Highly weather-resistant nano thermal insulation coating and preparation method thereof
By combining deionized water, hydroxyethyl cellulose, aerogels, glass beads, nanomaterials and tungsten-containing compounds in the formulation of the paint, the problems of shrinkage, cracking and peeling of the paint in high solar radiation environments are solved, achieving Stable thermal insulation effect and radiation protection performance improvement.
Patent Information
- Application Number
- CN202311269780.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-28
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-09-28
AI Technical Summary
Existing thermal insulation coatings are prone to shrinkage, cracking and peeling in high solar radiation environments, affecting their insulation effect and durability.
It adopts a highly weather-resistant nano-insulation coating formula, including deionized water, hydroxyethyl cellulose, aerogel, glass beads, nano-silica, nano-alumina, elastic emulsion and tungsten-containing compounds. It is formed by stirring evenly and then letting it stand. Uniform coating and enhance the thermal insulation, radiation protection and mechanical properties of the coating.
Maintain the stable performance of coatings in high solar radiation environments, prevent shrinkage, cracking and peeling, improve thermal insulation and radiation protection properties, and extend the service life of coatings.
Smart Images

Figure BDA0004475234960000091
Abstract
Description
Technical Field
[0001] The invention relates to a highly weather-resistant nano thermal insulation coating and a preparation method thereof. Background Art
[0002] In modern construction projects, thermal insulation coatings play an important role in the thermal insulation of exterior walls. In particular, coatings containing aerogels and glass beads have been widely used in various types of buildings due to their excellent thermal insulation properties. Such coatings can effectively isolate the transmission of heat, thereby greatly improving the energy efficiency of buildings and bringing great comfort to people's lives. However, despite the above advantages of such coatings, their performance may be seriously affected in some special environments.
[0003] In particular, conventional thermal insulation coatings may have some problems in high solar radiation environments. For example, high solar radiation environments may accelerate the oxidation, discoloration and even aging of the coating, thus affecting its protection and durability. More seriously, high solar radiation environments may cause the coating to shrink, crack or even fall off, further affecting the thermal insulation effect of the coating and may eventually lead to the failure of the coating.
[0004] These problems are mainly caused by the uneven distribution of stress inside the coating and the weakening of the adhesion between the coating and the substrate. High solar radiation environment may accelerate the speed of chemical reactions inside the coating, resulting in a large number of free radicals inside the coating, which will destroy the molecular structure inside the coating, thereby causing the coating to shrink and crack. At the same time, high solar radiation environment may also destroy the chemical bond between the coating and the substrate, causing the coating to fall off.
[0005] Therefore, in the face of the severe challenges posed by high solar radiation environments to coatings, developing a thermal insulation coating that can maintain stable performance in a high solar radiation environment and is not prone to shrinkage, cracking, and falling off problems in order to meet a wider range of application needs has become an important research topic in this field. Summary of the invention
[0006] In view of the defects of the prior art, the present invention provides a highly weather-resistant nano-insulating coating and a preparation method, which can effectively solve the problems of shrinkage, cracking and falling off that are prone to occur in existing coatings under high solar radiation environments.
[0007] The technical solution of the present invention is as follows:
[0008] The present invention provides a highly weather-resistant nano thermal insulation coating, comprising the following raw materials:
[0009] Deionized water: 80-300 parts by weight;
[0010] Hydroxyethyl cellulose: 1-15 parts by weight;
[0011] Aerogel: 40-120 parts by weight;
[0012] Glass microspheres: 80-250 parts by weight;
[0013] Nano silicon dioxide: 80-250 parts by weight;
[0014] Nano-alumina: 3-50 parts by weight;
[0015] Elastic emulsion: 80-250 parts by weight;
[0016] Tungsten-containing compound: 10-80 parts by weight.
[0017] Preferably, a highly weather-resistant nano thermal insulation coating comprises the following raw materials:
[0018] Deionized water: 100-250 parts by weight;
[0019] Hydroxyethyl cellulose: 2-10 parts by weight;
[0020] Aerogel: 50-100 parts by weight;
[0021] Glass microspheres: 100-200 parts by weight;
[0022] Nano silicon dioxide: 100-200 parts by weight;
[0023] Nano-alumina: 5-40 parts by weight;
[0024] Elastic emulsion: 100-200 parts by weight;
[0025] Tungsten-containing compound: 20-70 parts by weight.
[0026] Preferably, a highly weather-resistant nano thermal insulation coating comprises the following raw materials:
[0027] Deionized water: 150-200 parts by weight;
[0028] Hydroxyethyl cellulose: 4-7 parts by weight;
[0029] Aerogel: 60-80 parts by weight;
[0030] Glass microspheres: 120-160 parts by weight;
[0031] Nano silicon dioxide: 130-150 parts by weight;
[0032] Nano-alumina: 10-30 parts by weight;
[0033] Elastic emulsion: 120-150 parts by weight;
[0034] Tungsten-containing compound: 30-60 parts by weight.
[0035] Preferably, a highly weather-resistant nano thermal insulation coating comprises the following raw materials:
[0036] Deionized water: 160-180 parts by weight;
[0037] Hydroxyethyl cellulose: 5-6 parts by weight;
[0038] Aerogel: 65-75 parts by weight;
[0039] Glass microspheres: 130-140 parts by weight;
[0040] Nano silicon dioxide: 135-145 parts by weight;
[0041] Nano-alumina: 15-25 parts by weight;
[0042] Elastic emulsion: 130-140 parts by weight;
[0043] Tungsten-containing compound: 30-50 parts by weight.
[0044] In the present invention, the specific functions of each raw material are as follows:
[0045] Deionized water is the basic solvent for making coatings and can effectively mix other raw materials.
[0046] Hydroxyethyl cellulose is a high-quality thickener and stabilizer that can improve the viscosity and stability of the paint, making it easier to apply and preventing other ingredients in the paint from settling.
[0047] Aerogel is a highly efficient thermal insulation material with extremely low thermal conductivity and high thermal resistance. It can effectively block the transfer of heat and provide excellent thermal insulation effect.
[0048] Glass microspheres have good thermal insulation and mechanical properties, and can increase the thermal insulation effect and wear and pressure resistance of coatings.
[0049] Nano-silica has good UV blocking properties and enhances the wear resistance of coatings, and can protect the coatings to maintain stable performance in high solar radiation environments.
[0050] Nano-alumina has high thermal stability and wear resistance, which can increase the stability of coatings in high temperature environments and prevent thermal aging of coatings.
[0051] The elastic emulsion can provide the coating with good ductility and toughness, and prevent the coating from cracking and falling off during thermal expansion and contraction. Preferably, the elastic emulsion is selected from: BATF Acronal 7588, BATF RS-9699H, BASF Acronal 7016G, Arkema ENCOR 187, and these elastic emulsions have good weather resistance and wear resistance.
[0052] The tungsten-containing compound has good radiation protection performance, can block high-energy radiation, and further improve the stability, color and physical properties of the coating in a high solar radiation environment. The tungsten-containing compound can be a water-soluble tungsten-containing compound or a water-insoluble tungsten-containing compound. The water-soluble tungsten-containing compound can be sodium tungstate or ammonium tungstate; the water-insoluble tungsten-containing compound can be calcium tungstate, barium tungstate, tungsten carbide or copper tungstate. Selecting a water-insoluble tungsten-containing compound can improve the water resistance of the coating and reduce the risk of the coating falling off when washed by rain. Particularly preferably, the tungsten-containing compound is barium tungstate and / or tungsten carbide.
[0053] The present invention also provides, for example, a method for preparing a highly weather-resistant nano thermal insulation coating, comprising the following steps:
[0054] Hydroxyethyl cellulose is added into deionized water, and then aerogel, glass microbeads, nano silicon dioxide, nano aluminum oxide, elastic emulsion and tungsten-containing compound are added and stirred evenly to obtain the high weather-resistant nano thermal insulation coating of the present invention.
[0055] The highly weather-resistant nano thermal insulation coating of the present invention can not only provide excellent thermal insulation effect, but also maintain stable performance in high solar radiation environment, effectively solving the problem of easy shrinkage, cracking and shedding of coating in high solar radiation environment. In addition, this coating further improves the radiation protection performance of the coating by introducing special radiation protection ingredients, such as sodium tungstate, so that the coating can maintain good color and physical properties in high solar radiation environment.
[0056] In summary, the full-effect gel thermal insulation coating and its preparation method of the present invention fully consider the performance requirements of the coating in a high solar radiation environment. Through scientific formula design and advanced preparation technology, it successfully solves the shrinkage, cracking and falling problems that are prone to occur in existing coatings in a high solar radiation environment, provides a new solution, and broadens new areas for the application of coatings. DETAILED DESCRIPTION
[0057] The present invention provides a highly weather-resistant nano thermal insulation coating, comprising the following raw materials:
[0058] Deionized water: 160-180 parts by weight;
[0059] Hydroxyethyl cellulose: 5-6 parts by weight;
[0060] Aerogel: 65-75 parts by weight;
[0061] Glass microspheres: 130-140 parts by weight;
[0062] Nano silicon dioxide: 135-145 parts by weight;
[0063] Nano-alumina: 15-25 parts by weight;
[0064] Elastic emulsion: 130-140 parts by weight;
[0065] Tungsten-containing compound: 30-50 parts by weight.
[0066] The tungsten-containing compound is a water-soluble tungsten-containing compound or a water-insoluble tungsten-containing compound. The water-soluble tungsten-containing compound may be sodium tungstate or ammonium tungstate; the water-insoluble tungsten-containing compound may be calcium tungstate, barium tungstate, tungsten carbide or copper tungstate.
[0067] In the present invention, hydroxyethyl cellulose plays a role of thickening and stabilization, improves the fluidity and stability of the coating, makes it more convenient to apply, and avoids the precipitation of various components in the coating. Aerogel is an excellent thermal insulation material with extremely low thermal conductivity and high thermal resistance, which effectively prevents the loss of heat. Glass beads enhance the thermal insulation performance and wear and pressure resistance of the coating. Nano-silicon dioxide has excellent ultraviolet resistance and the characteristics of improving the wear resistance of the coating, ensuring that the coating still maintains stable performance under strong solar radiation. Nano-alumina has high heat resistance and wear resistance, which helps to improve the stability of the coating under high temperature conditions and prevent premature aging of the coating. Elastic emulsion gives the coating good elasticity and toughness, avoids cracks or falling off in the thermal expansion and contraction caused by temperature changes, and enhances the weather resistance and wear resistance of the coating. Tungsten-containing compounds show excellent radiation protection capabilities and can resist high-energy radiation, thereby further improving the stability, color retention and physical properties of the coating in a high-radiation environment.
[0068] The preparation method of the highly weather-resistant nano thermal insulation coating comprises the following steps:
[0069] First, take 160-180 parts by weight of deionized water, adjust the temperature to 25-35° C., and keep the temperature constant.
[0070] Add 5-6 parts by weight of hydroxyethyl cellulose to deionized water maintained at a constant temperature, and stir with a stirrer at a speed of 300-500 rpm until the hydroxyethyl cellulose is dissolved. The stirring time is about 60-90 minutes.
[0071] 65-75 parts by weight of aerogel are gradually added to the hydroxyethyl cellulose solution, and the mixture is stirred again at a speed of 300-500 rpm for about 30-60 minutes using a stirrer.
[0072] Then, 130-140 parts by weight of glass micro beads and 135-145 parts by weight of nano silicon dioxide are added to the mixed solution, and stirring is continued at a speed of 300-500 rpm for about 30-60 minutes.
[0073] Next, 15-25 parts by weight of nano-alumina and 130-140 parts by weight of elastic emulsion are added, and stirring is continued at a speed of 300-500 rpm for about 30-60 minutes.
[0074] Finally, 5-7 parts by weight of a tungsten-containing compound is added, and stirring is continued at a speed of 300-500 rpm for about 30-60 minutes.
[0075] After stirring, the coating is placed at room temperature for 24-48 hours to allow all components to fully contact and form a uniform, highly weather-resistant nano-insulating coating.
[0076] The obtained coating is packaged and stored in a cool and dry environment for use.
[0077] In the preparation process of the highly weather-resistant nano thermal insulation coating of the present invention, the interaction and cooperation between the raw materials achieve the thermal insulation effect in a unique and efficient way. First, hydroxyethyl cellulose, as a thickener and stabilizer, improves the viscosity of the coating, so that various thermal insulation materials such as aerogel and glass microspheres can be evenly distributed in the coating, and their thermal insulation effect is maximized. Aerogel effectively blocks the transfer of heat with its extremely low thermal conductivity and high thermal resistance. The unique microstructure of glass microspheres forms a large number of tiny air gaps, which form an effective thermal insulation layer. The synergistic effect of the two greatly enhances the thermal insulation effect of the coating. On this basis, the addition of nano silicon dioxide and nano aluminum oxide further enhances the performance of the coating. These two nano materials prevent the influence of ultraviolet radiation on the coating, and their high thermal stability can resist high temperature and protect the coating from the influence of thermal aging. This not only maintains the thermal insulation performance of aerogel and glass microspheres in the coating, but also ensures the stability of the coating under high solar radiation environment. In addition, the addition of elastic emulsion provides good ductility and toughness for the coating, preventing the coating from cracking and falling off during thermal expansion and contraction. In this way, no matter how the ambient temperature changes, the coating can maintain good thermal insulation properties, thereby maintaining and enhancing the thermal insulation system constructed by aerogel, glass beads and nanomaterials.
[0078] The present invention adopts the addition of tungsten-containing compounds to the coating formula for the first time, which greatly improves the stability and physical and chemical properties of the coating in a high solar radiation environment. First, the high melting point and high stability of tungsten make it stable in a high temperature environment, which is crucial for coatings used in a high solar radiation environment. Tungsten can improve the thermal stability of the coating and prevent the attenuation and aging of the coating performance at high temperatures. Secondly, tungsten has good radiation protection capabilities. High-energy solar radiation includes various forms of electromagnetic radiation such as ultraviolet rays, visible light and infrared rays. Tungsten compounds can absorb and block these radiations, especially high-energy ultraviolet rays, to prevent them from causing damage to the coating and the objects it protects. This is of great significance for improving the stability and physical and chemical properties of the coating in a high solar radiation environment. Furthermore, tungsten compounds may form a microstructure in the coating, which helps to form a more uniform radiation protection layer, further improving the protective effect of the coating. At the same time, the addition of tungsten compounds may also improve the mechanical properties of the coating, such as hardness and wear resistance, and further extend the service life of the coating.
[0079] In the following examples:
[0080] Hydroxyethyl cellulose: select DOW HEC CELLOSIZE QP-100.
[0081] Aerogel, nano aerogel powder with a pore size of 20nm (hydrophilic) and item number 06 provided by Dacheng County Arigo New Materials Co., Ltd.
[0082] Glass beads, 3M K20 with specification DZ46mm TM Nano hollow glass microspheres, particle size 65μm.
[0083] Nanosilica, AJ-20 nanosilica provided by Foshan Hongchang New Materials Co., Ltd., particle size 20-50nm, specific surface area 640m 2 / g.
[0084] Nano-alumina, provided by Hubei Huifu Nanomaterials Co., Ltd., gas-phase aluminum oxide with item number ALuna100.
[0085] As the elastic emulsion, Acronal 7588, a styrene acrylic emulsion for coatings produced by BASF, is selected.
[0086] Sodium tungstate, sodium tungstate with item number 002 provided by Suzhou Tianheng Chemical Technology Co., Ltd.
[0087] Calcium tungstate, calcium tungstate powder provided by Zhengzhou Lishengyuan Chemical Products Co., Ltd.
[0088] Barium tungstate, barium tungstate powder provided by Wuhan Kamik Technology Co., Ltd.
[0089] Tungsten carbide, use 0.6-15um tungsten carbide powder of grade FWC08-10 provided by Ganzhou Chuangfeng Tungsten Industry Co., Ltd.
[0090] Example 1
[0091] The preparation method of the highly weather-resistant nano thermal insulation coating comprises the following steps:
[0092] First, 170 parts by weight of deionized water was taken, and the temperature was adjusted to 30° C. and kept constant.
[0093] 5.5 parts by weight of hydroxyethyl cellulose was added to deionized water maintained at a constant temperature, and the mixture was stirred at a speed of 400 rpm using a stirrer until the hydroxyethyl cellulose was dissolved. The stirring time was about 80 minutes.
[0094] 70 parts by weight of aerogel were gradually added to the hydroxyethyl cellulose aqueous solution, and the mixture was stirred again at a speed of 400 rpm for 50 minutes using a stirrer.
[0095] Then, 135 parts by weight of glass microspheres and 140 parts by weight of nano-silicon dioxide were added to the mixed solution, and stirring was continued at a speed of 400 rpm for 50 minutes.
[0096] Next, 20 parts by weight of nano-alumina and 135 parts by weight of elastic emulsion were added, and stirring was continued at a speed of 400 rpm for 50 minutes.
[0097] Finally, 32 parts by weight of sodium tungstate, a tungsten-containing compound, was added, and stirring was continued at a speed of 400 rpm for 50 minutes.
[0098] After stirring, the coating was placed at room temperature for 36 hours to allow all components to fully contact and form a uniform, highly weather-resistant nano-insulating coating.
[0099] The obtained coating is packaged and stored in a cool and dry environment for use.
[0100] Example 2
[0101] The difference between Example 2 and Example 1 is only that the tungsten-containing compound is different.
[0102] The tungsten-containing compound selected in Example 2 is a water-insoluble tungsten-containing compound calcium tungstate powder.
[0103] The added amount of calcium tungstate is 32 parts by weight.
[0104] Example 3
[0105] The difference between Example 3 and Example 1 is only that the tungsten-containing compound is different.
[0106] The tungsten-containing compound selected in Example 3 is a water-insoluble tungsten-containing compound barium tungstate powder.
[0107] The added amount of barium tungstate is 32 parts by weight.
[0108] Example 4
[0109] The difference between Example 4 and Example 1 is only that the tungsten-containing compound is different.
[0110] The tungsten-containing compound selected in Example 4 is a water-insoluble tungsten-containing compound tungsten carbide powder.
[0111] The added amount of tungsten carbide is 32 parts by weight.
[0112] Example 5
[0113] The difference between Example 5 and Example 1 is that the tungsten-containing compound is different. The tungsten-containing compound selected is a mixed powder of water-insoluble tungsten-containing compounds calcium tungstate and barium tungstate. The added amounts of calcium tungstate and barium tungstate are both 16 parts by weight.
[0114] Comparative Example 1
[0115] The preparation method of the highly weather-resistant nano thermal insulation coating comprises the following steps:
[0116] First, 170 parts by weight of deionized water was taken, and the temperature was adjusted to 30° C. and kept constant.
[0117] 5.5 parts by weight of hydroxyethyl cellulose was added to deionized water maintained at a constant temperature, and the mixture was stirred at a speed of 400 rpm using a stirrer until the hydroxyethyl cellulose was dissolved. The stirring time was about 80 minutes.
[0118] 70 parts by weight of aerogel were gradually added to the hydroxyethyl cellulose aqueous solution, and the mixture was stirred again at a speed of 400 rpm for 50 minutes using a stirrer.
[0119] Then, 135 parts by weight of glass microspheres and 140 parts by weight of nano-silicon dioxide were added to the mixed solution, and stirring was continued at a speed of 400 rpm for 50 minutes.
[0120] Next, 20 parts by weight of nano-alumina and 135 parts by weight of elastic emulsion were added, and stirring was continued at a speed of 400 rpm for 50 minutes.
[0121] After stirring, the coating was placed at room temperature for 36 hours to allow all components to fully contact and form a uniform, highly weather-resistant nano-insulating coating.
[0122] The obtained coating is packaged and stored in a cool and dry environment for use.
[0123] Test Example 1:
[0124] The preparation and curing of mortar blocks are carried out in accordance with the provisions of the People's Republic of China Building Materials Industry Standard JC / T1024-2019 "Wall Finishing Mortar". The preparation and curing of the test panels are in accordance with JG / T24-2018 "Synthetic Resin Emulsion Sand Wall Architectural Paint". The test pieces are cured in the laboratory curing room under the conditions of temperature 23°C and humidity 65% for 14 days, and then the tensile bond strength is tested in accordance with JG / T24-2018 "Synthetic Resin Emulsion Sand Wall Architectural Paint". The test pieces are baked at 70°C for 2h (intention: to simulate strong sunlight) to test their tensile bond strength, and the bond strength retention rate is calculated.
[0125] Table 1 Test results of tensile bonding strength of coatings
[0126]
[0127] Test Example 2:
[0128] The thermal conductivity of the coating was tested according to GB / T10294-2008 standard. The thermal conductivity of Example 4 was 0.02 W / (mK); the thermal conductivity of Example 5 was 0.02 W / (mK).
[0129] Example 1 uses water-soluble sodium tungstate, while Examples 2, 3, and 4 use different water-insoluble tungsten-containing compounds: calcium tungstate, barium tungstate, and tungsten carbide. The amount of tungsten-containing compounds added in all examples is the same. The preparation method of Comparative Example 1 is the same as that of Example 1, but no tungsten-containing compound is added. The preparation process of all coatings is basically the same, that is, various raw materials are added successively to constant temperature deionized water, then stirred and allowed to stand, and finally the prepared coatings are packaged and stored.
[0130] After testing the bonding strength of the coatings under a high solar radiation environment, the results showed that Example 4 (coating using tungsten carbide) had the greatest bonding strength, followed by Example 3 (coating using barium tungstate), Example 2 (coating using calcium tungstate) and Example 1 (coating using sodium tungstate), while Comparative Example 1 (coating without the addition of tungsten-containing compounds) had the lowest bonding strength.
[0131] These results show that the addition of tungsten-containing compounds significantly improves the bonding strength of the coating, and different types of tungsten-containing compounds have different effects on the performance of the coating. Among these tungsten-containing compounds, tungsten carbide has the best effect, which can make the coating have greater bonding strength and almost no shrinkage, cracking and falling off problems, while the comparative example 1 without adding tungsten-containing compounds performs very poorly.
[0132] The sodium tungstate used in Example 1 is a water-soluble compound, which means that it can be easily dissolved and dispersed in water. Although this may help improve the initial uniformity of the coating, under high temperature or high radiation environment, the water in the coating may evaporate, resulting in a decrease in the solubility of sodium tungstate, thereby affecting the stability and bonding strength of the coating.
[0133] In contrast, water-insoluble tungsten-containing compounds (calcium tungstate, barium tungstate and tungsten carbide) are used in Examples 2, 3 and 4. These water-insoluble compounds may be difficult to disperse in the coating, but once a uniform coating is formed, they can provide more stable performance, especially in high temperature and high radiation environments. This is because water-insoluble compounds will not undergo significant performance changes due to evaporation of water, thereby maintaining the stability and bonding strength of the coating.
[0134] Therefore, the inventors speculate that the use of a water-insoluble tungsten-containing compound may be one of the reasons why the coatings of Examples 2, 3, and 4 have better bonding strength than that of Example 1.
[0135] In addition, from the perspective of chemical stability, the stability of calcium tungstate, barium tungstate and tungsten carbide increases in turn. Sodium tungstate has low stability and is easily affected by factors such as moisture and oxygen in the environment, while calcium tungstate and barium tungstate have high stability, and tungsten carbide has the highest stability. This difference in chemical stability may lead to certain differences in the performance of the coating under high temperature and high radiation environments. Secondly, from the perspective of thermal stability, tungsten carbide has the highest thermal stability, which may be because tungsten carbide has a tighter structure and poorer heat conductivity, which can better maintain the stability of the coating under high temperature environments. Thirdly, tungsten compounds may form different microstructures in the coating. The particle size, shape and distribution of tungsten carbide, calcium tungstate and barium tungstate may differ, and these differences may affect the uniformity and thermal insulation properties of the coating. For example, tungsten carbide may form smaller and more uniform particles, which will help form a more uniform protective layer, thereby improving the protective effect of the coating. In general, the differences in chemical stability, thermal stability and microstructure of the three tungsten compounds, calcium tungstate, barium tungstate and tungsten carbide, may lead to differences in the performance of the coating, making tungsten carbide the best, followed by barium tungstate and then calcium tungstate.
Claims
1. A highly weather-resistant nano thermal insulation coating, characterized in that: Including the following raw materials: Deionized water 170 parts by weight; 5.5 parts by weight of hydroxyethyl cellulose; the hydroxyethyl cellulose is DOW HEC hydroxyethyl cellulose CELLOSIZEQ P-100; 70 parts by weight of aerogel; the aerogel is a hydrophilic nano-aerogel powder with a pore size of 20 nm and a product number of 06 provided by Dacheng County Aerigo New Materials Co., Ltd.; 135 parts by weight of glass microspheres; the glass microspheres are 3M K20 with a specification of DZ46mm TM Nano hollow glass microspheres, particle size 65μm; 140 parts by weight of nano-silicon dioxide; the nano-silicon dioxide is AJ-20 nano-silicon dioxide provided by Foshan Hongchang New Materials Co., Ltd., with a particle size of 20-50nm and a specific surface area of 640m 2 / g; 20 parts by weight of nano-alumina; the nano-alumina is fumed aluminum oxide with the product number ALuna100 provided by Hubei Huifu Nanomaterials Co., Ltd.; 135 parts by weight of elastic emulsion; the elastic emulsion is Acronal 7588, a styrene acrylic emulsion for coatings produced by BASF; 16 parts by weight of calcium tungstate; the calcium tungstate is calcium tungstate powder provided by Zhengzhou Lishengyuan Chemical Products Co., Ltd.; 16 parts by weight of barium tungstate; the barium tungstate is barium tungstate powder provided by Wuhan Kamik Technology Co., Ltd.