A method for forming a 5m long busbar with a large diameter-to-thickness ratio cone bottom

Through the overall spin forming method, the temperature field and spin parameters are controlled, and the forming accuracy and reliability of the 5m-level long busbar large diameter and thickness ratio cone bottom structure is solved, and a high-precision and high-reliability cone bottom ring manufacturing is realized. Reduces the labor intensity and production costs of workers.

CN117548553BActive Publication Date: 2024-11-15TIANJIN AEROSPACE CHANGZHENG ROCKET MFGCO
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311498019.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-10
Publication Date
2024-11-15
Estimated Expiration
2043-11-10

AI Technical Summary

Technical Problem

When manufacturing a 5m-level long busbar, the forming accuracy is difficult to control, and problems such as distortion and out-synchronization of the upper and lower ends are prone to insufficient product accuracy and reliability, and the overall forming process cost is high, and production is Inefficient.

Method used

The overall spin forming method is adopted, by controlling the temperature field distribution and spinning process parameters, combining preforming and multi-pass spinning design, ensuring the roundness and straightness of the cone bottom ring, reducing the number of welds, and improving product reliability and assembly accuracy.

Benefits of technology

It realizes high-precision forming of the cone-bottom ring, reduces the labor intensity of workers, improves the reliability and consistency of products, and is suitable for recyclable use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117548553B_ABST
    Figure CN117548553B_ABST
Patent Text Reader

Abstract

The present invention provides a method for forming a 5m-long busbar with a large diameter-to-thickness ratio cone bottom, which includes welding and rounding; preforming the product; and controlling the product by spinning. The present invention has the following beneficial effects: by adopting overall spinning forming control, the product has only one weld seam, and the reliability of the cone bottom is greatly improved, laying the foundation for repeatable recycling; the overall spinning profile has a better profile, which is conducive to ensuring the subsequent assembly accuracy; the above processes all use large-scale equipment and process guarantees, which greatly reduces the manual labor intensity of workers and is conducive to ensuring the consistency of products.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of rocket box bottom forming, and in particular relates to a 5m-long busbar large diameter-to-thickness ratio cone bottom forming method. Background Art

[0002] The new launch vehicle inherits the existing rocket box bottom module and adopts a cone bottom structure design to meet the engine space position for easy installation and force transmission effect. At the same time, in order to reduce the cost of the launch vehicle to a greater extent, give full play to the manufacturing advantages and meet the requirements of reusable recycling. The large and small ends of the cone bottom ring need to be connected to the adapter ring in an annular direction, and its forming accuracy directly affects the subsequent assembly accuracy.

[0003] The cone bottom ring is designed to be 2219 aluminum alloy, with a cone angle of 90°, a thickness of 20mm, a large end diameter of Ф5000mm, a small end diameter of about Ф2000mm, and a busbar length of about 2100mm. Therefore, the cone bottom ring has a maximum size of 5 meters, and the upper and lower ends have a large difference in the forming curvature radius. In order to ensure the force transmission effect, the roundness and straightness of the product need to be controlled to 2mm. Considering the deformation of the large cone angle and the control of the deflection of the ultra-long busbar, there are great challenges to the forming consistency. Distortion and asynchronism between the upper and lower ends are very likely to occur during the forming process, which restricts the overall accuracy.

[0004] For the cone bottom structure, the process methods currently used are split welding or integral manufacturing. The split manufacturing methods include roll forming, press bending and creep forming, while the integral forming mainly includes stamping and spinning.

[0005] In the split-flap welding process, its rolling forming is affected by the difference in rolling friction during the actual production process, which makes it difficult to control. The deformation and curvature gap of the formed product are difficult to control, accompanied by a large amount of manual finishing work, making it difficult to apply in engineering and making welding operability poor. The basic principle of press bending forming is to rely on the accumulation of successive deformations to produce overall deformation. Problems such as surface scratches, high internal stress, and inconsistent springback are very likely to occur during the forming process, which restricts product precision and surface quality and affects the subsequent welding assembly accuracy. For creep forming, the overall wall panel needs to be sealed, vacuumed, and pressurized during the forming process. The product has a large deformation amount, and the stress concentration trend of the root fillet is obvious, which is very easy to cause cracks. Different product structures need to match different molds, which is costly, low in production efficiency, and delayed model cycle.

[0006] In the overall forming process, the stamping forming: hydraulic forming is adopted for male and female dies. Due to the large overall size of the cone bottom, the unfolded size needs to reach 6.5m. The current maximum width is only 4.2m. Two sheets are required for welding. The weld is subjected to tensile stress during the forming process, and the risk of cracks is relatively high. At the same time, a large-tonnage hydraulic press and upper and lower dies are required to cooperate, and the overall cost is relatively high. Its spinning forming has high requirements for the control of process parameters. Summary of the invention

[0007] In view of this, the present invention aims to propose a method for forming a 5m-long busbar with a large diameter-to-thickness ratio cone bottom, so as to control the temperature distribution ratio and spinning process parameter setting of the spinning process according to the size characteristics of the 5m-large cone-bottom ultra-long busbar and the high-precision and high-quality overall manufacturing requirements of the product, solve the problem of unstable edge wrapping at the large end during the forming process, and it is difficult to realize the bottleneck process of the full process forming of the spinning long busbar cone, solidify the process and parameters, and improve product quality and reliability.

[0008] To achieve the above object, the technical solution of the present invention is achieved as follows:

[0009] A method for forming a 5m-long busbar with a large diameter-to-thickness ratio cone bottom comprises the following steps:

[0010] S1, welding and rounding, and then proceed to step S2 and step S3;

[0011] S2, pre-forming the product;

[0012] S3, control the spinning of products;

[0013] In step S1, tailor-made welding and rounding include:

[0014] Two rectangular sheets are hoisted onto the welding platform, cleaned before welding to remove the oxide film, and then assembled and electron beam welded in sequence;

[0015] After electron beam welding, the protrusions are ground and the round plate is cut, and the processing size is set to Φ5100mm-5200mm.

[0016] Furthermore, in step S1, the original thickness of the sheet material is set to range from 50 mm to 55 mm.

[0017] Furthermore, in step S2, the product is preformed, including:

[0018] Make the center of the sheet material concentric with the center of the drum die by operating the preforming equipment travel and rotating device;

[0019] Control to 200-300mm away from the edge of the sheet, and apply 2-2.5MPa pressure to the position;

[0020] Press evenly in the circumferential direction. After each circle is completed, feed 200-400mm in the axial direction to press each circle until the same pressure is applied to each circle to cover the board surface.

[0021] Complete preforming.

[0022] Furthermore, the pressing drum mold includes a symmetrically arranged pre-forming male mold and a pre-forming female mold, and the pre-forming male mold and the pre-forming female mold are used for pressing the sheet material.

[0023] Furthermore, the curved surface dimensions of the preforming male mold and the preforming female mold are R1900-2500 mm.

[0024] Furthermore, the preformed product presents a butterfly shape, and the height of the flange is 150-165 mm from the horizontal bottom end surface H.

[0025] Furthermore, in step S3, the product is subjected to spin forming control, including:

[0026] S31, temperature field distribution control;

[0027] S32, setting spinning process parameters and trajectory;

[0028] S33, demoulding.

[0029] Furthermore, in step S31, the temperature field distribution control includes:

[0030] The tail top is pressed by the center positioning hole of the preformed sheet and the pressure of the tail top, sheet and spinning tire;

[0031] The cone bottom ring is heated by 3 spray guns, 2 of which heat the outer surface and 1 heats the mold and inner surface of the preformed sheet;

[0032] The outer surface spray gun is calculated according to the heating volume of the large and small ends. One spray gun is heated along the edge of the tail top of the preformed sheet. The distance between the spray gun and the sheet is always kept at 400-550mm, and the travel path moves along the overall generatrix. The distance between the second spray gun and the sheet is also always kept at 400-550mm. Considering the large volume of the large end, the travel path is from 1 / 2 of the sheet to the edge of the large end of the product.

[0033] The inner surface spray gun is placed at an angle of 65-70° to the sheet material, so that the spinning tire and the inner surface of the sheet material are heated at the same time, and the position is placed at the edge of the large end;

[0034] Temperature detection uses contact thermocouples to monitor the internal and external surface temperatures. After the temperature of the open preformed sheet is stably controlled at 200-230℃, spinning is carried out.

[0035] Furthermore, in step S32, the spinning process parameters and trajectory are set, including:

[0036] The cone bottom ring is used to maximize the enveloping processing allowance, and the product ring and straightness are set. The multi-pass spinning design is adopted, that is, the shear spinning is gradually deviated and the straight end multi-pass ordinary spinning control is adopted, among which,

[0037] Gradual deviation shear spinning: According to the spinning sine law, the theoretical tire-attaching trajectory is set, and the negative deviation pressure at the small end is established as the trajectory translation Δ = (3-3.3) mm = (50-55) × 6%, and the large end deviation rate is Δ = (5-5.5) mm = (50-55) × 10%. The linear relationship is formed by point fitting to form a gradual deviation shear spinning trajectory;

[0038] Straight end multi-pass ordinary spinning: the second pass is connected to the first pass, and is realized by the rounded corner transition at 1 / 2 of the mold. The trajectory arc and the rounded corner tangent mode are adopted. The arc design is R250-300mm, the tangent angle and the mold semi-cone angle are 20-27°, and the feed ratio is set to 12.5mm / rev;

[0039] The third pass is mainly to achieve the rounded corner transition of the other 1 / 2 of the mold. The trajectory arc and the rounded corner tangent mode are adopted. The arc is designed to be R300-350mm, the tangent angle and the mold semi-cone angle are 32-38°, and the feed ratio is set to 12.5mm / rev;

[0040] The fourth pass is mainly for the straight end area of ​​the mold, which is 45° to the semi-cone angle of the mold and is formed by progressive passes.

[0041] Compared with the prior art, the method for forming a 5m long busbar with a large diameter-to-thickness ratio cone bottom according to the present invention has the following advantages:

[0042] The present invention discloses a method for forming a 5m-long busbar with a large diameter-to-thickness ratio cone bottom, which adopts overall spinning forming control. The product has only one weld seam, and the reliability of the cone bottom is greatly improved, laying a foundation for repeatable recycling. The overall spinning profile has a better contour, which is beneficial to ensuring the subsequent assembly accuracy. The above processes all use large-scale equipment and process guarantees, which greatly reduces the manual labor intensity of workers and is beneficial to ensuring the consistency of products. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] The accompanying drawings constituting a part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the accompanying drawings:

[0044] Figure 1 A schematic diagram of the preforming process and morphology according to an embodiment of the present invention;

[0045] Figure 2 This is a schematic diagram of heating the product and mold before spinning according to an embodiment of the present invention;

[0046] Figure 3 A schematic diagram of the trajectory setting of the cone-bottom circular ring spinning according to an embodiment of the present invention;

[0047] Figure 4It is a schematic diagram of the processing process described in an embodiment of the present invention.

[0048] Description of reference numerals:

[0049] 1. Sheet material; 2. Pre-forming male mold; 3. Pre-forming female mold; 4. Spinning tire; 5. Tail top; 6. Spray gun; 7. Spinning wheel. DETAILED DESCRIPTION

[0050] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments may be combined with each other.

[0051] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", and the like are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, features defined as "first", "second", and the like may explicitly or implicitly include one or more of the features. In the description of the present invention, unless otherwise specified, "multiple" means two or more.

[0052] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood by specific circumstances.

[0053] The present invention will be described in detail below with reference to the accompanying drawings and in conjunction with embodiments.

[0054] like Figures 1 to 4 As shown, a method for forming a 5m-long busbar with a large diameter-to-thickness ratio cone bottom comprises the following steps:

[0055] S1, welding and rounding, and then proceed to step S2 and step S3;

[0056] S2, pre-forming the product;

[0057] S3. Control the spinning of the product.

[0058] In a preferred embodiment of the present invention, according to the product structure and material characteristics, the cone bottom ring is a typical rotating body part, and it is suitable to be processed by the integral spinning process. Considering the characteristics of the sine law of equal cone angle thinning, subsequent heat treatment and machining deformation, the part semi-cone angle is 45°, and the thinning rate after one deformation is 30%. According to the calculation based on the unchanged volume, the sheet diameter is about Φ4800mm, the original sheet thickness is selected to be 50-55mm, and the sheet diameter is determined to be Φ5000mm. It is necessary to weld two rectangular sheets, and the size of a single sheet is 5000mm long × 2500mm wide × (50-55)mm thick.

[0059] In a preferred embodiment of the present invention, the tailor-made welding and rounding process comprises:

[0060] The two large flat plates are hoisted onto the welding platform, cleaned before welding to remove the oxide film, assembled in time, and electron beam welded. After welding, the protrusions are polished and the round plates are cut to a size of Φ5100-5200mm.

[0061] In a preferred embodiment of the present invention, the preforming comprises:

[0062] The weld leak surface with higher elongation is placed on the outer surface of the pre-forming drum, and the outer edge circle is pre-formed using a R1900-2500mm drum die to increase the rigidity constraint of the original slab and offset the unstable hemming during the spinning process.

[0063] First, the center of the sheet is concentric with the center of the drum die, and the pre-forming equipment is operated to move and rotate the device to control the distance to 200-300mm from the edge of the sheet, and apply 2-2.5MPa pressure to the position. After the initial development, the deformation is observed to produce obvious plastic deformation, and the circumferential pressure is uniformly pressed. After each circle is completed, the axial feed is 200-400mm for each circle of pressing until the same pressure is applied to each circle to cover the sheet surface.

[0064] After preforming, the product presents a butterfly shape, and the height of the flange is 150-165mm from the horizontal bottom end surface H.

[0065] The pressing drum die comprises a symmetrically arranged pre-forming male die 2 and a pre-forming female die 3 , and the pre-forming male die 2 and the pre-forming female die 3 are used for pressing the sheet material 1 .

[0066] In a preferred embodiment of the present invention, the spin forming control comprises:

[0067] (1) Temperature field distribution control

[0068] The product has a large size and needs to be spun in an open environment. During the process, the sheet is prone to uneven temperature loss. At the same time, because it is far away from the spinning tire 4, the temperature difference during tire attachment has a great impact on the stability of forming control.

[0069] The tail top 5, the sheet 1 and the spinning tire 4 are pressed by the central positioning hole of the preformed sheet and the pressure, ensuring that the sheet 1 does not move abnormally when the spinning tire 4 rotates with the main shaft.

[0070] The cone bottom ring is heated by three spray guns 6, two of which heat the outer surface and one heats the mold and the inner surface of the preformed sheet.

[0071] The outer surface spray gun 6 is calculated according to the heating volume of the large and small ends. One spray gun heats along the edge of the tail top 3 of the preformed sheet. The distance between the spray gun 6 and the sheet 1 is always maintained at 400-550mm, and the travel path moves along the overall busbar (the spinning wheel 7 feeds radially and axially relative to the core mold busbar); the second spray gun 6 is also always maintained at a distance of 400-550mm from the sheet. Considering the large volume of the large end, the travel path is from 1 / 2 of the sheet to the edge of the large end of the product.

[0072] The inner surface spray gun 6 is at an angle of 65-70° to the sheet material 1 so that the spinning tire 4 and the inner surface of the sheet material 1 are heated at the same time, and is located at the edge of the large end.

[0073] The temperature detection adopts contact temperature measuring thermocouple to monitor the temperature of the inner and outer surfaces. After the temperature of the open preformed sheet 1 is stably controlled at 200-230°C, spinning is carried out.

[0074] (2) Spinning process parameters and trajectory setting

[0075] The cone bottom ring adopts the product ring + straightness setting to maximize the enveloping processing allowance, and adopts a multi-pass spinning design, that is, super-long busbar shear spinning + multi-pass ordinary spinning control at the straight end.

[0076] Gradual deviation shear spinning: According to the sine law of spinning, the theoretical tire-sticking trajectory is set. Taking into account the yield and rebound of the equipment, the negative deviation pressure at the small end is established as the trajectory translation Δ=(3-3.3)mm=(50-55)×6%, and the large end deviation rate is Δ=(5-5.5)mm=(50-55)×10%. Through point fitting into a linear relationship, a gradually deviated shear spinning trajectory is formed.

[0077] Multi-pass ordinary spinning of the straight end: During the straightness spinning process, it is subjected to a large deformation amount, and it is necessary to perform multi-pass small deformation trajectories. Three passes are used to achieve straightness deformation control, that is, the second pass is connected to the first pass, and it is mainly realized for the transition of the fillet at 1 / 2 of the mold, that is, the trajectory arc and the fillet tangent mode are adopted, the arc is designed to be R250-300mm, the tangent angle is 20-27° with the mold semi-cone angle, and the feed ratio is set to 12.5mm / rev; the third pass is mainly realized for the transition of the fillet at the other 1 / 2 of the mold, that is, the trajectory arc and the fillet tangent mode are adopted, the arc is designed to be R300-350mm, the tangent angle is 32-38° with the mold semi-cone angle, and the feed ratio is set to 12.5mm / rev; the fourth pass is mainly for the straight end area of ​​the mold, which is 45° with the mold semi-cone angle, and is formed by progressive passes.

[0078] (3) Demolding

[0079] Due to the heat shrinkage during the spinning process, the product will stick to the mold after cooling. After the whole product is cooled and shrunk, only the straight line segment is heated and demolded.

[0080] Example 1

[0081] The specific processing process of the present invention is as follows Figure 4 As shown, the following steps are included:

[0082] A1, cutting;

[0083] A2, welding;

[0084] A3. Weld inspection;

[0085] A4, annealing;

[0086] A5, lower circle;

[0087] A6, Spinning;

[0088] A7. Heat treatment;

[0089] A8, turning the inner and outer shapes;

[0090] A9, grid milling;

[0091] A10, detection;

[0092] A11. Delivery.

[0093] Advantages of the present invention:

[0094] By adopting overall spinning forming control, the product has only one weld, and the reliability of the cone bottom is greatly improved, laying the foundation for repeatable recycling; the overall spinning surface contour is better, which is conducive to ensuring the subsequent assembly accuracy; the above processes all use large-scale equipment and process guarantees, which greatly reduces the manual labor intensity of workers and is conducive to ensuring product consistency.

[0095] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for forming a 5m long busbar with a large diameter-to-thickness ratio cone bottom. Features: The following steps are involved: S1, welding and rounding; S2, pre-forming the product; S3, control the spinning of products; In step S1, tailor-made welding and rounding include: Two rectangular plates (1) are hoisted onto a welding platform, cleaned before welding to remove the oxide film, and then assembled and electron beam welded in sequence; After electron beam welding, the protrusions are polished and the round plate is cut. The processing size is set to Φ5100mm-5200mm; In step S2, the product is preformed, including: The center of the sheet material (1) is concentric with the center of the drum die, wherein the drum die comprises a symmetrically arranged pre-forming male die (2) and a pre-forming female die (3), wherein the pre-forming male die (2) and the pre-forming female die (3) are used to press the sheet material (1); The curved surface dimensions of the preforming male mold (2) and the preforming female mold (3) are R1900-2500 mm; Using a drum die to press the position 200-300 mm away from the edge of the sheet material (1) at a pressure of 2-2.5 MPa; Press uniformly in the circumferential direction, and after each circle is completed, feed 200-400 mm in the axial direction to press each circle until the preformed sheet (1) presents a butterfly shape, and the height of the flange is 150-165 mm from the horizontal bottom end surface H; Complete preforming; In step S3, the product is subjected to spin forming control, including: S31, temperature field distribution control; S32, setting spinning process parameters and trajectory; S33, demoulding; In step S31, the temperature field distribution control includes: The tail top (5) is pressed by the center positioning hole of the preformed sheet (1) and the pressure, and the tail top (5), the preformed sheet (1) and the spinning tire (4) are ensured that when the spinning tire (4) rotates with the main shaft, the preformed sheet (1) does not move abnormally; The cone bottom ring is heated by three spray guns (6), two of which are used to heat the outer surface of the preformed sheet material (1), and one is used to heat the inner surface of the preformed sheet material (1) by spinning the tire (4) and the inner surface; 1. The outer surface spray gun (6) is used to heat the edge of the tail top of the preformed sheet (1). The distance between the outer surface spray gun (6) and the preformed sheet (1) is always maintained at 400-550 mm, and the travel path is along the overall generatrix; the distance between the second outer surface spray gun (6) and the preformed sheet (1) is also always maintained at 400-550 mm. Considering the large volume of the large end, the travel path is from 1 / 2 of the preformed sheet (1) to the large end edge of the preformed sheet (1); The inner surface spray gun (6) is at an angle of 65-70° to the preformed sheet (1), so that the spinning tire (4) and the inner surface of the preformed sheet (1) are heated at the same time, and the inner surface spray gun (6) is placed at the edge of the large end; The temperature detection uses a contact thermocouple to monitor the internal and external surface temperatures. After the temperature of the preformed sheet (1) is stably controlled at 200-230°C, spinning is performed; In step S32, the spinning process parameters and trajectory are set, including: In order to maximize the envelopment of the machining allowance, the cone bottom ring adopts the product ring and straightness setting, and adopts a multi-pass spinning design, that is, gradually deviating from the shear spinning and the straight end multi-pass ordinary spinning control, among which, Gradual deviation shear spinning: According to the spinning sine law, it is set as the theoretical tire-attaching trajectory, and the negative deviation pressure reduction at the small end is established as the trajectory translation Δ=(3-3.3)mm=(50-55)mm×6%, and the negative deviation pressure reduction at the large end is Δ=(5-5.5)mm=(50-55)mm×10%. Through point fitting into a linear relationship, a gradual deviation shear spinning trajectory is formed; Straight end multi-pass ordinary spinning: the second pass is the gradual deviation shear spinning connection of the first pass, mainly for the rounded corner transition at 1 / 2 of the spinning tire (4), using the trajectory arc and rounded corner tangent mode, the arc design is R250-300mm, the tangent angle and the semi-cone angle of the spinning tire (4) are 20-27°, and the feed ratio is set to 12.5mm / rev; The third pass is mainly to realize the transition of the other 1 / 2 of the rounded corner of the spinning tire (4), using the trajectory arc and the rounded corner tangent mode, the arc design is R300-350mm, the tangent angle and the semi-cone angle of the spinning tire (4) are 32-38°, and the feed ratio is set to 12.5mm / rev; The fourth pass is mainly for the straight end area of ​​the spinning tire (4), which is 45 degrees with the semi-cone angle of the spinning tire (4) and is formed by progressive passes.

2. According to claim 1, a 5m long busbar large diameter-thickness ratio cone bottom forming method, Features: In step S1, the original thickness of the sheet material (1) is set to range from 50 mm to 55 mm.