As oxetane resins, commonly known substances can be used. Examples include oxetane, 2-methyloxetane, 2,2-dimethyloxetane, 3-methyloxetane, 3,3-dimethyloxetane and other alkyloxetanes, 3-methyl-3-methoxymethyloxetane, 3,3-di(trifluoromethyl)perfluorooxetane, 2-chloromethyloxetane, 3,3-bis(chloromethyl)oxetane, biphenyl-type oxetane, OXT-101 (manufactured by Toa Synthetic Co., Ltd., trade name), OXT-121 (manufactured by Toa Synthetic Co., Ltd., trade name), and OXT-221 (manufactured by Toa Synthetic Co., Ltd., trade name), etc. These oxetane resins can be used alone or in appropriate mixtures of two or more.

[0359] In the resin composition, the content of oxetane resin is 0.01 to 40 parts by weight relative to 100 parts by weight of the resin solids in the resin composition.

[0360] <Benzoxazine compounds>

[0361] As benzoxazine compounds, any compound having two or more dihydrobenzoxazine rings in one molecule can use commonly known substances. Examples include bisphenol A type benzoxazine BA-BXZ (trade name, manufactured by Konishi Chemical Industry Co., Ltd.), bisphenol F type benzoxazine BF-BXZ (trade name, manufactured by Konishi Chemical Industry Co., Ltd.), bisphenol S type benzoxazine BS-BXZ (trade name, manufactured by Konishi Chemical Industry Co., Ltd.), Pd type benzoxazine (trade name, manufactured by Shikoku Chemical Industry Co., Ltd.), Fa type benzoxazine (trade name, manufactured by Shikoku Chemical Industry Co., Ltd.), and phenolphthalein type benzoxazine, etc. These benzoxazine compounds can be used alone or in appropriate combinations of two or more.

[0362] In the resin composition, the content of benzoxazine compound is 0.01 to 40 parts by weight relative to 100 parts by weight of the resin solids in the resin composition.

[0363] <Epoxy Resin>

[0364] There are no particular limitations on epoxy resins; commonly known substances can be used. Examples include bisphenol A type epoxy resin, bisphenol E type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, bisphenol A phenolic varnish epoxy resin, biphenyl type epoxy resin, phenolic varnish epoxy resin, cresol phenolic varnish epoxy resin, xylene phenolic varnish epoxy resin, polyfunctional phenol type epoxy resin, naphthalene type epoxy resin, naphthalene skeleton modified phenolic varnish epoxy resin, naphthalene ether type epoxy resin, phenol aralkyl type epoxy resin, anthracene type epoxy resin, trifunctional phenol type epoxy resin, tetrafunctional phenol type epoxy resin, triglycidyl isocyanurate, and so on. Hydroglyceride-type epoxy resins, alicyclic epoxy resins, dicyclopentadiene phenolic varnish-type epoxy resins, biphenyl phenolic varnish-type epoxy resins, phenol aralkyl phenolic varnish-type epoxy resins, naphthol aralkyl phenolic varnish-type epoxy resins, aralkyl phenolic varnish-type epoxy resins, naphthol aralkyl type epoxy resins, dicyclopentadiene type epoxy resins, polyol type epoxy resins, phosphorus-containing epoxy resins, glycidylamine, compounds obtained by epoxidation of the double bonds of butadiene, etc., compounds obtained by the reaction of hydroxyl-containing organosilicon resins with epichlorohydrin, and their halides. These epoxy resins can be used alone or in appropriate mixtures of two or more.

[0365] As epoxy resins, commercially available products can be used, such as epoxy resins shown in formula (34) (NC-3000FH (trade name) manufactured by Nippon Kayaku Co., Ltd., where n5 is approximately 4 in formula (34)); and naphthalene-type epoxy resins shown in formula (35) (HP-4710 (trade name) manufactured by DIC Co., Ltd.).

[0366]

[0367] These epoxy resins can be used alone or in appropriate combinations of two or more.

[0368] In the resin composition, the content of epoxy resin is 0.01 to 40 parts by weight relative to 100 parts by weight of the solid resin component in the resin composition.

[0369] <Other Compounds>

[0370] Other compounds include vinyl ethers such as ethyl vinyl ether, propyl vinyl ether, hydroxyethyl vinyl ether, and ethylene glycol divinyl ether; styrene compounds such as styrene, methylstyrene, ethylstyrene, and divinylbenzene; and triallyl isocyanurate, trimethylallyl isocyanurate, and diallyl nadicimide. These compounds can be used alone or in appropriate combinations of two or more.

[0371] In the resin composition, the content of other compounds is 0.01 to 40 parts by mass relative to 100 parts by mass of the resin solids in the resin composition.

[0372] [Organic solvents]

[0373] The resin composition of this embodiment may contain an organic solvent as needed. Using an organic solvent allows for adjustment of the viscosity during the preparation of the resin composition. There are no particular limitations on the type of organic solvent, as long as it can dissolve some or all of the resin in the resin composition. Examples of organic solvents include halogenated solvents such as dichloromethane, chloroform, dichloroethane, and chlorobenzene; aprotic polar solvents such as dimethylformamide, dimethylacetamide, dimethyl sulfoxide, tetrahydrofuran, dioxane, and acetonitrile; ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclopentanone, and cyclohexanone; cellosol solvents such as 2-ethoxyethanol and propylene glycol monomethyl ether; aliphatic alcohol solvents such as methanol, ethanol, propanol, isopropanol, and butanol; phenol solvents containing aromatic groups such as phenol and cresol; ester solvents such as ethyl lactate, methyl acetate, ethyl acetate, butyl acetate, isoamyl acetate, methyl methoxypropionate, methyl hydroxyisobutyrate, γ-butyrolactone, and propylene glycol monomethyl ether acetate; and aromatic hydrocarbon solvents such as toluene and xylene.

[0374] From the viewpoint that these also exhibit superior solubility for bismaleimide compound (A) and photocuring initiator (B), compounds (C) and (D) mixed as needed, and other resins and compounds, aprotic polar solvents, ketone solvents, cellosol solvents and ester solvents are preferred, and from the viewpoint that they exhibit superior solubility, aprotic polar solvents, ketone solvents and ester solvents are more preferred.

[0375] Dimethylacetamide is preferred as an aprotic polar solvent. Methyl ethyl ketone is preferred as a ketone solvent. Propylene glycol monomethyl ether is preferred as a cellosol solvent. Butyl acetate, γ-butyrolactone, and propylene glycol monomethyl ether acetate are preferred as ester solvents.

[0376] These organic solvents can be used alone or in appropriate combinations of two or more.

[0377] [Other ingredients]

[0378] In the resin composition of this embodiment, various polymeric compounds such as thermosetting resins, thermoplastic resins and their oligomers, and elastomers not mentioned above may be used in combination without impairing the characteristics of this embodiment; flame-retardant compounds not mentioned above; additives, etc. These are not particularly limited as long as they are commonly used substances. For example, flame-retardant compounds may include nitrogen-containing compounds such as melamine and benzoguanamine; compounds containing oxazine rings; phosphorus-based compounds such as phosphate esters, aromatic condensed phosphate esters, and halogenated condensed phosphate esters. Additives may include ultraviolet absorbers, antioxidants, fluorescent whitening agents, photosensitizers, dyes, pigments, thickeners, lubricants, defoamers, surface conditioners, brighteners, polymerization inhibitors, and thermosetting accelerators. These components may be used individually or in appropriate combinations of two or more.

[0379] In a resin composition, the content of other components is usually 0.1 to 10 parts by mass relative to 100 parts by mass of the resin solids in the resin composition.

[0380] [Method for manufacturing resin composition and varnish]

[0381] The resin composition of this embodiment can be prepared by appropriately mixing a bismaleimide compound (A), a photocuring initiator (B), a desired compound (C), a maleimide compound (D), other maleimide compounds, fillers, other resins, other compounds, and additives. Regarding the method of manufacturing the resin composition, for example, a method in which the aforementioned components are sequentially mixed in a solvent and thoroughly stirred.

[0382] When manufacturing a resin composition, known treatments (stirring, mixing, and kneading, etc.) for uniformly dissolving or dispersing the components can be performed as needed. Specifically, by using a stirring tank equipped with a stirrer having appropriate stirring capacity, the dispersibility of components such as the bismaleimide compound (A) and the photocuring initiator (B) in the resin composition can be improved. Stirring, mixing, and kneading can be performed appropriately using known devices such as stirring apparatus for dispersion (e.g., ultrasonic homogenizer), mixing apparatus for mixing (e.g., three-roll mill, ball mill, bead mill, and sand mill), or rotary or self-rotating mixing apparatus. Furthermore, organic solvents can be used as needed when preparing the resin composition. The type of organic solvent is not particularly limited as long as it can dissolve the resin in the resin composition; specific examples are as described above.

[0383] The resin composition can be suitably used in the form of a varnish for making the resin sheet described in this embodiment later. The varnish can be obtained by known methods. For example, the varnish can be obtained by adding 10 to 900 parts by weight, preferably 30 to 500 parts by weight, of an organic solvent relative to 100 parts by weight of the components other than the organic solvent in the resin composition, and performing the aforementioned known treatment (stirring, mixing, and kneading, etc.). It should be noted that the organic solvent used to prepare the varnish is not particularly limited, and specific examples are as described above.

[0384] [use]

[0385] The resin composition of this embodiment can be suitably used to manufacture multilayer printed circuit boards, and is preferably used for applications requiring an insulating resin composition. It can be used, for example, in photosensitive films, photosensitive films with supports, prepregs, resin sheets, circuit boards (for laminate applications, multilayer printed circuit board applications, etc.), solder resists, underfill materials, chip bonding materials, semiconductor sealing materials, via-filling resins, and component-filling resins. Among these, the resin composition exhibits excellent photocurability and alkaline developability, therefore, it can be suitably used for insulating layers or solder resist applications in multilayer printed circuit boards.

[0386] [cured material]

[0387] A cured product is obtained by curing a resin composition. For example, a cured product can be obtained by melting or dissolving the resin composition in a solvent, pouring it into a mold, and then curing it under normal conditions using light. Regarding the wavelength range of the light, curing is preferably carried out in the range of 100–500 nm, where curing is highly efficient using photopolymerization initiators or the like.

[0388] [Resin Sheet]

[0389] The resin sheet of this embodiment is a resin sheet with a support, having a support and a resin layer disposed on one or both sides of the support, the resin layer containing the resin composition of this embodiment. The resin sheet can be manufactured by coating the resin composition onto the support and drying it. The resin layer in the resin sheet has excellent photocurability and alkali developability.

[0390] The support can be any known support, without particular limitation, but a resin film is preferred. Examples of resin films include polyimide films, polyamide films, polyester films, polyethylene terephthalate (PET) films, polybutylene terephthalate (PBT) films, polypropylene (PP) films, polyethylene (PE) films, polyethylene naphthalate films, polyvinyl alcohol films, and triacetyl acetate films. Among these, PET films are preferred.

[0391] To facilitate peeling from the resin layer, the resin film is preferably coated with a release agent on its surface. The thickness of the resin film is preferably in the range of 5 to 100 μm, more preferably in the range of 10 to 50 μm. When the thickness is less than 5 μm, the support tends to break easily during support peeling before alkaline development; when the thickness exceeds 100 μm, there is a tendency for reduced resolution during exposure from the support. In this specification, the thickness can be measured using, for example, a micrometer.

[0392] In addition, to reduce light scattering during exposure, the resin film is preferably highly transparent.

[0393] Furthermore, in the resin sheet, the resin layer can be protected with a protective film.

[0394] By protecting the resin layer with a protective film, it is possible to prevent the adhesion and / or scratching of dust and other contaminants to the surface of the resin layer. The protective film can be made of the same material as the resin film. The thickness of the protective film is preferably in the range of 1 to 50 μm, more preferably in the range of 5 to 40 μm. When the thickness is less than 1 μm, the processability of the protective film tends to decrease; when it exceeds 50 μm, its cost-effectiveness tends to deteriorate. It should be noted that, regarding the protective film, it is preferable that the adhesion strength between the resin layer and the protective film is less than the adhesion strength between the resin layer and the support.

[0395] Methods for manufacturing resin sheets include, for example, coating a resin composition onto a support such as a PET film, drying it to remove organic solvents, and thus manufacturing a resin sheet.

[0396] Regarding the coating method, it can be carried out using known methods such as roller coaters, comma coaters, gravure coaters, die coaters, bar coaters, lip coaters, doctor blade coaters, and extrusion coaters. Drying can be carried out, for example, by heating in a dryer at 60–200°C for 1–60 minutes.

[0397] From the viewpoint of further preventing the diffusion of organic solvents in subsequent processes, the amount of organic solvent remaining in the resin layer is preferably set to 5% by mass or less relative to the total mass of the resin layer. From the viewpoint of improving processability, the thickness of the resin layer is preferably set to 1 to 50 μm.

[0398] Resin sheets are preferably used in the manufacture of insulating layers for multilayer printed circuit boards.

[0399] Multilayer printed circuit boards

[0400] The multilayer printed circuit board of this embodiment has an insulating layer and a conductor layer formed on one or both sides of the insulating layer. The insulating layer contains the resin composition of this embodiment. The insulating layer can also be obtained, for example, by overlapping one or more resin sheets and curing them. The number of layers for the insulating layer and the conductor layer can be appropriately set according to the intended use. Furthermore, the order of the insulating layer and the conductor layer is not particularly limited. The conductor layer can be a metal foil used in various printed circuit board materials, such as copper and aluminum foil. Examples of copper foils include rolled copper foil and electrolytic copper foil. The thickness of the conductor layer is typically 1 to 100 μm. Specifically, it can be manufactured by the following method.

[0401] (Lamination process)

[0402] In the lamination process, a vacuum laminator is used to laminate the resin layer side of the resin sheet onto one or both sides of the circuit board. Examples of circuit boards include glass epoxy boards, metal substrates, ceramic substrates, silicon substrates, semiconductor sealing resin substrates, polyester substrates, polyimide substrates, BT resin substrates, and thermosetting polyphenylene ether substrates. It should be noted that a circuit board refers to a substrate on one or both sides of the substrate described above where a patterned conductor layer (circuit) is formed. Furthermore, in multilayer printed circuit boards (PCBs) formed by alternating layers of conductor and insulating layers, the outermost layer of the PCB with one or both sides having a patterned conductor layer (circuit) is also included within the category of circuit boards. It should be noted that the insulating layer laminated in a multilayer PCB can be an insulating layer obtained by overlapping and curing one or more resin sheets of this embodiment, or an insulating layer obtained by overlapping one or more resin sheets of this embodiment and a known resin sheet different from the resin sheet of this embodiment. It should be noted that the overlapping method of the resin sheet in this embodiment and a known resin sheet different from that in this embodiment is not particularly limited. Roughening treatment can be performed beforehand by pre-performing a blackening treatment and / or copper etching on the surface of the conductor layer. In the lamination process, if the resin sheet has a protective film, after the protective film is peeled off, the resin sheet and the circuit board are preheated as needed, and the resin layer of the resin sheet is pressed onto the circuit board while under pressure and heat. In this embodiment, a method of laminating the resin layer of the resin sheet onto the circuit board under reduced pressure using a vacuum lamination method is suitable.

[0403] Regarding the conditions for the lamination process, the preferred options are, for example, setting the pressing temperature (lamination temperature) to 50–140℃ and the pressing pressure to 1–15 kgf / cm². 2 The lamination time is set to 5–300 seconds, and lamination is performed under reduced air pressure of 20 mmHg or less. Furthermore, the lamination process can be intermittent or continuous using rollers. Vacuum lamination can be performed using commercially available vacuum laminators. Examples of commercially available vacuum laminators include, for instance, the two-stage lamination laminator manufactured by NIKKO MATERIALS.

[0404] (Exposure process)

[0405] In the exposure process, after a resin layer is deposited on the circuit board through a lamination process, a designated portion of the resin layer is irradiated with active energy rays, which serve as a light source, causing the irradiated portion of the resin layer to cure. The compound (C) mixed as needed does not interfere with the photocuring reaction during the exposure process.

[0406] Irradiation can be achieved through mask patterns or by direct irradiation. Examples of active energy rays include ultraviolet light, visible light, electron beams, and X-rays. The wavelengths of active energy rays are, for example, in the range of 200–600 nm. When using ultraviolet light, the irradiation dose is approximately 5–1000 mJ / cm². 2 Furthermore, when manufacturing printed circuit boards with high-density and high-precision wiring formation (patterning) using a step-projection lithography machine that performs projection exposure in a step-by-step repeating manner, active energy rays, such as those containing a wavelength of 365 nm (i-rays), are used as the active energy rays. When using active energy rays containing a wavelength of 365 nm (i-rays), the irradiation dose is approximately 5 to 10,000 mJ / cm². 2 .

[0407] Among the exposure methods using mask patterns, there are contact exposure methods where the mask pattern is tightly adhered to a multilayer printed circuit board; and non-contact exposure methods where the mask pattern is not tightly adhered but projected using lenses or mirrors. Either method can be used. Furthermore, if a support is present on the resin layer, exposure can be performed from the support or after the support has been peeled off.

[0408] (Alkali development process)

[0409] In the absence of a support on the resin layer, after the exposure process, the uncured portion (unexposed portion) can be removed directly by alkaline development, and then development can be performed to form the pattern of the insulating layer.

[0410] In addition, when a support is present on the resin layer, after the exposure process, the uncured portion (unexposed portion) can be removed by alkaline development after the support is removed, and then development can be performed to form a pattern of the insulating layer.

[0411] By including compound (C) in the unexposed resin layer containing the resin composition of this embodiment, excellent alkaline developability is achieved, enabling rapid removal of the unexposed resin composition. Therefore, printed circuit boards with high-precision patterns can be obtained.

[0412] In the case of alkaline development, there are no particular limitations on the developer as long as it selectively washes away the unexposed portions; alkaline developers such as tetramethylammonium hydroxide aqueous solution, sodium carbonate aqueous solution, potassium carbonate aqueous solution, sodium hydroxide aqueous solution, and potassium hydroxide aqueous solution can be used. In this embodiment, tetramethylammonium hydroxide aqueous solution is more preferred. These alkaline developers can be used alone or in appropriate combinations of two or more.

[0413] In addition, as an alkaline development method, known methods such as immersion, agitation, spraying, shaking immersion, brushing, and scraping can be used. These development methods can also be combined as needed during pattern formation. Furthermore, as a development method, high-pressure spraying is suitable for further improving resolution. The spray pressure when using a spraying method is preferably 0.02 to 0.5 MPa.

[0414] (Post-baking process)

[0415] In this embodiment, a post-baking process is performed after the alkaline development step to form an insulating layer (cured material). Examples of post-baking processes include ultraviolet irradiation using a high-pressure mercury lamp and heating using a cleanroom oven; combinations of these methods are also possible. When irradiating with ultraviolet light, the irradiation dose can be adjusted as needed, for example, from 0.05 to 10 J / cm². 2 Irradiation is performed at approximately the same level. Furthermore, heating conditions can be appropriately selected as needed, preferably within the range of 150–220°C for 20–180 minutes, and more preferably within the range of 160–200°C for 30–150 minutes.

[0416] (Conductor layer formation process)

[0417] After the insulating layer (cured material) is formed, a conductor layer is formed on the surface of the insulating layer by dry plating.

[0418] It should be noted that, when forming the conductor layer, the surface of the insulating layer can be modified before dry plating. Known methods such as plasma etching, reverse sputtering, and corona treatment can be used for surface modification.

[0419] As a dry plating process, known methods such as vapor deposition, sputtering, and ion plating can be used. Regarding vapor deposition (vacuum vapor deposition), a metal film can be formed on an insulating layer by, for example, placing a multilayer printed circuit board in a vacuum container and heating and evaporating the metal. Regarding sputtering, a metal film can also be formed on an insulating layer by, for example, placing a multilayer printed circuit board in a vacuum container, introducing an inert gas such as argon, and applying a DC voltage, causing the ionized inert gas to bombard a target metal, and using the ejected metal to form a metal film on the insulating layer.

[0420] Next, a conductor layer is formed by chemical plating, electroplating, or other methods. Subsequent patterning methods can include subtractive or semi-additive processes.

[0421] [Semiconductor Devices]

[0422] The semiconductor device of this embodiment comprises the resin composition of this embodiment. Specifically, it can be manufactured by the following method. The semiconductor device can be manufactured by mounting a semiconductor chip on a conductive portion of a multilayer printed circuit board. Here, a conductive portion refers to a portion of the multilayer printed circuit board that transmits electrical signals; its location can be on the surface or in a filled portion. Furthermore, the semiconductor chip is not particularly limited as long as it is a circuit element made of semiconductor material.

[0423] There are no particular limitations on the mounting methods for semiconductor chips during the manufacture of semiconductor devices, as long as the semiconductor chip functions effectively. Specifically, examples include wire bonding mounting methods, flip chip mounting methods, bump-free uplift (BBUL) mounting methods, anisotropic conductive film (ACF) mounting methods, and non-conductive film (NCF) mounting methods.

[0424] Alternatively, semiconductor devices can also be manufactured by forming an insulating layer containing a resin composition on a semiconductor chip or on a substrate on which the semiconductor chip is mounted. The substrate on which the semiconductor chip is mounted can be in the shape of a wafer or a panel. It can be manufactured using the same method as the aforementioned multilayer printed circuit board after its formation.

[0425] Example

[0426] Hereinafter, this embodiment will be described in more detail using examples and comparative examples. This embodiment is not limited in any way by the examples described below.

[0427] [Synthesis Example 1] Synthesis of photocuring initiator (B1)

[0428] As a photocuring initiator (B1), a photocuring initiator (B1A) of formula (14) was synthesized according to the method described in Japanese Patent Application Publication No. 2014-500852, paragraph

[0344] . 1 H-NMR analysis confirmed that it is the photocuring initiator (B1A) shown in formula (14).

[0429] The following shows the photocuring initiator (B1A) shown in formula (14). 1 The assignment of H-NMR. Additionally, 1 The H-NMR spectrum is shown in Figure 1 .

[0430] 1H-NMR (500MHz, CDCl3) δ (ppm): 9.54 (d, 1H), 8.72 (d, 1H), 8.36 (s, 1H), 8.2 9(s, 1H), 7.79-7.77(m, 2H), 7.61-7.56(m, 3H), 7.25(d, 2H), 7.07(d, 1H), 7.00(s, 2H), 5.36(m, 1H), 4.80(m, 2H), 4.38(m, 2H), 2.43(s, 3H), 2.32(m, 1H), 2.19(s, 6H), 2.07(s, 3H), 1.38-1.22(m, 8H), 0.92(t, 3H), 0.84(t, 3H)

[0431] [Synthesis Example 2] Synthesis of Photocuring Initiator (B2)

[0432] As the photocuring initiator (B1), the photocuring initiator (B2A) shown in formula (15) was synthesized according to the method described in Japanese Patent Application Publication No. 2016-531926, paragraph

[0357] . 1 H-NMR analysis confirmed that it is the photocuring initiator (B2A) shown in formula (15).

[0433] The following shows the photocuring initiator (B2A) shown in formula (15). 1 The assignment of H-NMR. Additionally, 1 The H-NMR spectrum is shown in Figure 2 .

[0434] 1 H-NMR (500MHz, CDCl3) δ (ppm): 8.03 (m, 2H), 7.81-7.77 (m, 3H), 7.68 (d, 1H), 7.59-7.54 (m, 4H ), 7.45(m, 2H), 7.38(m, 1H), 2.88(m, 2H), 2.26(s, 3H), 1.69(m, 1H), 1.49(m, 2H), 1.00(s, 6H)

[0435] [Synthetic Example 3] Synthesis of maleimide compound (TMDM)

[0436] The compound (TMDM) shown in formula (24) was synthesized as follows.

[0437] Synthesis of Amide Acid Compounds (hereinafter referred to as MA-TMDA)

[0438] First, the MA-TMDA shown in formula (36) is synthesized using the following method.

[0439]

[0440] Add 5.2 g (53 mmol) of maleic anhydride, 20 mL of N-methylpyrrolidone (NMP), and 20 mL of toluene to a 100 mL four-necked flask equipped with an argon inlet, a Dean-Stark apparatus, a serpentine condenser, and a thermometer. Stir at room temperature (25 °C) under an argon gas flow until the maleic anhydride is completely dissolved. Add 5.0 g (19 mmol) of TMDA (a mixture of 5-amino-1,3,3-trimethyl-1-(4-aminophenyl)-indane and 6-amino-1,3,3-trimethyl-1-(4-aminophenyl)-indane, manufactured by Junra Pharmaceutical Co., Ltd. of Japan) and 10 mL of NMP to the solution. Stir at room temperature (25 °C) for 17 hours.

[0441] A portion of the reaction solution was removed, and water and ethyl acetate were added, followed by shaking. The organic layer was then removed and dried over magnesium sulfate. The supernatant was distilled off at 40°C to obtain a yellow oil. 1 H-NMR measurements confirmed that it was MA-TMDA as shown in formula (36).

[0442] The following shows the MA-TMDA represented by equation (36). 1 The assignment of H-NMR. Additionally, 1 The H-NMR spectrum is shown in Figure 3 .

[0443] 1 H-NMR (300MHz, DMSO-d6) δ (ppm): 10.40 (m, 2H, -COOH), 7.30 (m, 7H, ArH), 6.33 (m, 4H ,=CH-), 2.11(m, 2H, -CH2-), 1.48(d, 3H, -CH3), 1.21(d, 3H, -CH3), 0.92(d, 3H, -CH3)

[0444] [Synthesis of TMDM]

[0445] 0.67 g (3.5 mmol) of p-toluenesulfonic acid monohydrate was added to the aforementioned reaction solution, and the mixture was heated under reflux at 127 °C for 2.5 hours. After cooling to room temperature (25 °C), the cooled reaction solution was added, while stirring, to a mixture of 50 mL of saturated sodium bicarbonate aqueous solution and 100 mL of ethyl acetate. Then, 100 mL of water and 100 mL of ethyl acetate were added and stirred, and the mixture was allowed to stand for 5 minutes. The mixture was then separated, and the aqueous layer was extracted three times with 50 mL of ethyl acetate. The organic layers were combined, washed once with 100 mL of water, once with 10 mL of saturated brine, and twice with 5 mL of saturated brine. After drying with magnesium sulfate and filtering the solid components, the solid was distilled off at 40 °C to obtain a yellow solid.

[0446] The obtained yellow solid was dissolved in 6.5 mL of acetone, and the acetone solution was added to 300 mL of water. The precipitated solid was collected by filtration, washed with a small amount of isopropanol (IPA), and dried under reduced pressure at 50 °C for 20 hours to obtain 5.71 parts by mass of the yellow solid. 1 H-NMR analysis confirmed that it was the maleimide compound (TMDM) shown in formula (24).

[0447] TMDM 1 The H-NMR attribution is shown below. Additionally, 1 H-NMR diagram is shown in Figure 4 .

[0448] 1 H-NMR (300MHz, DMSO-d6) δ (ppm): 7.19 (m, 11H, ArH, -CH=CH-), 2.42 (m, 2H, -CH2-), 1.66 (d, 3H, -CH3), 1.32 (d, 3H, -CH3), 1.00 (d, 3H, -CH3)

[0449] [Synthetic Example 4] Synthesis of the compound shown in formula (20)

[0450] The compound (C1) shown in formula (20) is synthesized as follows.

[0451] Add 12.52 g (50 mmol) of bis(trimethylolpropane) (manufactured by Tokyo Chemical Industry Co., Ltd.), 41.62 g (210 mmol) of cis,cis-cyclohexane-1,2,4-tricarboxylic acid-1,2-anhydride (manufactured by Mitsubishi Gas Chemical Co., Ltd., H-TMAn-S (trade name)), 6.10 g (50 mmol) of 4-dimethylaminopyridine, 22.26 g of triethylamine and 150 g of dichloromethane to a 200 mL flask, and stir at room temperature (25 °C) for 9 hours.

[0452] 200 mL of 10% hydrochloric acid and 200 mL of methyl ethyl ketone were added to the reaction solution, which was then transferred to a separatory funnel. The solution was washed twice with 100 mL of 10% hydrochloric acid and twice with 150 mL of saturated saline solution. The solution was dried over magnesium sulfate, and the solvent was removed by distillation. The solution was then dried under vacuum at 120 °C to obtain 44.00 g of a white solid. The obtained white solid was subjected to… 1 H-NMR determination confirmed that it was the compound (C1) shown in formula (20).

[0453] The following shows the compound (C1) 1 The assignment of H-NMR. Additionally, 1 The H-NMR spectrum is shown in Figure 5 .

[0454] 1 H-NMR (500MHz, DMSO-d6) δ (ppm): 12.25 (s, 8H, -COOH), 3.85 (s, 8H), 3.20 (s, 4H), 3.08 (s, 4H), 2.58 (m, 4H), 2.26 (t, 4H), 2.09 (m, 8H), 1.74 (m, 8H), 1.60 (m, 4H), 1.33 (m, 4H), 1.15 (m, 4H), 0.78 (t, 6H)

[0455] In addition, for the aforementioned reaction solution, the content and mass-average molecular weight of the compound (C1) contained in the reaction solution were determined by the following method.

[0456] Add 50 mg of reaction solution to 4500 mg of THF (tetrahydrofuran) to prepare the sample solution, and perform GPC analysis on this solution under the following conditions. Calculate the peak area based on the obtained elution curve, and determine the GPC area percentage (content) of each component in the reaction solution. It should be noted that the peak area is calculated from the area between the elution curve and the baseline; for incompletely separated peaks, vertical segmentation is used for calculation. Additionally, the mass-average molecular weight is determined using polystyrene as a standard.

[0457] (Measurement conditions)

[0458] Measuring instrument: Prominence (trade name) manufactured by Shimadzu Corporation.

[0459] Pillars: KF-801 (trade name), KF-802 (trade name), KF-803 (trade name), and KF-804 (trade name) manufactured by Showa Denko Corporation.

[0460] Flow rate: 1 mL / min

[0461] Column temperature: 40℃

[0462] Detector: RI (Refractive Index) detector

[0463] Regarding the GPC determination results, the reaction solution contained 88% of the compound (C1). Additionally, the mass-average molecular weight was 1500.

[0464] [Evaluation of raw materials]

[0465] [Transmittance and Absorbance]

[0466] As the bismaleimide compound (A), a chloroform solution containing MIZ-001 (trade name, mass-average molecular weight (Mw): 3000) manufactured by Nippon Kayaku Co., Ltd. was prepared, and the transmittance at a wavelength of 365 nm was measured using a UV-vis measuring device (Hitachi High Technology Co., Ltd. Hitachi Spectrophotometer U-4100 (trade name)).

[0467] Similarly, as maleimide compound (D), the transmittance at a wavelength of 365 nm was measured for the compound (TMDM) shown in formula (24) and the compound (BCPH01 (trade name)) shown in formula (25) obtained in Synthesis Example 3.

[0468] As the photocuring initiator (B), the photocuring initiator (B1A) obtained in Synthesis Example 1 was used to prepare a chloroform solution containing 0.01% by mass of the photocuring initiator (B1A), and the absorbance at a wavelength of 365 nm was measured using a UV-vis measuring device (U-4100 (trade name)).

[0469] Similarly, the absorbance at a wavelength of 365 nm was measured using the photocuring initiator (B2A) obtained in Synthesis Example 2, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (Omnirad 819, a registered trademark manufactured by IGM Resins BV), 1-[4-(phenylthio)]-1,2-octanedione 2-(O-benzoyl oxime) (Irgacure OXE01, a registered trademark manufactured by BASF JAPAN), and 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3-yl]-acetyl ketone 1-(O-acetyl oxime) (Irgacure OXE02, a registered trademark manufactured by BASF JAPAN).

[0470] As compound (C), using compound (C1) obtained in Synthesis Example 4, an N-methylpyrrolidone solution containing 1% by mass of compound (C1) was prepared, and the transmittance at a wavelength of 365 nm was measured using a UV-vis measuring device (Hitachi High Technology Co., Ltd. Hitachi Spectrophotometer U-4100).

[0471] Similarly, as compound (C), cis,cis-1,2,4-cyclohexanetricarboxylic acid-1,2-anhydride (H-TMAn-S (trade name) manufactured by Mitsubishi Gas Chemical Co., Ltd.) was used to determine the transmittance at a wavelength of 365 nm.

[0472] The results are shown in Table 1.

[0473] [Table 1]

[0474]

[0475] [Example 1]

[0476] (Preparation of resin compositions and resin sheets)

[0477] 60 parts by mass of MIZ-001 (trade name, mass-average molecular weight (Mw): 3000) manufactured by Nippon Kayaku Co., Ltd. as bismaleimide compound (A), 5 parts by mass of compound (B1A) as photocuring initiator (B), 5.25 parts by mass of compound (C) as compound (C) represented by formula (20), and 1.08 parts by mass of cis,cis-cyclohexane-1,2,4-tricarboxylic acid-1,2-anhydride (H-TMAn-S (trade name) manufactured by Mitsubishi Gas Chemical Co., Ltd.) as compound (C). 25 parts by mass of compound (BCPH01, trade name) of formula (25) as maleimide compound (D), 15 parts by mass of compound (TMDM) of formula (24) as maleimide compound (D), and 3 parts by mass of N-phenyl-3-aminopropyltrimethoxysilane (Tokyo Chemical Industry Co., Ltd.) were mixed, and 213.3 parts by mass of methyl ethyl ketone (MEK) were added. The mixture was heated on a heating plate at 90°C to obtain a varnish (resin composition). The varnish was dropped onto a 25 μm thick PET film (UNIPEEL TR1-25, trade name) of UNITIKA Co., Ltd., and a coating was formed by spin coating (500 rpm for 10 seconds, then 1000 rpm for 30 seconds). The resulting coating was dried at 90°C for 5 minutes to obtain a resin sheet with a resin layer thickness of 5 μm supported by a PET film.

[0478] (Evaluation of the creation of layered bodies)

[0479] The obtained resin sheet was placed on the oxide film side of a silicon wafer (Advantech, 625 μm thick, with 1 μm oxide film) with the resin surface facing it. A vacuum laminator (NIKKO MATERIALS) was used to evacuate the wafer for 30 seconds (below 5.0 hPa). Then, a pressure of 10 kgf / cm² was applied. 2 The material is laminated at 100°C for 30 seconds. Then, it is laminated under a pressure of 7 kgf / cm². 2 The silicon wafer, resin layer and support are laminated at 100°C for 60 seconds to obtain an evaluation laminate.

[0480] [Example 2]

[0481] 60 parts by weight of MIZ-001 (trade name, mass-average molecular weight (Mw): 3000) manufactured by Nippon Kayaku Co., Ltd. as bismaleimide compound (A), 4.25 parts by weight of compound (B1A) as photocuring initiator (B), 5.25 parts by weight of compound (C) as compound (C) represented by formula (20), and 1 part by weight of cis,cis-cyclohexane-1,2,4-tricarboxylic acid-1,2-anhydride (H-TMAn-S (trade name) manufactured by Mitsubishi Gas Chemical Co., Ltd.) as compound (C). 0.08 parts by weight, 25 parts by weight of compound (BCPH01 (trade name) manufactured by Gunei Chemical Industry Co., Ltd.) as maleimide compound (D) of formula (25), 15 parts by weight of compound (TMDM) as maleimide compound (D) of formula (24), and 3 parts by weight of N-phenyl-3-aminopropyltrimethoxysilane (manufactured by Tokyo Chemical Industry Co., Ltd.) were mixed, and 210.9 parts by weight of methyl ethyl ketone were added. The mixture was heated on a heating plate heated to 90°C to obtain a varnish (resin composition).

[0482] Using the obtained varnish, resin sheets and evaluation laminates were obtained using the same method as in Example 1.

[0483] [Example 3]

[0484] 60 parts by weight of MIZ-001 (trade name, mass-average molecular weight (Mw): 3000) manufactured by Nippon Kayaku Co., Ltd. as bismaleimide compound (A), 4 parts by weight of compound (B1A) as photocuring initiator (B), 5.25 parts by weight of compound (C) as compound (C) represented by formula (20), and 1.0 parts by weight of cis,cis-cyclohexane-1,2,4-tricarboxylic acid-1,2-anhydride (H-TMAn-S (trade name) manufactured by Mitsubishi Gas Chemical Co., Ltd.) as compound (C). 8 parts by mass, 25 parts by mass of compound (BCPH01 (trade name) manufactured by Gunei Chemical Industry Co., Ltd.) as maleimide compound (D) as formula (25), 15 parts by mass of compound (TMDM) as maleimide compound (D) as formula (24), and 3 parts by mass of N-phenyl-3-aminopropyltrimethoxysilane (manufactured by Tokyo Chemical Industry Co., Ltd.) were mixed, and 210.5 parts by mass of methyl ethyl ketone were added. The mixture was heated on a heating plate heated to 90°C to obtain a varnish (resin composition).

[0485] Using the obtained varnish, resin sheets and evaluation laminates were obtained using the same method as in Example 1.

[0486] [Example 4]

[0487] 60 parts by weight of MIZ-001 (trade name, mass-average molecular weight (Mw): 3000) manufactured by Nippon Kayaku Co., Ltd. as bismaleimide compound (A), 2 parts by weight of compound (B1A) as photocuring initiator (B), 5.25 parts by weight of compound (C) as compound (C) represented by formula (20), and 1.0 parts by weight of cis,cis-cyclohexane-1,2,4-tricarboxylic acid-1,2-anhydride (H-TMAn-S (trade name) manufactured by Mitsubishi Gas Chemical Co., Ltd.) as compound (C). 8 parts by mass, 25 parts by mass of compound (BCPH01 (trade name) manufactured by Gunei Chemical Industry Co., Ltd.) as maleimide compound (D) as formula (25), 15 parts by mass of compound (TMDM) as maleimide compound (D) as formula (24), and 3 parts by mass of N-phenyl-3-aminopropyltrimethoxysilane (manufactured by Tokyo Chemical Industry Co., Ltd.) were mixed, and 206.8 parts by mass of methyl ethyl ketone were added. The mixture was heated on a heating plate heated to 90°C to obtain a varnish (resin composition).

[0488] Using the obtained varnish, resin sheets and evaluation laminates were obtained using the same method as in Example 1.

[0489] [Example 5]

[0490] 60 parts by weight of MIZ-001 (trade name, mass-average molecular weight (Mw): 3000) manufactured by Nippon Kayaku Co., Ltd. as bismaleimide compound (A), 1 part by weight of compound (B1A) as photocuring initiator (B), 5.25 parts by weight of compound (C) as compound (C) represented by formula (20), and 1.0 part by weight of cis,cis-cyclohexane-1,2,4-tricarboxylic acid-1,2-anhydride (H-TMAn-S (trade name) manufactured by Mitsubishi Gas Chemical Co., Ltd.) as compound (C). 8 parts by mass, 25 parts by mass of compound (BCPH01 (trade name) manufactured by Gunei Chemical Industry Co., Ltd.) as maleimide compound (D) as formula (25), 15 parts by mass of compound (TMDM) as maleimide compound (D) as formula (24), and 3 parts by mass of N-phenyl-3-aminopropyltrimethoxysilane (manufactured by Tokyo Chemical Industry Co., Ltd.) were mixed, and 204.9 parts by mass of methyl ethyl ketone were added. The mixture was heated on a heating plate heated to 90°C to obtain a varnish (resin composition).

[0491] Using the obtained varnish, resin sheets and evaluation laminates were obtained using the same method as in Example 1.

[0492] [Example 6]

[0493] The following compounds were prepared: 60 parts by weight of MIZ-001 (trade name, mass-average molecular weight (Mw): 3000) manufactured by Nippon Kayaku Co., Ltd. as bismaleimide compound (A); 4.25 parts by weight of compound (B1A) as photocuring initiator (B); 5.25 parts by weight of compound (C) represented by formula (20); 1.08 parts by weight of cis,cis-cyclohexane-1,2,4-tricarboxylic acid-1,2-anhydride (H-TMAn-S (trade name) manufactured by Mitsubishi Gas Chemical Co., Ltd.) as compound (C); 25 parts by weight of compound (D) represented by formula (25) (BCPH01 (trade name) manufactured by Gunei Chemical Industry Co., Ltd.) as maleimide compound (D); 15 parts by weight of compound (D) represented by formula (24) (TMDM); and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (IGM) as photocuring initiator. 0.75 parts by weight of Omnirad 819 (trade name) manufactured by Resins BV and 3 parts by weight of N-phenyl-3-aminopropyltrimethoxysilane (manufactured by Tokyo Chemical Industry Co., Ltd.) were mixed, and 213.3 parts by weight of methyl ethyl ketone were added. The mixture was heated on a heating plate at 90°C to obtain a varnish (resin composition).

[0494] Using the obtained varnish, resin sheets and evaluation laminates were obtained using the same method as in Example 1.

[0495] [Example 7]

[0496] 60 parts by weight of MIZ-001 (trade name, mass-average molecular weight (Mw): 3000) manufactured by Nippon Kayaku Co., Ltd. as bismaleimide compound (A), 4 parts by weight of compound (B2A) as photocuring initiator (B), 5.25 parts by weight of compound (C) as compound (C) represented by formula (20), and 1.0 parts by weight of cis,cis-cyclohexane-1,2,4-tricarboxylic acid-1,2-anhydride (H-TMAn-S (trade name) manufactured by Mitsubishi Gas Chemical Co., Ltd.) as compound (C). 8 parts by mass, 25 parts by mass of compound (BCPH01 (trade name) manufactured by Gunei Chemical Industry Co., Ltd.) as maleimide compound (D) as formula (25), 15 parts by mass of compound (TMDM) as maleimide compound (D) as formula (24), and 3 parts by mass of N-phenyl-3-aminopropyltrimethoxysilane (manufactured by Tokyo Chemical Industry Co., Ltd.) were mixed, and 210.5 parts by mass of methyl ethyl ketone were added. The mixture was heated on a heating plate heated to 90°C to obtain a varnish (resin composition).

[0497] Using the obtained varnish, resin sheets and evaluation laminates were obtained using the same method as in Example 1.

[0498] [Example 8]

[0499] 60 parts by weight of MIZ-001 (trade name, mass-average molecular weight (Mw): 3000) manufactured by Nippon Kayaku Co., Ltd. as bismaleimide compound (A), 2.5 parts by weight of compound (B2A) as photocuring initiator (B), 5.25 parts by weight of compound (C) as compound (C) represented by formula (20), and 1 part by weight of cis,cis-cyclohexane-1,2,4-tricarboxylic acid-1,2-anhydride (H-TMAn-S (trade name) manufactured by Mitsubishi Gas Chemical Co., Ltd.) as compound (C). 0.8 parts by weight, 25 parts by weight of compound (BCPH01 (trade name) manufactured by Gunei Chemical Industry Co., Ltd.) as maleimide compound (D) of formula (25), 15 parts by weight of compound (TMDM) as maleimide compound (D) of formula (24), and 3 parts by weight of N-phenyl-3-aminopropyltrimethoxysilane (manufactured by Tokyo Chemical Industry Co., Ltd.) were mixed, and 207.7 parts by weight of methyl ethyl ketone were added. The mixture was heated on a heating plate heated to 90°C to obtain a varnish (resin composition).

[0500] Using the obtained varnish, resin sheets and evaluation laminates were obtained using the same method as in Example 1.

[0501] [Example 9]

[0502] 60 parts by weight of MIZ-001 (trade name, mass-average molecular weight (Mw): 3000) manufactured by Nippon Kayaku Co., Ltd. as bismaleimide compound (A), 2 parts by weight of compound (B2A) as photocuring initiator (B), 5.25 parts by weight of compound (C) as compound (C) represented by formula (20), and 1.0 parts by weight of cis,cis-cyclohexane-1,2,4-tricarboxylic acid-1,2-anhydride (H-TMAn-S (trade name) manufactured by Mitsubishi Gas Chemical Co., Ltd.) as compound (C). 8 parts by mass, 25 parts by mass of compound (BCPH01 (trade name) manufactured by Gunei Chemical Industry Co., Ltd.) as maleimide compound (D) as formula (25), 15 parts by mass of compound (TMDM) as maleimide compound (D) as formula (24), and 3 parts by mass of N-phenyl-3-aminopropyltrimethoxysilane (manufactured by Tokyo Chemical Industry Co., Ltd.) were mixed, and 206.8 parts by mass of methyl ethyl ketone were added. The mixture was heated on a heating plate heated to 90°C to obtain a varnish (resin composition).

[0503] Using the obtained varnish, resin sheets and evaluation laminates were obtained using the same method as in Example 1.

[0504] [Example 10]

[0505] 60 parts by weight of MIZ-001 (trade name, mass-average molecular weight (Mw): 3000) manufactured by Nippon Kayaku Co., Ltd. as bismaleimide compound (A), 1 part by weight of compound (B2A) as photocuring initiator (B), 5.25 parts by weight of compound (C) as compound (C) represented by formula (20), and 1.0 part by weight of cis,cis-cyclohexane-1,2,4-tricarboxylic acid-1,2-anhydride (H-TMAn-S (trade name) manufactured by Mitsubishi Gas Chemical Co., Ltd.) as compound (C). 8 parts by mass, 25 parts by mass of compound (BCPH01 (trade name) manufactured by Gunei Chemical Industry Co., Ltd.) as maleimide compound (D) as formula (25), 15 parts by mass of compound (TMDM) as maleimide compound (D) as formula (24), and 3 parts by mass of N-phenyl-3-aminopropyltrimethoxysilane (manufactured by Tokyo Chemical Industry Co., Ltd.) were mixed, and 204.9 parts by mass of methyl ethyl ketone were added. The mixture was heated on a heating plate heated to 90°C to obtain a varnish (resin composition).

[0506] Using the obtained varnish, resin sheets and evaluation laminates were obtained using the same method as in Example 1.

[0507] [Example 11]

[0508] 60 parts by mass of MIZ-001 (trade name, mass-average molecular weight (Mw): 3000) manufactured by Nippon Kayaku Co., Ltd. as bismaleimide compound (A), 10 parts by mass of compound (B1A) as photocuring initiator (B), 5.25 parts by mass of compound (C1) as compound (C) represented by formula (20), 1.08 parts by mass of cis,cis-cyclohexane-1,2,4-tricarboxylic acid-1,2-anhydride (H-TMAn-S (trade name) manufactured by Mitsubishi Gas Chemical Co., Ltd.) as compound (C), 40 parts by mass of compound (D) represented by formula (25) (BCPH01 (trade name) manufactured by Gunei Chemical Industry Co., Ltd.), and 3 parts by mass of N-phenyl-3-aminopropyltrimethoxysilane (manufactured by Tokyo Kasei Co., Ltd.) were mixed, and 214.4 parts by mass of methyl ethyl ketone were added. The mixture was heated on a heating plate heated to 90°C to obtain a varnish (resin composition).

[0509] Using the obtained varnish, resin sheets and evaluation laminates were obtained using the same method as in Example 1.

[0510] [Example 12]

[0511] The following compounds were prepared: 60 parts by weight of MIZ-001 (trade name, mass-average molecular weight (Mw): 3000) manufactured by Nippon Kayaku Co., Ltd. as bismaleimide compound (A); 8.5 parts by weight of compound (B1A) as photocuring initiator (B); 5.25 parts by weight of compound (C) represented by formula (20); 1.08 parts by weight of cis,cis-cyclohexane-1,2,4-tricarboxylic acid-1,2-anhydride (H-TMAn-S (trade name) manufactured by Mitsubishi Gas Chemical Co., Ltd.) as compound (C); 40 parts by weight of compound (D) represented by formula (25) (BCPH01 (trade name) manufactured by Gunei Chemical Industry Co., Ltd.) as maleimide compound (D); and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (IGM Resins) as photocuring initiator. 1.5 parts by weight of Omnirad 819 (trade name) manufactured by BV and 3 parts by weight of N-phenyl-3-aminopropyltrimethoxysilane (manufactured by Tokyo Chemical Industry Co., Ltd.) were mixed, and 214.4 parts by weight of methyl ethyl ketone were added. The mixture was heated on a heating plate at 90°C to obtain a varnish (resin composition).

[0512] Using the obtained varnish, resin sheets and evaluation laminates were obtained using the same method as in Example 1.

[0513] [Example 13]

[0514] The following compounds were prepared: 60 parts by weight of MIZ-001 (trade name, mass-average molecular weight (Mw): 3000) manufactured by Nippon Kayaku Co., Ltd. as bismaleimide compound (A); 7.5 parts by weight of compound (B1A) as photocuring initiator (B); 5.25 parts by weight of compound (C) represented by formula (20); 1.08 parts by weight of cis,cis-cyclohexane-1,2,4-tricarboxylic acid-1,2-anhydride (H-TMAn-S (trade name) manufactured by Mitsubishi Gas Chemical Co., Ltd.) as compound (C); 40 parts by weight of compound (D) represented by formula (25) (BCPH01 (trade name) manufactured by Gunei Chemical Industry Co., Ltd.) as maleimide compound (D); and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (IGM Resins) as photocuring initiator. 2.5 parts by weight of Omnirad (registered trademark) 819 (trade name) manufactured by BV and 3 parts by weight of N-phenyl-3-aminopropyltrimethoxysilane (manufactured by Tokyo Chemical Industry Co., Ltd.) were mixed, and 214.4 parts by weight of methyl ethyl ketone were added. The mixture was heated on a heating plate heated to 90°C to obtain a varnish (resin composition).

[0515] Using the obtained varnish, resin sheets and evaluation laminates were obtained using the same method as in Example 1.

[0516] [Example 14]

[0517] The following compounds were prepared: 60 parts by weight of MIZ-001 (trade name, mass-average molecular weight (Mw): 3000) manufactured by Nippon Kayaku Co., Ltd. as bismaleimide compound (A); 5 parts by weight of compound (B1A) as photocuring initiator (B); 5.25 parts by weight of compound (C1) as compound (C) represented by formula (20); 1.08 parts by weight of cis,cis-cyclohexane-1,2,4-tricarboxylic acid-1,2-anhydride (H-TMAn-S (trade name) manufactured by Mitsubishi Gas Chemical Co., Ltd.) as compound (C); 40 parts by weight of compound (D) represented by formula (25) (BCPH01 (trade name) manufactured by Gunei Chemical Industry Co., Ltd.) as maleimide compound (D); and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (IGM Resins) as photocuring initiator. Five parts by weight of Omnirad 819 (trade name) manufactured by BV and three parts by weight of N-phenyl-3-aminopropyltrimethoxysilane (manufactured by Tokyo Chemical Industry Co., Ltd.) were mixed, and 214.4 parts by weight of methyl ethyl ketone were added. The mixture was heated on a heating plate at 90°C to obtain a varnish (resin composition).

[0518] Using the obtained varnish, resin sheets and evaluation laminates were obtained using the same method as in Example 1.

[0519] [Example 15]

[0520] 60 parts by mass of MIZ-001 (trade name, mass-average molecular weight (Mw): 3000) manufactured by Nippon Kayaku Co., Ltd. as bismaleimide compound (A), 7.5 parts by mass of compound (B1A) as photocuring initiator (B), 5.25 parts by mass of compound (C1) as compound (C) represented by formula (20), 1.08 parts by mass of cis,cis-cyclohexane-1,2,4-tricarboxylic acid-1,2-anhydride (H-TMAn-S (trade name) manufactured by Mitsubishi Gas Chemical Co., Ltd.) as compound (C), 40 parts by mass of compound (D) represented by formula (25) (BCPH01 (trade name) manufactured by Gunei Chemical Industry Co., Ltd.), and 3 parts by mass of N-phenyl-3-aminopropyltrimethoxysilane (manufactured by Tokyo Kasei Co., Ltd.) were mixed, and 209.7 parts by mass of methyl ethyl ketone were added. The mixture was heated on a heating plate heated to 90°C to obtain a varnish (resin composition).

[0521] Using the obtained varnish, resin sheets and evaluation laminates were obtained using the same method as in Example 1.

[0522] [Example 16]

[0523] The following compounds were prepared: 60 parts by weight of MIZ-001 (trade name, mass-average molecular weight (Mw): 3000) manufactured by Nippon Kayaku Co., Ltd. as bismaleimide compound (A); 6.75 parts by weight of compound (B1A) as photocuring initiator (B); 5.25 parts by weight of compound (C) represented by formula (20); 1.08 parts by weight of cis,cis-cyclohexane-1,2,4-tricarboxylic acid-1,2-anhydride (H-TMAn-S (trade name) manufactured by Mitsubishi Gas Chemical Co., Ltd.) as compound (C); 40 parts by weight of compound (D) represented by formula (25) (BCPH01 (trade name) manufactured by Gunei Chemical Industry Co., Ltd.) as maleimide compound (D); and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (IGM Resins) as photocuring initiator. 0.75 parts by weight of Omnirad 819 (trade name) manufactured by BV and 3 parts by weight of N-phenyl-3-aminopropyltrimethoxysilane (manufactured by Tokyo Chemical Industry Co., Ltd.) were mixed, and 209.7 parts by weight of methyl ethyl ketone were added. The mixture was heated on a heating plate at 90°C to obtain a varnish (resin composition).

[0524] Using the obtained varnish, resin sheets and evaluation laminates were obtained using the same method as in Example 1.

[0525] [Example 17]

[0526] The following compounds were prepared: 60 parts by weight of MIZ-001 (trade name, mass-average molecular weight (Mw): 3000) manufactured by Nippon Kayaku Co., Ltd. as bismaleimide compound (A); 6.38 parts by weight of compound (B1A) as photocuring initiator (B); 5.25 parts by weight of compound (C) represented by formula (20); 1.08 parts by weight of cis,cis-cyclohexane-1,2,4-tricarboxylic acid-1,2-anhydride (H-TMAn-S (trade name) manufactured by Mitsubishi Gas Chemical Co., Ltd.) as compound (C); 40 parts by weight of compound (D) represented by formula (25) (BCPH01 (trade name) manufactured by Gunei Chemical Industry Co., Ltd.) as maleimide compound (D); and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (IGM Resins) as photocuring initiator. 1.12 parts by weight of Omnirad 819 (trade name) manufactured by BV and 3 parts by weight of N-phenyl-3-aminopropyltrimethoxysilane (manufactured by Tokyo Chemical Industry Co., Ltd.) were mixed, and 209.7 parts by weight of methyl ethyl ketone were added. The mixture was heated on a heating plate at 90°C to obtain a varnish (resin composition).

[0527] Using the obtained varnish, resin sheets and evaluation laminates were obtained using the same method as in Example 1.

[0528] [Example 18]

[0529] The following compounds were prepared: 60 parts by weight of MIZ-001 (trade name, mass-average molecular weight (Mw): 3000) manufactured by Nippon Kayaku Co., Ltd. as bismaleimide compound (A); 5.63 parts by weight of compound (B1A) as photocuring initiator (B); 5.25 parts by weight of compound (C) represented by formula (20); 1.08 parts by weight of cis,cis-cyclohexane-1,2,4-tricarboxylic acid-1,2-anhydride (H-TMAn-S (trade name) manufactured by Mitsubishi Gas Chemical Co., Ltd.) as compound (C); 40 parts by weight of compound (D) represented by formula (25) (BCPH01 (trade name) manufactured by Gunei Chemical Industry Co., Ltd.) as maleimide compound (D); and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (IGM Resins) as photocuring initiator. 1.87 parts by weight of Omnirad (registered trademark) 819 (trade name) manufactured by BV and 3 parts by weight of N-phenyl-3-aminopropyltrimethoxysilane (manufactured by Tokyo Chemical Industry Co., Ltd.) were mixed, and 209.7 parts by weight of methyl ethyl ketone were added. The mixture was heated on a heating plate at 90°C to obtain a varnish (resin composition).

[0530] Using the obtained varnish, resin sheets and evaluation laminates were obtained using the same method as in Example 1.

[0531] [Example 19]

[0532] 60 parts by mass of MIZ-001 (trade name, mass-average molecular weight (Mw): 3000) manufactured by Nippon Kayaku Co., Ltd. as bismaleimide compound (A), 6 parts by mass of compound (B1A) as photocuring initiator (B), 5.25 parts by mass of compound (C1) as compound (C) represented by formula (20), 1.08 parts by mass of cis,cis-cyclohexane-1,2,4-tricarboxylic acid-1,2-anhydride (H-TMAn-S (trade name) manufactured by Mitsubishi Gas Chemical Co., Ltd.) as compound (C), 40 parts by mass of compound (D) represented by formula (25) (BCPH01 (trade name) manufactured by Gunei Chemical Industry Co., Ltd.), and 3 parts by mass of N-phenyl-3-aminopropyltrimethoxysilane (manufactured by Tokyo Kasei Co., Ltd.) were mixed, and 206.9 parts by mass of methyl ethyl ketone were added. The mixture was heated on a heating plate heated to 90°C to obtain a varnish (resin composition).

[0533] Using the obtained varnish, resin sheets and evaluation laminates were obtained using the same method as in Example 1.

[0534] [Example 20]

[0535] The following compounds were prepared: 60 parts by weight of MIZ-001 (trade name, mass-average molecular weight (Mw): 3000) manufactured by Nippon Kayaku Co., Ltd. as bismaleimide compound (A); 5.4 parts by weight of compound (B1A) as photocuring initiator (B); 5.25 parts by weight of compound (C) represented by formula (20); 1.08 parts by weight of cis,cis-cyclohexane-1,2,4-tricarboxylic acid-1,2-anhydride (H-TMAn-S (trade name) manufactured by Mitsubishi Gas Chemical Co., Ltd.) as compound (C); 40 parts by weight of compound (D) represented by formula (25) (BCPH01 (trade name) manufactured by Gunei Chemical Industry Co., Ltd.) as maleimide compound (D); and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (IGM Resins) as photocuring initiator. 0.6 parts by weight of Omnirad 819 (trade name) manufactured by BV and 3 parts by weight of N-phenyl-3-aminopropyltrimethoxysilane (manufactured by Tokyo Chemical Industry Co., Ltd.) were mixed, and 206.9 parts by weight of methyl ethyl ketone were added. The mixture was heated on a heating plate at 90°C to obtain a varnish (resin composition).

[0536] Using the obtained varnish, resin sheets and evaluation laminates were obtained using the same method as in Example 1.

[0537] [Example 21]

[0538] The following compounds were prepared: 60 parts by weight of MIZ-001 (trade name, mass-average molecular weight (Mw): 3000) manufactured by Nippon Kayaku Co., Ltd. as bismaleimide compound (A); 5.1 parts by weight of compound (B1A) as photocuring initiator (B); 5.25 parts by weight of compound (C) represented by formula (20); 1.08 parts by weight of cis,cis-cyclohexane-1,2,4-tricarboxylic acid-1,2-anhydride (H-TMAn-S (trade name) manufactured by Mitsubishi Gas Chemical Co., Ltd.) as compound (C); 40 parts by weight of compound (D) represented by formula (25) (BCPH01 (trade name) manufactured by Gunei Chemical Industry Co., Ltd.) as maleimide compound (D); and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (IGM Resins) as photocuring initiator. 0.9 parts by weight of Omnirad 819 (trade name) manufactured by BV and 3 parts by weight of N-phenyl-3-aminopropyltrimethoxysilane (manufactured by Tokyo Chemical Industry Co., Ltd.) were mixed, and 206.9 parts by weight of methyl ethyl ketone were added. The mixture was heated on a heating plate at 90°C to obtain a varnish (resin composition).

[0539] Using the obtained varnish, resin sheets and evaluation laminates were obtained using the same method as in Example 1.

[0540] [Example 22]

[0541] The following compounds were prepared: 60 parts by weight of MIZ-001 (trade name, mass-average molecular weight (Mw): 3000) manufactured by Nippon Kayaku Co., Ltd. as bismaleimide compound (A); 4.5 parts by weight of compound (B1A) as photocuring initiator (B); 5.25 parts by weight of compound (C) represented by formula (20); 1.08 parts by weight of cis,cis-cyclohexane-1,2,4-tricarboxylic acid-1,2-anhydride (H-TMAn-S (trade name) manufactured by Mitsubishi Gas Chemical Co., Ltd.) as compound (C); 40 parts by weight of compound (D) represented by formula (25) (BCPH01 (trade name) manufactured by Gunei Chemical Industry Co., Ltd.) as maleimide compound (D); and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (IGM Resins) as photocuring initiator. 1.5 parts by weight of Omnirad 819 (trade name) manufactured by BV and 3 parts by weight of N-phenyl-3-aminopropyltrimethoxysilane (manufactured by Tokyo Chemical Industry Co., Ltd.) were mixed, and 206.9 parts by weight of methyl ethyl ketone were added. The mixture was heated on a heating plate at 90°C to obtain a varnish (resin composition).

[0542] Using the obtained varnish, resin sheets and evaluation laminates were obtained using the same method as in Example 1.

[0543] [Example 23]

[0544] The following compounds were prepared: 60 parts by weight of MIZ-001 (trade name, mass-average molecular weight (Mw): 3000) manufactured by Nippon Kayaku Co., Ltd. as bismaleimide compound (A); 3 parts by weight of compound (B1A) as photocuring initiator (B); 5.25 parts by weight of compound (C1) as compound (C) represented by formula (20); 1.08 parts by weight of cis,cis-cyclohexane-1,2,4-tricarboxylic acid-1,2-anhydride (H-TMAn-S (trade name) manufactured by Mitsubishi Gas Chemical Co., Ltd.) as compound (C); 40 parts by weight of compound (D) represented by formula (25) (BCPH01 (trade name) manufactured by Gunei Chemical Industry Co., Ltd.) as maleimide compound (D); and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (IGM Resins) as photocuring initiator. BV Corporation's Omnirad (registered trademark) 819 (trade name) 3 parts by weight and N-phenyl-3-aminopropyltrimethoxysilane (manufactured by Tokyo Chemical Industry Co., Ltd.) 3 parts by weight are mixed, and 206.9 parts by weight of methyl ethyl ketone are added. The mixture is heated on a heating plate heated to 90°C to obtain a varnish (resin composition).

[0545] Using the obtained varnish, resin sheets and evaluation laminates were obtained using the same method as in Example 1.

[0546] [Example 24]

[0547] The following compounds were prepared: 60 parts by weight of MIZ-001 (trade name, mass-average molecular weight (Mw): 3000) manufactured by Nippon Kayaku Co., Ltd. as bismaleimide compound (A); 3 parts by weight of compound (B1A) as photocuring initiator (B); 5.25 parts by weight of compound (C1) as compound (C) represented by formula (20); 1.08 parts by weight of cis,cis-cyclohexane-1,2,4-tricarboxylic acid-1,2-anhydride (H-TMAn-S (trade name) manufactured by Mitsubishi Gas Chemical Co., Ltd.) as compound (C); 40 parts by weight of compound (D) represented by formula (25) (BCPH01 (trade name) manufactured by Gunei Chemical Industry Co., Ltd.) as maleimide compound (D); and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (IGM Resins) as photocuring initiator. One part by weight of Omnirad 819 (trade name) manufactured by BV and three parts by weight of N-phenyl-3-aminopropyltrimethoxysilane (manufactured by Tokyo Chemical Industry Co., Ltd.) were mixed, and 203.2 parts by weight of methyl ethyl ketone were added. The mixture was heated on a heating plate heated to 90°C to obtain a varnish (resin composition).

[0548] Using the obtained varnish, resin sheets and evaluation laminates were obtained using the same method as in Example 1.

[0549] [Example 25]

[0550] The following compounds were selected: 60 parts by weight of MIZ-001 (trade name, mass-average molecular weight (Mw): 3000) manufactured by Nippon Kayaku Co., Ltd. as bismaleimide compound (A); 1.7 parts by weight of compound (B1A) as photocuring initiator (B); 5.25 parts by weight of compound (C) represented by formula (20); 1.08 parts by weight of cis,cis-cyclohexane-1,2,4-tricarboxylic acid-1,2-anhydride (H-TMAn-S (trade name) manufactured by Mitsubishi Gas Chemical Co., Ltd.) as compound (C); 40 parts by weight of compound (D) represented by formula (25) (BCPH01 (trade name) manufactured by Gunei Chemical Industry Co., Ltd.) as maleimide compound (D); and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (IGM Resins) as photocuring initiator. 0.3 parts by weight of Omnirad 819 (trade name) manufactured by BV and 3 parts by weight of N-phenyl-3-aminopropyltrimethoxysilane (manufactured by Tokyo Chemical Industry Co., Ltd.) were mixed, and 199.5 parts by weight of methyl ethyl ketone were added. The mixture was heated on a heating plate at 90°C to obtain a varnish (resin composition).

[0551] Using the obtained varnish, resin sheets and evaluation laminates were obtained using the same method as in Example 1.

[0552] [Example 26]

[0553] The following compounds were prepared: 60 parts by weight of MIZ-001 (trade name, mass-average molecular weight (Mw): 3000) manufactured by Nippon Kayaku Co., Ltd. as bismaleimide compound (A); 1 part by weight of compound (B1A) as photocuring initiator (B); 5.25 parts by weight of compound (C1) as compound (C) represented by formula (20); 1.08 parts by weight of cis,cis-cyclohexane-1,2,4-tricarboxylic acid-1,2-anhydride (H-TMAn-S (trade name) manufactured by Mitsubishi Gas Chemical Co., Ltd.) as compound (C); 40 parts by weight of compound (D) represented by formula (25) (BCPH01 (trade name) manufactured by Gunei Chemical Industry Co., Ltd.) as maleimide compound; and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (IGM Resins) as photocuring initiator. One part by weight of Omnirad (registered trademark) 819 (trade name) manufactured by BV and three parts by weight of N-phenyl-3-aminopropyltrimethoxysilane (manufactured by Tokyo Chemical Industry Co., Ltd.) were mixed, and 199.5 parts by weight of methyl ethyl ketone were added. The mixture was heated on a heating plate at 90°C to obtain a varnish (resin composition).

[0554] Using the obtained varnish, resin sheets and evaluation laminates were obtained using the same method as in Example 1.

[0555] [Example 27]

[0556] The following compounds were prepared: 80 parts by weight of MIZ-001 (trade name, mass-average molecular weight (Mw): 3000) manufactured by Nippon Kayaku Co., Ltd. as bismaleimide compound (A); 7.5 parts by weight of compound (B1A) as photocuring initiator (B); 5.25 parts by weight of compound (C) represented by formula (20); 1.08 parts by weight of cis,cis-cyclohexane-1,2,4-tricarboxylic acid-1,2-anhydride (H-TMAn-S (trade name) manufactured by Mitsubishi Gas Chemical Co., Ltd.) as compound (C); 20 parts by weight of compound (D) represented by formula (25) (BCPH01 (trade name) manufactured by Gunei Chemical Industry Co., Ltd.) as maleimide compound (D); and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (IGM Resins) as photocuring initiator. 2.5 parts by weight of Omnirad 819 (trade name) manufactured by BV and 3 parts by weight of N-phenyl-3-aminopropyltrimethoxysilane (manufactured by Tokyo Chemical Industry Co., Ltd.) were mixed, and 221.6 parts by weight of methyl ethyl ketone were added. The mixture was heated on a heating plate at 90°C to obtain a varnish (resin composition).

[0557] Using the obtained varnish, resin sheets and evaluation laminates were obtained using the same method as in Example 1.

[0558] [Example 28]

[0559] 50 parts by weight of MIZ-001 (trade name, mass-average molecular weight (Mw): 3000) manufactured by Nippon Kayaku Co., Ltd. as bismaleimide compound (A), 7.5 parts by weight of compound (B1A) as photocuring initiator (B), 5.25 parts by weight of compound (C) represented by formula (20) as compound (C), 1.08 parts by weight of cis,cis-cyclohexane-1,2,4-tricarboxylic acid-1,2-anhydride (H-TMAn-S (trade name) manufactured by Mitsubishi Gas Chemical Co., Ltd.) as compound (C), 50 parts by weight of compound (D) represented by formula (25) (BCPH01 (trade name) manufactured by Gunei Chemical Industry Co., Ltd.) as maleimide compound (D), and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (IGM Resins) as photocuring initiator. 2.5 parts by weight of Omnirad 819 (trade name) manufactured by BV and 3 parts by weight of N-phenyl-3-aminopropyltrimethoxysilane (manufactured by Tokyo Chemical Industry Co., Ltd.) were mixed, and 221.6 parts by weight of methyl ethyl ketone were added. The mixture was heated on a heating plate at 90°C to obtain a varnish (resin composition).

[0560] Using the obtained varnish, resin sheets and evaluation laminates were obtained using the same method as in Example 1.

[0561] [Example 29]

[0562] The following compounds were prepared: 60 parts by weight of MIZ-001 (trade name, mass-average molecular weight (Mw): 3000) manufactured by Nippon Kayaku Co., Ltd. as bismaleimide compound (A); 7.5 parts by weight of compound (B1A) as photocuring initiator (B); 8.29 parts by weight of compound (C) represented by formula (20); 1.71 parts by weight of cis,cis-cyclohexane-1,2,4-tricarboxylic acid-1,2-anhydride (H-TMAn-S (trade name) manufactured by Mitsubishi Gas Chemical Co., Ltd.) as compound (C); 40 parts by weight of compound (D) represented by formula (25) (BCPH01 (trade name) manufactured by Gunei Chemical Industry Co., Ltd.) as maleimide compound (D); and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (IGM Resins) as photocuring initiator. 2.5 parts by weight of Omnirad (registered trademark) 819 (trade name) manufactured by BV and 3 parts by weight of N-phenyl-3-aminopropyltrimethoxysilane (manufactured by Tokyo Chemical Industry Co., Ltd.) were mixed, and 228.4 parts by weight of methyl ethyl ketone were added. The mixture was heated on a heating plate heated to 90°C to obtain a varnish (resin composition).

[0563] Using the obtained varnish, resin sheets and evaluation laminates were obtained using the same method as in Example 1.

[0564] [Comparative Example 1]

[0565] The following compounds were prepared: 60 parts by weight of MIZ-001 (trade name, mass-average molecular weight (Mw): 3000) manufactured by Nippon Kayaku Co., Ltd. as bismaleimide compound (A); 5.25 parts by weight of compound (C) represented by formula (20); 1.08 parts by weight of cis,cis-cyclohexane-1,2,4-tricarboxylic acid-1,2-anhydride (H-TMAn-S (trade name) manufactured by Mitsubishi Gas Chemical Co., Ltd.) represented by formula (25) as maleimide compound (D) (BCPH01 (trade name) manufactured by Gunei Chemical Industry Co., Ltd.); 15 parts by weight of compound (TMDM) represented by formula (24) as maleimide compound (D); and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (IGM Resins) as a photocuring initiator. BV Corporation's Omnirad (registered trademark) 819 (trade name) 4 parts by weight and N-phenyl-3-aminopropyltrimethoxysilane (manufactured by Tokyo Chemical Industry Co., Ltd.) 3 parts by weight are mixed, and 210.5 parts by weight of methyl ethyl ketone are added. The mixture is heated on a heating plate heated to 90°C to obtain a varnish (resin composition).

[0566] Using the obtained varnish, resin sheets and evaluation laminates were obtained using the same method as in Example 1.

[0567] [Comparative Example 2]

[0568] 60 parts by weight of MIZ-001 (trade name, mass average molecular weight (Mw): 3000) manufactured by Nippon Kayaku Co., Ltd. as bismaleimide compound (A), 5.25 parts by weight of compound (C) represented by formula (20), 1.08 parts by weight of cis,cis-cyclohexane-1,2,4-tricarboxylic acid-1,2-anhydride (H-TMAn-S (trade name) manufactured by Mitsubishi Gas Chemical Co., Ltd.) as compound (C), and 25 parts by weight of compound (D) represented by formula (25) (BCPH01 (trade name) manufactured by Gunei Chemical Industry Co., Ltd.) 15 parts by mass of compound (TMDM) of formula (24) as maleimide compound (D), 4 parts by mass of 1-[4-(phenylthio)phenyl]-1,2-octanedione 2-(O-benzoyl oxime) (manufactured by BASF JAPAN, Irgacure (registered trademark) OXE01 (trade name)) as photocuring initiator, and 3 parts by mass of N-phenyl-3-aminopropyltrimethoxysilane (manufactured by Tokyo Chemical Industry Co., Ltd.) were mixed, and 210.5 parts by mass of methyl ethyl ketone were added. The mixture was heated on a heating plate heated to 90°C to obtain a varnish (resin composition).

[0569] Using the obtained varnish, resin sheets and evaluation laminates were obtained using the same method as in Example 1.

[0570] [Comparative Example 3]

[0571] The following compounds were prepared: 60 parts by weight of MIZ-001 (trade name, mass-average molecular weight (Mw): 3000) manufactured by Nippon Kayaku Co., Ltd. as bismaleimide compound (A); 5.25 parts by weight of compound (C) represented by formula (20); 1.08 parts by weight of cis,cis-cyclohexane-1,2,4-tricarboxylic acid-1,2-anhydride (H-TMAn-S (trade name) manufactured by Mitsubishi Gas Chemical Co., Ltd.) represented by formula (25) represented by maleimide compound (D) (BCPH01 (trade name) manufactured by Gunei Chemical Industry Co., Ltd.) represented by formula (24) represented by maleimide compound (D); 15 parts by weight of 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3-yl]-acetone 1-(O-acetyl oxime) (BASF) represented by formula (24) represented by maleimide compound (D) represented by maleimide compound (D); and 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3-yl]-acetyl ketone 1-(O-acetyl oxime) represented by formula (24) represented by maleimide compound (D) represented by BASF. A mixture of 4 parts by weight of Irgacure (registered trademark) OXE02 (trade name) manufactured by JAPAN Corporation and 3 parts by weight of N-phenyl-3-aminopropyltrimethoxysilane (manufactured by Tokyo Chemical Industry Co., Ltd.), and 210.5 parts by weight of methyl ethyl ketone, was heated on a heating plate to 90°C to obtain a varnish (resin composition).

[0572] Using the obtained varnish, resin sheets and evaluation laminates were obtained using the same method as in Example 1.

[0573] [Comparative Example 4]

[0574] The following compounds were prepared: 60 parts by weight of MIZ-001 (trade name, mass-average molecular weight (Mw): 3000) manufactured by Nippon Kayaku Co., Ltd. as bismaleimide compound (A); 5.25 parts by weight of compound (C) represented by formula (20); 1.08 parts by weight of cis,cis-cyclohexane-1,2,4-tricarboxylic acid-1,2-anhydride (H-TMAn-S (trade name) manufactured by Mitsubishi Gas Chemical Co., Ltd.) represented by formula (25) as maleimide compound (D) (BCPH01 (trade name) manufactured by Gunei Chemical Industry Co., Ltd.); 15 parts by weight of compound (TMDM) represented by formula (24) as maleimide compound (D); and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (IGM Resins) as a photocuring initiator. 3.7 parts by weight of Omnirad 819 (trade name) manufactured by BV Corporation, 1.3 parts by weight of 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3-yl]-ethyl ketone 1-(O-acetyl oxime) (manufactured by BASF JAPAN Corporation, Irgacure OXE02 (trade name) manufactured by BV Corporation) as a photocuring initiator, and 3 parts by weight of N-phenyl-3-aminopropyltrimethoxysilane (manufactured by Tokyo Chemical Industry Co., Ltd.) were mixed, and 213.3 parts by weight of methyl ethyl ketone were added. The mixture was heated on a heating plate heated to 90°C to obtain a varnish (resin composition).

[0575] Using the obtained varnish, resin sheets and evaluation laminates were obtained using the same method as in Example 1.

[0576] [Comparative Example 5]

[0577] The following compounds were prepared: 60 parts by weight of MIZ-001 (trade name, mass-average molecular weight (Mw): 3000) manufactured by Nippon Kayaku Co., Ltd. as bismaleimide compound (A); 5.25 parts by weight of compound (C) represented by formula (20); 1.08 parts by weight of cis,cis-cyclohexane-1,2,4-tricarboxylic acid-1,2-anhydride (H-TMAn-S (trade name) manufactured by Mitsubishi Gas Chemical Co., Ltd.) as compound (C); 40 parts by weight of compound (D) represented by formula (25) (BCPH01 (trade name) manufactured by Gunei Chemical Industry Co., Ltd.); and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (IGM Resins) as photocuring initiator. Two parts by weight of Omnirad 819 (trade name) manufactured by BV and three parts by weight of N-phenyl-3-aminopropyltrimethoxysilane (manufactured by Tokyo Chemical Industry Co., Ltd.) were mixed, and 199.5 parts by weight of methyl ethyl ketone were added. The mixture was heated on a heating plate at 90°C to obtain a varnish (resin composition).

[0578] Using the obtained varnish, resin sheets and evaluation laminates were obtained using the same method as in Example 1.

[0579] 〔evaluate〕

[0580] The resin sheets and evaluation laminates were measured and evaluated using the following methods. The results are shown in Tables 2–5.

[0581] <Photocurability>

[0582] Using a Photo-DSC (TA Instruments DSC-2500) and an optical filter (Lumen Dynamics Group Inc., with wavelengths of 360nm-385nm) that is equipped with a light source (U-VIX Omnicure S2000) capable of irradiating active energy rays containing wavelengths of 200-600nm, the obtained resin sheet was irradiated with active energy rays containing wavelength of 365nm at an illuminance of 14mW for an exposure time of 3.5 minutes, and a curve was obtained with time (sec) on the horizontal axis and heat flux (mW) on the vertical axis.

[0583] In the resulting curve, the peak area at which a horizontal line is drawn from the end of the curve is set as the enthalpy (J / g). Curing properties are evaluated according to the following criteria.

[0584] “AA”: Enthalpy is 1 (J / g) or higher.

[0585] “CC”: Enthalpy less than 1 (J / g).

[0586] It should be noted that an enthalpy of 1 (J / g) or higher means that the resin can be fully cured by exposure at a specified wavelength.

[0587] <Seamlessness>

[0588] For the resulting evaluation laminate, a light source (MIKASA MA-20, trade name) and an optical filter (MIKASA, wavelength 346nm-384nm) capable of irradiating with active energy rays containing wavelengths of 200-600nm were used, with an illuminance of 5mW and an irradiation dose of 50mJ / cm². 2 Irradiation with active energy rays containing a wavelength of 365 nm was performed. Subsequently, the silicon wafer was heated to 90°C for 60 seconds using a heating plate heated to 90°C. It was then cooled to room temperature. The support (PET film) was then peeled off and the wafer was agitated for 180 seconds in a 2.38% TMAH (tetramethylammonium hydroxide) aqueous solution (developer, TOKUYAMA) at 35°C. Adhesion was visually evaluated according to the following criteria.

[0589] “AA”: No resin layer peeling occurred after 180 seconds of oscillation.

[0590] "CC": After oscillation for 180 seconds, the resin layer peels off.

[0591] <Alkali-developable properties>

[0592] For the resulting evaluation laminate, a light source (MIKASA MA-20, trade name) capable of irradiating active energy rays containing wavelengths of 200–600 nm and an optical filter (MIKASA, with an extraction wavelength of 346 nm–384 nm) were used. The light was emitted from the support through a chromium mask with a through-hole pattern (through-hole diameter of 50 μm) at an illuminance of 5 mW and an irradiation dose of 50 mJ / cm². 2 Irradiation with active energy rays containing a wavelength of 365 nm was performed. Subsequently, the silicon wafer was heated at 90°C for 60 seconds using a heating plate heated to 90°C. It was then cooled to room temperature. The support (PET film) was then peeled off and the wafer was agitated for 180 seconds in a 2.38% TMAH (tetramethylammonium hydroxide) aqueous solution (developer, TOKUYAMA) at 35°C. One hundred 50 μm diameter vias were then observed using an optical microscope, and the via aperture ratio was calculated. Alkali developability was evaluated according to the following criteria.

[0593] "AA": After oscillation for 180 seconds, the orifice opening rate is above 50%.

[0594] "AB": After oscillation for 180 seconds, the orifice opening ratio is greater than 30% and less than 50%.

[0595] "CC": After oscillation for 180 seconds, the orifice opening ratio is less than 30%.

[0596] "Unable to evaluate": After oscillation for 180 seconds, the resin layer peeled off, making it impossible to calculate the through-hole opening ratio.

[0597] [Table 2]

[0598]

[0599] [Table 3]

[0600]

[0601] [Table 4]

[0602]

[0603] [Table 5]

[0604]

[0605] As clearly shown in Table 2, according to this embodiment, even when exposed to active energy rays containing a wavelength of 365 nm (i-rays), good photosensitivity is achieved, enabling photocuring. Furthermore, according to this embodiment, a cured product with excellent alkali developability can be obtained.

[0606] This application claims priority to Japanese Patent Application No. 2021-099141, filed with the Japan Patent Office on June 15, 2021, the contents of which are incorporated herein by reference.

[0607] Industrial availability

[0608] The resin composition of this embodiment exhibits excellent photocurability to i-rays with a wavelength of 365 nm during the exposure process and excellent alkaline developability during the development process when manufacturing multilayer printed circuit boards. Therefore, it is industrially useful and can be used in photosensitive films, photosensitive films with supports, prepregs, resin sheets, circuit boards (for laminates, multilayer printed circuit boards, etc.), solder resists, underfill materials, chip bonding materials, semiconductor sealing materials, via filling resins, and component embedding resins, etc.

Claims

1. A resin composition comprising a maleimide compound (A) and a photocurable initiator (B), wherein the maleimide compound (A) comprises a structural unit represented by formula (1) and maleimide groups located at both ends of the molecular chain, and the photocurable initiator (B) has an absorbance of 2.0 or more for i-rays at a wavelength of 365 nm. In formula (1), R1 represents a straight-chain or branched alkylene group with 1 to 16 carbon atoms, or a straight-chain or branched alkenyl group with 2 to 16 carbon atoms; R2 represents a straight-chain or branched alkylene group with 1 to 16 carbon atoms, or a straight-chain or branched alkenyl group with 2 to 16 carbon atoms; R3 independently represents a hydrogen atom, a straight-chain or branched alkyl group with 1 to 16 carbon atoms, or a straight-chain or branched alkenyl group with 2 to 16 carbon atoms; n1 independently represents an integer from 1 to 10. The photocuring initiator (B) comprises the photocuring initiator (B1) shown in formula (2) below and / or the photocuring initiator (B2) shown in formula (3) below. In formula (2), R4 represents acetyl or benzoyl; R5 represents phenyl or naphthyl, optionally with substituents; R6 represents a hydrogen atom, or an alkyl group having 1 to 16 carbon atoms, optionally with substituents, in a straight-chain or branched manner; R7 each independently represents a hydrogen atom, or an alkyl group having 1 to 6 carbon atoms, optionally with substituents, in a straight-chain or branched manner; n2 each independently represents an integer from 1 to 5. In formula (3), R8 represents an aryl group with 6 to 24 carbon atoms that may be substituted, or a heteroaryl group with 3 to 24 carbon atoms that may be substituted; R9 represents an acetyl group or a benzoyl group; R 10 X represents a hydrogen atom, or an alkyl group having 1 to 16 carbon atoms (optionally with substituents) in a straight-chain or branched form; X represents an oxygen atom or a sulfur atom. The resin composition further comprises: a compound (C) containing one or more carboxyl groups. in, The compound (C) containing one or more carboxyl groups includes the compound shown in formula (4) below. In equation (4), R 11 Each independently represents the group or hydrogen atom shown in formula (5) below; R 12 Each of the following independently represents a hydrogen atom or a straight-chain or branched alkyl group having 1 to 6 carbon atoms; wherein at least one R 11 The group is represented by the following formula (5). In equation (5), It represents an atomic bond.

2. The resin composition according to claim 1, further comprising at least one maleimide compound (D) selected from the group consisting of the compound shown in formula (6), the compound shown in formula (7), the compound shown in formula (8), the compound shown in formula (9), the compound shown in formula (10), and the compound shown in formula (11). In equation (6), R 13 R 14 and R 15 Each can independently represent a hydrogen atom, or optionally a straight-chain or branched alkyl group with 1 to 8 carbon atoms and substituents. In equation (7), R 16 R 17 and R 18 Each of the following independently represents a hydrogen atom, a hydroxyl group, or an alkyl group with 1 to 6 carbon atoms that may be substituented; n2 represents an integer from 1 to 10. In equation (8), R 19 Each can independently represent a hydrogen atom, a methyl group, or an ethyl group; R 20 Each can independently represent a hydrogen atom or a methyl group. In equation (9), R 21 Each can independently represent a hydrogen atom or a methyl group; n3 represents an integer from 1 to 10. In equation (10), R 22 Each can independently represent a hydrogen atom, a methyl group, or an ethyl group. In equation (11), R 23 Each can be used to represent a hydrogen atom or a methyl group independently; n4 represents an integer from 1 to 10.

3. A resin sheet having a support body and a resin layer disposed on one or both sides of the support body, The resin layer comprises the resin composition of claim 1.

4. The resin sheet according to claim 3, wherein, The thickness of the resin layer is 1~50μm.

5. A multilayer printed circuit board having an insulating layer and conductor layers formed on one or both sides of the insulating layer, The insulating layer comprises the resin composition of claim 1.

6. A semiconductor device comprising the resin composition of claim 1.

Citation Information

Patent Citations

  • Polyamide resin originated from dimer diamine and optical material made of synthetic resin containing the polyamide

    JP1997012712A

  • Use of oxime ester derivatives of benzocarbazole compounds and photoinitiators in photopolymerizable compositions of said derivatives

    JP2014500852A

  • oxime ester photoinitiator

    JP2016531926A

  • Actuator and actuator element

    JP2021099141A

  • Resin composition, wiring layer laminate for semiconductor, and semiconductor device