A highly conductive, self-lubricating, and highly wear-resistant POE masterbatch and a preparation method thereof
By using a combination of maleic anhydride graft-modified POE, nanomaterials and dispersants in POE masterbatch, the problem of insufficient conductivity and wear resistance of POE masterbatch is solved, and high conductivity, self-lubricating and mechanical properties are achieved. Improved performance, suitable for a variety of applications.
Patent Information
- Application Number
- CN202311292559.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-08
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-10-08
AI Technical Summary
The existing POE masterbatch has deficiencies in improving electrical conductivity, self-lubrication and wear resistance, and cannot take into account mechanical properties, which limits the application of polymer alloy materials.
Using raw materials such as maleic anhydride graft-modified POE, molybdenum disulfide nanosheets, graphene nanosheets, lauric acid-coated high-pigment carbon black, titanate coupling agent and benzene derivative dispersant, etc., through melt grafting Reaction and dispersion treatment, improve interface compatibility and dispersion, enhance conductivity and mechanical properties.
It significantly improves the conductivity, self-lubrication and wear resistance of POE masterbatch, optimizes the mechanical properties, and is suitable for a variety of application scenarios.
Smart Images

Figure CN117534933B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of functional polymer materials, and in particular relates to a highly conductive, self-lubricating and highly wear-resistant POE masterbatch and a preparation method thereof. Background Art
[0002] Polymers have been widely used in aerospace, automotive, semiconductor, electrical industry and other fields. People expect materials to have better mechanical properties, which has promoted more in-depth research on polymer materials. Studies have found that the mechanical properties of polymer composites can be significantly improved by adding one or more modifiers. Small amounts of additives such as fibers, whiskers and particles can be used.
[0003] POE is a new type of thermoplastic elastomer that has both the plasticity of plastic and the elasticity of rubber, giving it excellent processing properties. However, the non-polarity of POE leads to poor compatibility with some polar resins or plastics, and it cannot play a good toughening role; at the same time, it has low impact strength and poor conductivity.
[0004] With the improvement of performance requirements, it is urgent to study polyolefin elastomer POE to improve its performance. Existing research on POE masterbatch focuses on improving wear resistance, but does not take into account other mechanical properties and conductive properties of POE, which greatly limits the application of polymer alloy materials. Summary of the invention
[0005] In view of the deficiencies and needs of the prior art, the purpose of the present invention is to provide a highly conductive, self-lubricating, and highly wear-resistant POE masterbatch and a preparation method thereof. The present invention focuses on improving its conductive properties, self-lubricating properties, wear resistance, and related mechanical properties; ultimately a POE masterbatch with excellent comprehensive performance is obtained.
[0006] In order to achieve the purpose of this application, this application is implemented through the following technical solutions:
[0007] A highly conductive, self-lubricating, and highly wear-resistant POE masterbatch, comprising the following raw materials in parts by weight:
[0008] Maleic anhydride grafted modified POE 60-80 parts,
[0009] 20-30 parts of molybdenum disulfide nanosheets,
[0010] 10-20 parts of graphene nanosheets,
[0011] 6-9 parts of titanate coupling agent,
[0012] 15-20 parts of lauric acid coated high pigment carbon black,
[0013] 5-10 parts of polyethylene wax,
[0014] 1-2 parts of benzene derivative dispersant;
[0015] The preparation steps of the maleic anhydride grafted modified POE are:
[0016] (1) Weigh 50-55 parts of polyolefin elastomer POE, 20-25 parts of maleic anhydride, 7-15 parts of glycidyl methacrylate, and 2-3 parts of diisopropyl peroxide and mix them evenly;
[0017] (2) adding the above mixture into a torque rheometer to melt it and cause a grafting reaction, controlling the grafting temperature to be 170-185°C and the reaction time to be 9-12 minutes;
[0018] (3) After cooling, the reactants are crushed into granules for later use.
[0019] Furthermore, the preparation steps of the lauric acid-coated high-pigment carbon black are as follows: add 20-30 parts of carbon black to a 5wt% NaOH solution, and stir for 5-10 minutes; then filter and add to 40-50 parts of lauric acid, raise the temperature to 130-150°C, and reflux for 2-3 hours; filter, wash, and dry to obtain the lauric acid-coated high-pigment carbon black.
[0020] Furthermore, the ratio of the mass of carbon black to the volume of the NaOH solution is 1 g:10 mL.
[0021] Furthermore, the particle size of the carbon black is 20-30 nm.
[0022] Furthermore, the thickness of the molybdenum sulfide nanosheet is 10-15 nm and the diameter is 300-400 nm; the thickness of the graphene nanosheet is 5-10 nm and the diameter is 10-15 μm.
[0023] Furthermore, the titanate coupling agent is tetra-2-ethylhexyl titanate or tetra-isooctyl titanate.
[0024] The present application uses maleic anhydride as the main grafting agent and glycidyl methacrylate as the auxiliary grafting agent, and adopts a melt grafting method to effectively improve the interface compatibility, increase the interface bonding strength and impact strength.
[0025] When the grafting temperature is too low, the decomposition rate of the initiator will be slowed down, so that the free radical concentration cannot react effectively, resulting in a decrease in the grafting rate; when the temperature is too high, although the free radical concentration increases, it will cause a cross-linking side reaction and is not conducive to grafting. Based on this, the grafting temperature is controlled to be 170-185°C during the melt grafting reaction; more preferably, it is controlled to be 175-180°C.
[0026] Furthermore, the weight average molecular weight of the maleic anhydride grafted modified POE is 60000-65000 and the grafting rate is 2.1-3.2.
[0027] Due to the poor dispersibility of MoS2 nanosheets, they agglomerate during the masterbatch smelting process, resulting in uneven dispersion in the masterbatch, affecting its mechanical properties.
[0028] The σ bonds in graphene link with other carbon atoms to form a honeycomb layered structure of hexagonal rings. It has a unique ultra-thin layer structure and excellent self-lubricating properties. It is a good anti-friction additive; it is also a high thermal conductivity reinforcement material and has excellent electrical conductivity. However, graphene also has the defect of poor dispersibility.
[0029] In order to improve the dispersibility of molybdenum disulfide nanosheets and graphene nanosheets in the masterbatch, the present application uses a benzene derivative dispersant on the one hand; on the other hand, the molybdenum disulfide nanosheets and graphene nanosheets are pre-treated with a titanate coupling agent, and the titanate coupling agent can enter the nanosheet layer structure and form a chemical bond, so that the polarity of the molybdenum disulfide nanosheets and graphene nanosheets increases, which is conducive to bonding with maleic anhydride grafted modified POE during the mixing process, so that they are evenly dispersed in the masterbatch. The titanate coupling agent acts as a bridging medium, so that the molybdenum disulfide nanosheets and graphene nanosheets improve the rigidity of the masterbatch; at the same time, the introduction of molybdenum disulfide nanosheets and graphene nanosheets with polar groups also enhances the intermolecular force, thereby improving the mechanical properties and wear resistance of the masterbatch.
[0030] The present invention uses carbon black as a pigment to obtain a POE masterbatch with high blackness and high gloss. After the carbon black is treated in an alkaline solution, a large number of hydroxyl groups are formed on the surface, and then bonded with carboxyl groups in lauric acid to form condensation, so that the lauric acid is coated on the surface of the carbon black; the compatibility of the coated carbon black with the POE matrix material is significantly improved, the dispersibility in the matrix material is improved, and it is beneficial to improve the bonding strength of the interface.
[0031] Furthermore, the POE masterbatch comprises the following raw materials in parts by weight:
[0032] Maleic anhydride grafted modified POE 65-75 parts,
[0033] 23-37 parts of molybdenum disulfide nanosheets,
[0034] 12-18 parts of graphene nanosheets,
[0035] 7-8 parts of titanate coupling agent,
[0036] 16-18 parts of lauric acid coated high pigment carbon black,
[0037] 6-8 parts of polyethylene wax,
[0038] 1-2 parts of benzene derivative dispersant.
[0039] Furthermore, the preparation steps of the benzene derivative type dispersant are: dissolving 10-15 parts by weight of 4-hexadecylphenol in 30-40 parts by weight of xylene solvent, adding 4-5 parts by weight of γ-mercaptopropyltrimethoxysilane during stirring; introducing inert gas, raising the temperature of the reactor to 80-90°C, and slowly adding 3-4 parts by weight of dihydroxy polyether; continuing the reaction for 3-5 hours; after the reaction is completed, adding a sufficient amount of sodium hydroxide solution to the reactor to remove part of the ring-opened oligomers; separating the organic phase and drying it, and removing the solvent by vacuum evaporation to obtain a yellow liquid dispersant.
[0040] In the preparation of masterbatch, the selection of dispersant has a significant impact on the performance. The appropriate dispersant can ensure that the performance of the masterbatch will not deteriorate. There are also dispersants with good performance in the prior art. During the research process, this application also developed a good dispersant with comparable performance to the existing dispersants.
[0041] Furthermore, the POE masterbatch also includes at least one of an antioxidant and a flame retardant.
[0042] The content of the antioxidant is preferably 0.1-0.5 parts, more preferably 0.2-0.4 parts. The choice of the oxidant is not particularly limited, and any existing antioxidant is acceptable, such as hindered phenol antioxidants and phosphite antioxidants.
[0043] The content of the flame retardant is preferably 5-10 parts, more preferably 7-9 parts; the choice of the flame retardant is not particularly limited, and any existing flame retardant is acceptable, for example: phosphorus-based flame retardant, nitrogen-based flame retardant.
[0044] A method for preparing the above-mentioned highly conductive self-lubricating and highly wear-resistant POE masterbatch comprises the following steps:
[0045] (1) Weigh the raw materials according to the ratio and set aside;
[0046] (2) Adding molybdenum disulfide nanosheets and graphene nanosheets to 40-50 parts of anhydrous ethanol, stirring and dispersing, and then adding a titanate coupling agent; raising the temperature to 70-80°C, reflux reaction for 1-2 hours, filtering, washing, and drying for later use;
[0047] (3) The mixture prepared in step (2) is mixed evenly with lauric acid-coated high-color carbon black and polyethylene wax to obtain material A; maleic anhydride-grafted modified POE and a dispersant are mixed evenly to obtain material B;
[0048] (4) Add material A and material B into a continuous internal mixer and mix them evenly at high temperature;
[0049] (5) The product is then fed into a screw extruder via an automatic elevator. The temperature of the screw extruder is set as follows: 100-110°C for the first section, 110-120°C for the second section, 120-125°C for the third section, 110-120°C for the fourth section, and 105°C for the fifth section. The product is extruded by the screw extruder, air-cooled, and pelletized to obtain the POE masterbatch.
[0050] Furthermore, in step (2), the high-temperature banburying temperature is controlled at 105-115°C.
[0051] An application of the POE masterbatch in alloy materials such as PA, PC, ABS, PET, PBT, UPE, and PTFE.
[0052] Compared with the prior art, the present invention has the following beneficial effects:
[0053] (1) Molybdenum disulfide nanosheets and graphene nanosheets are excellent anti-friction materials. This application uses both of them as wear-resistant additives, which can significantly improve the self-lubricating and anti-friction properties of PEO masterbatch. In addition, based on the conductivity of graphene and carbon black, the PEO masterbatch is endowed with good conductivity, which can meet different application needs and scenarios.
[0054] (2) Maleic anhydride is used as the main grafting agent and glycidyl methacrylate is used as the auxiliary grafting agent for POE grafting treatment and used as the masterbatch substrate, which has the effect of effectively improving the interface compatibility, increasing the interface bonding strength and impact strength.
[0055] (3) The present invention utilizes alkaline solution and lauric acid to pretreat carbon black, so that lauric acid is coated on the surface of carbon black. The compatibility of the coated carbon black with the POE matrix material is significantly improved, the dispersibility in the matrix material is improved, and it is beneficial to improve the bonding strength of the interface.
[0056] (4) The present application also provides a benzene derivative dispersant, which has comparable performance to existing dispersants.
[0057] (5) The POE masterbatch prepared in the present application has excellent wear resistance and self-lubricating properties, as well as good electrical conductivity and mechanical properties. It can be widely used in the food, medical and health industries. BRIEF DESCRIPTION OF THE DRAWINGS
[0058] Figure 1 This is the infrared spectrum of the maleic anhydride grafted modified POE prepared in Example 1.
[0059] Figure 2 This is the infrared spectrum of the benzene derivative dispersant prepared in Example 1. DETAILED DESCRIPTION
[0060] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples, but it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention.
[0061] Example 1
[0062] Preparation of raw materials: POE was purchased from Dow Chemical Company of the United States. Glycidyl methacrylate was purchased from Guangzhou Yuanda New Materials Co., Ltd. Molybdenum disulfide nanosheets were purchased from Suzhou Kaifa New Materials Technology Co., Ltd., with a thickness of 10-15nm and a diameter of 300-400nm; graphene nanosheets were purchased from Guangzhou Hongwu Materials Technology Co., Ltd., with a thickness of 5-10nm and a diameter of 10-15μm. Carbon black powder was purchased from Tianjin Yihuachang New Materials Technology Co., Ltd., with a particle size of 20-30nm.
[0063] 1. The preparation steps of maleic anhydride grafted modified POE are:
[0064] (1) Weigh 52 parts of polyolefin elastomer POE, 24 parts of maleic anhydride, 10 parts of glycidyl methacrylate, and 2.4 parts of diisopropyl peroxide and mix them evenly; (2) Add the above mixture into a torque rheometer to melt it and cause a grafting reaction. The grafting temperature is controlled to be 175°C and the reaction time is 12 minutes; (3) After the reactants are cooled, they are crushed and granulated for later use.
[0065] 2. The preparation steps of lauric acid-coated high-pigment carbon black are as follows: add 25 parts of carbon black to 5wt% NaOH solution and stir for 7 minutes; then filter and add to 46 parts of lauric acid, raise the temperature to 138°C and reflux for 2.5 hours; filter, wash and dry to obtain lauric acid-coated high-pigment carbon black; wherein the ratio of the mass of carbon black to the volume of NaOH solution is 1g:10mL.
[0066] 3. The preparation steps of the benzene derivative type dispersant are as follows: dissolve 12 parts by weight of 4-hexadecylphenol in 36 parts by weight of xylene solvent, add 4.4 parts by weight of γ-mercaptopropyltrimethoxysilane during stirring; introduce inert gas, increase the temperature of the reactor to 86°C, and slowly add 3.7 parts by weight of dihydroxy polyether; continue the reaction for 4 hours; after the reaction is completed, add a sufficient amount of sodium hydroxide solution to the reactor to remove some of the ring-opened oligomers; separate the organic phase and dry it, and remove the solvent by vacuum evaporation to obtain a yellow liquid dispersant.
[0067] The prepared maleic anhydride grafted modified POE was pressed into a sheet and characterized by infrared spectroscopy. The scanning wavelength range was 4500-450 cm -1 . Infrared spectrum analysis shows that maleic anhydride and glycidyl methacrylate are successfully grafted onto the POE matrix. The grafting rate is 2.7 as measured by chemical titration, and the weight average molecular weight is 64300 as measured by viscosity method.
[0068] The prepared benzene derivative dispersant was pressed into tablets and characterized by infrared spectroscopy. The scanning wavelength range was 4000-500 cm -1 .
[0069] Figure 2 The infrared spectrum of the benzene derivatives shows a characteristic absorption band at 931 cm -1 and 1229cm -1 ; at 1460cm -1 、1509cm -1 、1582cm -1 Double peaks were observed at 1609cm -1 、2929cm -1 、3035cm -1 It is mainly due to the stretching vibration of CH2 of the benzene ring and the alkyl group caused by asymmetry and symmetry.
[0070] Unless otherwise specified, the raw materials used in the following examples are prepared in Example 1.
[0071] Example 2
[0072] A highly conductive, self-lubricating, and highly wear-resistant POE masterbatch, comprising the following raw materials in parts by weight:
[0073] 60 parts of maleic anhydride grafted modified POE, 20 parts of molybdenum disulfide nanosheets, 10 parts of graphene nanosheets, 6 parts of tetra-2-ethylhexyl titanate, 15 parts of lauric acid-coated high-color carbon black, 5 parts of polyethylene wax, and 1 part of benzene derivative dispersant.
[0074] The preparation method of the above-mentioned highly conductive self-lubricating and highly wear-resistant POE masterbatch comprises the following steps:
[0075] (1) Weigh the raw materials according to the ratio and set aside;
[0076] (2) Adding molybdenum disulfide nanosheets and graphene nanosheets to 40 parts of anhydrous ethanol, stirring and dispersing, and then adding tetra-2-ethylhexyl titanate; raising the temperature to 75° C., reflux reaction for 2 hours, filtering, washing, and drying for later use;
[0077] (3) The mixture prepared in step (2) is mixed evenly with lauric acid-coated high-color carbon black and polyethylene wax to obtain material A; maleic anhydride-grafted modified POE and a dispersant are mixed evenly to obtain material B;
[0078] (4) Add material A and material B into a continuous internal mixer and mix them evenly at high temperature. The temperature is controlled at 110°C.
[0079] (5) The product is then fed into a screw extruder via an automatic elevator. The temperature of the screw extruder is set as follows: 100° C. for the first section, 110° C. for the second section, 120° C. for the third section, 110° C. for the fourth section, and 105° C. for the fifth section. The product is extruded by the screw extruder, air-cooled, and pelletized to obtain the POE masterbatch.
[0080] Example 3
[0081] A highly conductive, self-lubricating, and highly wear-resistant POE masterbatch, comprising the following raw materials in parts by weight:
[0082] 80 parts of maleic anhydride grafted modified POE, 30 parts of molybdenum disulfide nanosheets, 20 parts of graphene nanosheets, 9 parts of tetra-2-ethylhexyl titanate, 20 parts of lauric acid-coated high-color carbon black, 10 parts of polyethylene wax, and 2 parts of benzene derivative dispersant.
[0083] The preparation method of the above-mentioned highly conductive self-lubricating and highly wear-resistant POE masterbatch comprises the following steps:
[0084] (1) Weigh the raw materials according to the ratio and set aside;
[0085] (2) Adding molybdenum disulfide nanosheets and graphene nanosheets to 50 parts of anhydrous ethanol, stirring and dispersing, and then adding tetra-2-ethylhexyl titanate; raising the temperature to 80° C., reflux reaction for 1 hour, filtering, washing, and drying for later use;
[0086] (3) The mixture prepared in step (2) is mixed evenly with lauric acid-coated high-color carbon black and polyethylene wax to obtain material A; maleic anhydride grafted modified POE and a dispersant are mixed evenly to obtain material B;
[0087] (4) Add material A and material B into a continuous internal mixer and mix them evenly at high temperature. The temperature is controlled at 108°C.
[0088] (5) The product is then sent to a screw extruder via an automatic elevator. The temperature of the screw extruder is set to: 110° C. for the first section, 120° C. for the second section, 125° C. for the third section, 120° C. for the fourth section, and 105° C. for the fifth section. The product is extruded by the screw extruder, air-cooled and pelletized to obtain the POE masterbatch.
[0089] Example 4
[0090] A highly conductive, self-lubricating, and highly wear-resistant POE masterbatch, comprising the following raw materials in parts by weight:
[0091] 70 parts of maleic anhydride grafted modified POE, 25 parts of molybdenum disulfide nanosheets, 15 parts of graphene nanosheets, 8 parts of tetraethylhexyl titanate, 17 parts of lauric acid-coated high-color carbon black, 8 parts of polyethylene wax, and 1.8 parts of benzene derivative dispersant.
[0092] The preparation method of the above-mentioned highly conductive self-lubricating and highly wear-resistant POE masterbatch comprises the following steps:
[0093] (1) Weigh the raw materials according to the ratio and set aside;
[0094] (2) Add molybdenum disulfide nanosheets and graphene nanosheets to 45 parts of anhydrous ethanol, stir and disperse, and then add tetraethyl hexyl titanate; raise the temperature to 80°C, reflux for 1.5 hours, filter, wash, and dry for later use;
[0095] (3) The mixture prepared in step (2) is mixed evenly with lauric acid-coated high-color carbon black and polyethylene wax to obtain material A; maleic anhydride-grafted modified POE and a dispersant are mixed evenly to obtain material B;
[0096] (4) Add material A and material B into a continuous internal mixer and mix them evenly at high temperature. The temperature is controlled at 115°C.
[0097] (5) The product is then fed into a screw extruder via an automatic elevator. The temperature of the screw extruder is set to: 105° C. for the first section, 115° C. for the second section, 120° C. for the third section, 115° C. for the fourth section, and 105° C. for the fifth section. The product is extruded by the screw extruder, air-cooled and pelletized to obtain the POE masterbatch.
[0098] Example 5
[0099] A highly conductive, self-lubricating, and highly wear-resistant POE masterbatch, comprising the following raw materials in parts by weight:
[0100] 62 parts of maleic anhydride grafted modified POE, 28 parts of molybdenum disulfide nanosheets, 13 parts of graphene nanosheets, 7 parts of tetraethyl heptyl titanate, 19 parts of lauric acid-coated high-color carbon black, 10 parts of polyethylene wax, and 1.3 parts of benzene derivative dispersant.
[0101] The preparation method of the above-mentioned highly conductive self-lubricating and highly wear-resistant POE masterbatch comprises the following steps:
[0102] (1) Weigh the raw materials according to the ratio and set aside;
[0103] (2) Add molybdenum disulfide nanosheets and graphene nanosheets to 50 parts of anhydrous ethanol, stir and disperse, and then add tetraethyl hexyl titanate; raise the temperature to 75°C, reflux for 2 hours, filter, wash, and dry for later use;
[0104] (3) The mixture prepared in step (2) is mixed evenly with lauric acid-coated high-color carbon black and polyethylene wax to obtain material A; maleic anhydride-grafted modified POE and a dispersant are mixed evenly to obtain material B;
[0105] (4) Add material A and material B into a continuous internal mixer and mix them evenly at high temperature. The temperature is controlled at 105°C.
[0106] (5) The product is then sent to a screw extruder via an automatic elevator. The temperature of the screw extruder is set as follows: 100° C. for the first section, 118° C. for the second section, 124° C. for the third section, 116° C. for the fourth section, and 105° C. for the fifth section. The product is extruded by the screw extruder, air-cooled and pelletized to obtain the POE masterbatch.
[0107] The performance of the POE masterbatch prepared in Example 2-5 was tested:
[0108] The friction and wear performance was tested according to GB / T 3960-2016 standard, with a sample size of 30×7×6mm, a load of 30kg, and a transmission speed of 200r·min -1 , stainless steel friction ring φ40×φ16×10mm. The bending strength is tested according to the national standard GB / T9341-2008, and the impact strength is tested according to GB / T1843-80.
[0109] The conductivity test uses the surface resistance test standard ASTM D257-2007, and the conductivity can be determined based on the surface resistance.
[0110] The blackness test is measured according to GB / T 7048-2012.
[0111] The experimental data of the above experiments are recorded in Table 1.
[0112] Table 1
[0113] ;
[0114] From the above data, it can be seen that the POE masterbatch prepared in this application has a low friction coefficient and wear amount, and the surface has self-lubricating and wear-resistant properties. The tensile strength is as high as 20MPa, the bending strength is about 30MPa, and the notched impact strength reaches 7 kJ·m 2 , showing excellent mechanical properties and good toughening effect. And the surface resistance is 9×10 4 The Ω level also shows that POE masterbatch has good conductivity.
[0115] From the appearance point of view, the POE masterbatch prepared in this application has high blackness and good gloss.
[0116] The above embodiments are preferred implementation schemes of the present invention. In addition, the present invention may also be implemented in other ways. Any obvious replacement without departing from the concept of the present invention is within the protection scope of the present invention.
Claims
1. A highly conductive, self-lubricating, and highly wear-resistant POE masterbatch, characterized in that: According to weight parts, it includes the following raw materials: Maleic anhydride grafted modified POE 60-80 parts, 20-30 parts of molybdenum disulfide nanosheets, 10-20 parts of graphene nanosheets, 6-9 parts of titanate coupling agent, 15-20 parts of lauric acid coated high pigment carbon black, 5-10 parts of polyethylene wax, 1-2 parts of benzene derivative dispersant; The preparation steps of the maleic anhydride grafted modified POE are: (1) Weigh 50-55 parts of polyolefin elastomer POE, 20-25 parts of maleic anhydride, 7-15 parts of glycidyl methacrylate, and 2-3 parts of dicumyl peroxide and mix them evenly; (2) adding the above mixture into a torque rheometer to melt it and cause a grafting reaction, controlling the grafting temperature to be 170-185° C. and the reaction time to be 9-12 min; (3) cooling the reactants and crushing and granulating them for later use; The preparation steps of the benzene derivative type dispersant are as follows: dissolving 10-15 parts by weight of 4-hexadecylphenol in 30-40 parts by weight of xylene solvent, adding 4-5 parts by weight of γ-mercaptopropyltrimethoxysilane during stirring; introducing inert gas, raising the temperature of the reactor to 80-90° C., and slowly adding 3-4 parts by weight of dihydroxy polyether; continuing the reaction for 3-5 hours; adding a sufficient amount of sodium hydroxide solution to the reactor after the reaction is completed; separating the organic phase and drying it, and removing the solvent by vacuum evaporation to obtain a yellow liquid dispersant.
2. The highly conductive, self-lubricating, and highly wear-resistant POE masterbatch according to claim 1, characterized in that: The POE masterbatch comprises the following raw materials in parts by weight: Maleic anhydride grafted modified POE 65-75 parts, 23-28 parts of molybdenum disulfide nanosheets, 12-18 parts of graphene nanosheets, 7-8 parts of titanate coupling agent, 16-18 parts of lauric acid coated high pigment carbon black, 6-8 parts of polyethylene wax, 1-2 parts of benzene derivative dispersant.
3. The highly conductive, self-lubricating, and highly wear-resistant POE masterbatch according to claim 1 or 2, characterized in that: The thickness of the molybdenum sulfide nanosheet is 10-15nm and the diameter is 300-400nm; the thickness of the graphene nanosheet is 5-10nm and the diameter is 10-15μm.
4. The highly conductive, self-lubricating, and highly wear-resistant POE masterbatch according to claim 1 or 2, characterized in that: The preparation steps of the lauric acid coated high-color carbon black are as follows: 20-30 parts of carbon black are added to a 5wt% NaOH solution, and stirred for 5-10 minutes; then filtered and added to 40-50 parts of lauric acid, and the temperature is raised to 130-150° C. and refluxed for 2-3 hours; Filtration, washing and drying are performed to obtain lauric acid-coated high-pigment carbon black; the ratio of the mass of carbon black to the volume of NaOH solution is 1 g:10 mL; and the particle size of the carbon black is 20-30 nm.
5. The highly conductive, self-lubricating, and highly wear-resistant POE masterbatch according to claim 1 or 2, characterized in that: The titanate coupling agent is tetra-2-ethylhexyl titanate or tetra-isooctyl titanate.
6. The highly conductive, self-lubricating, and highly wear-resistant POE masterbatch according to claim 1 or 2, characterized in that: The weight average molecular weight of the maleic anhydride grafted modified POE is 60,000-65,000.
7. The highly conductive, self-lubricating, and highly wear-resistant POE masterbatch according to claim 1 or 2, characterized in that: The POE masterbatch further comprises at least one of an antioxidant and a flame retardant.
8. A method for preparing the highly conductive self-lubricating and highly wear-resistant POE masterbatch according to any one of claims 1 to 7, characterized in that: The following steps are involved: (1) Weigh each raw material according to the ratio and set aside; (2) adding molybdenum disulfide nanosheets and graphene nanosheets to 40-50 parts of anhydrous ethanol, stirring and dispersing, and then adding a titanate coupling agent; raising the temperature to 70-80° C., reflux reaction for 1-2 hours, filtering, washing, and drying for later use; (3) The mixture prepared in step (2) is mixed evenly with lauric acid-coated high-color carbon black and polyethylene wax to form material A; maleic anhydride grafted modified POE and a dispersant are mixed evenly to form material B; (4) Add material A and material B into a continuous internal mixer and mix them evenly at high temperature; (5) The pellets are then fed into a screw extruder via an automatic elevator, and the temperatures of the screw extruder are set to: 100-110° C. for the first section, 110-120° C. for the second section, 120-125° C. for the third section, 110-120° C. for the fourth section, and 105° C. for the fifth section; the pellets are extruded through the screw extruder, air-cooled, and pelletized to obtain the POE masterbatch; In the step (4), the high temperature banburying temperature is controlled at 105-115°C.
9. An application of the highly conductive, self-lubricating, and highly wear-resistant POE masterbatch according to any one of claims 1 to 7 in PA, PC, ABS, PET, PBT, UPE, and PTFE alloy materials.