1.60 plus multifunctional polarized driving mirror and method of making same

Multifunctional polarized lenses, manufactured using specific formulas and processing techniques, solve the problems of transmittance and protection under different lighting conditions, achieving a combination of multifunctionality and fashion.

CN117551256BActive Publication Date: 2026-11-10JIANGSU CONANT OPTICS CO LTD +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202311484301.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-08
Publication Date
2026-11-10
Estimated Expiration
2043-11-08

AI Technical Summary

Technical Problem

Existing polarized driving glasses have limited functionality, especially when light conditions change, resulting in poor transmittance and protection, which poses safety hazards, and they also lack style.

Method used

By combining a specific formulation of resin monomers and additives with a polarizing film, and through a sandwich structure lens design and specialized processing technology, multifunctional lenses that block blue light, prevent glare, and polarize are produced, and their fashionability is enhanced by dyeing.

Benefits of technology

It achieves the desired transmittance and protection under different lighting conditions, enhancing safety while also being stylish enough for various occasions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117551256B_ABST
    Figure CN117551256B_ABST
Patent Text Reader

Abstract

The application provides a 1.60PLUS multifunctional polarized driving mirror and a preparation method thereof, which comprises a lens base and a polarized film; the lens base is prepared from the following raw materials in parts by weight: 100 parts of resin monomer, 0.03-0.06 parts of initiator, 0.01-0.03 parts of ultraviolet light absorber and 0.02-0.05 parts of yellow light absorber; wherein the resin monomer is a mixture of 2,5(or 2,6)-bis(isocyanate methyl)bicyclo[2.2.1]heptane, hexamethylene diisocyanate, tetra(3-mercaptopropionic acid)pentaerythritol ester and 4-mercaptomethyl-3,6-dithia-1,8-octanedithiol, and the mass ratio is (25-34):(16-24):(24-32):(18-27). The application can simultaneously meet the requirements of night driving for lens transmittance and anti-dazzling and the needs of daytime driving for protection against direct sunlight and dazzling light such as water surface reflection.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of resin lenses, and more specifically, relates to a 1.60PLUS multi-functional polarized driving mirror and its preparation method. Background Technology

[0002] Currently available polarized driving glasses on the market are mostly dark-colored and have limited functionality. However, with the improvement of people's living standards and the pursuit of fashion, resin lenses have been given more meaning beyond their single function or single use case. For example, their functions have become more diverse, from simply adjusting vision to meeting different needs, such as blue light protection, anti-glare, tinting, and photochromic effects. At the same time, the use cases for resin lenses have also expanded from single to multiple. For example, polarized driving glasses, due to their dark polarized base color, are generally only suitable for wearing in very strong sunlight or when direct sunlight is glaring. In relatively dark places or when driving at night, polarized glasses become a burden, as their low light transmittance leads to unclear vision and may even pose safety hazards. Summary of the Invention

[0003] The purpose of this invention is to address the above-mentioned shortcomings by providing a 1.60PLUS multi-functional polarized driving mirror and its manufacturing method, which can achieve multiple functions such as blue light protection, anti-glare, and polarization. It can not only meet the requirements of lens transmittance and anti-glare for night driving, but also meet the needs of daytime driving for protection against direct sunlight and glare from water reflection.

[0004] To achieve the above objectives, the present invention is implemented through the following technical solution:

[0005] This invention provides a 1.60PLUS multi-functional polarized driving mirror, comprising a lens substrate and a polarizing film;

[0006] The lens substrate is prepared from the following raw materials in parts by weight: 100 parts resin monomer, 0.03-0.06 parts initiator, 0.01-0.03 parts ultraviolet absorber, and 0.02-0.05 parts yellow light absorber; wherein the resin monomer is a mixture of 2,5 (or 2,6)-bis(isocyanate methyl)bicyclo[2.2.1]heptane, hexamethylene diisocyanate, pentaerythritol tetrakis(3-mercaptopropionic acid) and 4-mercaptomethyl-3,6-dithia-1,8-octanedithiol, in a mass ratio of (25-34):(16-24):(24-32):(18-27), preferably 30:20:27:23.

[0007] Preferably, the initiator is one or more of dimethyl carbonate, diethyl carbonate, and dimethyl tin dichloride.

[0008] Preferably, the ultraviolet absorber is one or more of 2-(2H-benzotriazole-2-yl)-6-(1-methyl-1-phenylethyl)-4-(1,1,3,3-tetramethylbutyl)phenol, 2'-(2'-hydroxy-3'-tert-butyl-5'-methylphenyl)-5-chlorobenzotriazole, and 2-(2'-hydroxy-5'-tert-octylphenyl)benzotriazole.

[0009] Preferably, the yellow light absorber can be one of ketophylline blue or anthocyanin dye.

[0010] Preferably, the polarizing film and the lens substrate form a sandwich structure of lens substrate-polarizing film-lens substrate.

[0011] Preferably, the polarizing film is a PVA film.

[0012] This invention also provides a method for manufacturing the aforementioned 1.60PLUS multi-functional polarized driving mirror, comprising:

[0013] Prepare polarizing films with the required curvature and dimensions;

[0014] The polarizing film is placed in the middle of the glass mold for casting the lens substrate, and the mold is closed.

[0015] The resin monomer, ultraviolet absorber, yellow light absorber and initiator are mixed evenly to prepare a casting refractory;

[0016] The casting material is poured into a glass mold with a polarizing film and then sealed.

[0017] Curing and shaping.

[0018] Preferably, the method for preparing the polarizing film with the required curvature and size is as follows:

[0019] After the polarizing film is softened, it is pressed into the required curvature by a film press and then placed in a film warehouse to set naturally. Finally, the polarizing film is cut to the required size by a film cutting machine.

[0020] Preferably, the curvature of the upper bending mold of the glass mold is consistent with the curvature of the polarizing film.

[0021] Preferably, the curing curve of the curing molding is as follows: set the initial temperature to 10-12℃, hold for 8-10 hours; raise the temperature to 35℃ in 3-4 hours; raise the temperature to 45℃ in 3-4 hours and hold for 5-6 hours; raise the temperature to 80℃ in 3-4 hours; raise the temperature to 110℃ in 10-12 hours; raise the temperature to 120℃ in 3-4 hours and hold; after 2-3 hours, cool down to 80℃ in 1 hour.

[0022] Preferably, the preparation method further includes: dyeing the cured lens in a dyeing tank at 90°C for 30 minutes, then fixing the color at 120°C for 3 hours, and then applying a hardening coating.

[0023] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0024] This invention utilizes a special resin monomer and additive formulation to enable the polarized driving glasses to achieve multiple functions such as blue light protection, anti-glare, and polarization.

[0025] By combining specific processing techniques, the resulting lenses can not only meet the requirements of lens transmittance and anti-glare for night driving, but also meet the requirements of daytime driving for protection against direct sunlight and glare from water reflections.

[0026] This invention can also enhance the fashionability of the glasses by dyeing and adding color-changing film layers, so that one pair of glasses can be used in multiple occasions. Attached Figure Description

[0027] Figure 1 This is a schematic diagram of the lens structure of the 1.60PLUS multi-functional polarized driving mirror described in this invention;

[0028] In the diagram: 1-Upper lens substrate layer; 2-Polarizing film layer; 3-Lower lens substrate layer. Detailed Implementation

[0029] Preferred embodiments of the present invention will now be described in more detail with reference to specific examples.

[0030] Example 1

[0031] This embodiment provides a 1.60PLUS multi-functional polarized driving mirror, in which the polarizing film and the lens substrate form a sandwich structure of lens substrate-polarizing film-lens substrate, as shown below. Figure 1 As shown, from top to bottom, it includes an upper lens substrate layer 1, a polarizing film layer 2, and a lower lens substrate layer 3.

[0032] The lens substrate is prepared from the following raw materials:

[0033] The resin monomers are: 2,5 (or 2,6)-bis(isocyanate-methyl)bicyclo[2.2.1]heptane 150g, hexamethylene diisocyanate 100g, pentaerythritol tetrakis(3-mercaptopropionic acid) ester 135g, 4-mercaptomethyl-3,6-dithia-1,8-octanedithiol 115g, initiator dimethyltin dichloride 0.15g, ultraviolet absorber 2'-(2'-hydroxy-3'-tert-butyl-5'-methylphenyl)-5-chlorobenzotriazole 0.1g, and yellow light absorber ketone phthalocyanine blue 0.15g.

[0034] The method for preparing the polarized driving mirror lens includes the following steps:

[0035] (1) After softening the PVA polarizing film, press it into 400W using a film presser and place it in the film warehouse to set naturally. Then cut the PVA polarizing film to size using a film cutting machine.

[0036] (2) Perform polarization mold assembly. The curvature of the upper bending mold used for mold assembly is also 400W. The polarization film is assembled between the two glass molds.

[0037] (3) Ingredients: Mix the above resin monomers with ultraviolet absorber, yellow light absorber and initiator evenly;

[0038] (4) Casting: The material mixed evenly in step (3) is injected into the glass mold through a 1μm filter and sealed with tape;

[0039] (5) One-time curing: Set the initial temperature to 10-12℃ and keep it at that temperature for 8-10 hours; raise the temperature to 35℃ in 3-4 hours; raise the temperature to 45℃ in 3-4 hours and keep it at that temperature for 5-6 hours; raise the temperature to 80℃ in 3-4 hours; raise the temperature to 110℃ in 10-12 hours; raise the temperature to 120℃ in 3-4 hours and keep it at that temperature; after 2-3 hours, lower the temperature to 80℃ in 1 hour.

[0040] (6) Mold opening, edge machining, and cleaning;

[0041] (7) Dye the product in a dyeing bath at 90°C for 30 minutes, and then harden it by fixing the color at 120°C for 3 hours.

[0042] Example 2

[0043] This embodiment provides a 1.60PLUS multi-functional polarized driving mirror, the structure of which is the same as in Embodiment 1.

[0044] Its lens substrate is made from the following raw materials:

[0045] Resin monomers: 2,5 (or 2,6)-bis(isocyanate-methyl)bicyclo[2.2.1]heptane 125g, hexamethylene diisocyanate 120g, pentaerythritol tetrakis(3-mercaptopropionic acid) ester 120g, 4-mercaptomethyl-3,6-dithia-1,8-octanedithiol 135g, initiator: dimethyl carbonate 0.2g, ultraviolet absorber: 2-(2'-hydroxy-5'-tert-octylphenyl)benzotriazole 0.12g, yellow light absorber: cyanine dye 0.18g.

[0046] The method for preparing the polarized driving mirror lens includes the following steps:

[0047] (1) After softening the PVA polarizing film, press it into 600W using a film presser and place it in the film warehouse to set naturally. Then cut the PVA polarizing film to size using a film cutting machine.

[0048] (2) Perform polarization mold assembly. The curvature of the upper bending mold used for mold assembly is also 600W. The polarization film is assembled between the two glass molds.

[0049] (3) Ingredients: Mix the above resin monomers with ultraviolet absorber, yellow light absorber and initiator evenly;

[0050] (4) Casting: The material mixed evenly in step (3) is injected into the glass mold through a 1μm filter and sealed with tape;

[0051] (5) One-time curing: Set the initial temperature to 10-12℃ and keep it at that temperature for 8-10 hours; raise the temperature to 35℃ in 3-4 hours; raise the temperature to 45℃ in 3-4 hours and keep it at that temperature for 5-6 hours; raise the temperature to 80℃ in 3-4 hours; raise the temperature to 110℃ in 10-12 hours; raise the temperature to 120℃ in 3-4 hours and keep it at that temperature; after 2-3 hours, lower the temperature to 80℃ in 1 hour.

[0052] (6) Mold opening, edge machining, and cleaning;

[0053] (7) Dye the product in a dyeing bath at 90°C for 30 minutes, and then harden it by fixing the color at 120°C for 3 hours.

[0054] Example 3

[0055] This embodiment provides a 1.60PLUS multi-functional polarized driving mirror, the structure of which is the same as in Embodiment 1.

[0056] Its lens substrate is made from the following raw materials:

[0057] Resin monomers: 2,5 (or 2,6)-bis(isocyanate-methyl)bicyclo[2.2.1]heptane 170g, hexamethylene diisocyanate 80g, pentaerythritol tetrakis(3-mercaptopropionic acid) 160g, 4-mercaptomethyl-3,6-dithia-1,8-octanedithiol 90g, initiator diethyl carbonate 0.28g, ultraviolet absorber 2-(2H-benzotriazol-2-yl)-6-(1-methyl-1-phenylethyl)-4-(1,1,3,3-tetramethylbutyl)phenol 0.15g, yellow light absorber ketone phthalocyanine blue 0.23g.

[0058] The method for preparing the polarized driving mirror lens includes the following steps:

[0059] (1) After softening the PVA polarizing film, press it into 800W using a film presser and place it in the film warehouse to set naturally. Then cut the PVA polarizing film to size using a film cutting machine.

[0060] (2) Perform polarization mold assembly. The curvature of the upper bending mold used for mold assembly is also 800W. The polarization film is assembled between the two glass molds.

[0061] (3) Ingredients: Mix the above resin monomers with ultraviolet absorber, yellow light absorber and initiator evenly;

[0062] (4) Casting: The material mixed evenly in step (3) is injected into the glass mold through a 1μm filter and sealed with tape;

[0063] (5) One-time curing: Set the initial temperature to 10-12℃ and keep it at that temperature for 8-10 hours; raise the temperature to 35℃ in 3-4 hours; raise the temperature to 45℃ in 3-4 hours and keep it at that temperature for 5-6 hours; raise the temperature to 80℃ in 3-4 hours; raise the temperature to 110℃ in 10-12 hours; raise the temperature to 120℃ in 3-4 hours and keep it at that temperature; after 2-3 hours, lower the temperature to 80℃ in 1 hour.

[0064] (6) Mold opening, edge machining, and cleaning;

[0065] (7) Dye the product in a dyeing bath at 90°C for 30 minutes, and then harden it by fixing the color at 120°C for 3 hours.

[0066] Comparative Example 1

[0067] A 1.60PLUS polarized driving mirror, the lens matrix raw materials include: 100g of resin monomer 2,5 (or 2,6)-bis(isocyanate-methyl)bicyclo[2.2.1]heptane, 150g of hexamethylene diisocyanate, 90g of pentaerythritol tetrakis(3-mercaptopropionic acid) ester, 160g of 4-mercaptomethyl-3,6-dithia-1,8-octanedithiol, and 0.1g of initiator dimethyltin dichloride. The preparation method is the same as in Example 1.

[0068] Comparative Example 2

[0069] A resin lens, comprising the following raw materials: 200g of resin monomer 2,5 (or 2,6)-bis(isocyanate-methyl)bicyclo[2.2.1]heptane, 50g of hexamethylene diisocyanate, 175g of pentaerythritol tetrakis(3-mercaptopropionic acid), 75g of 4-mercaptomethyl-3,6-dithia-1,8-octanedithiol, 0.4g of initiator dimethyltin dichloride, 0.3g of ultraviolet absorber 2-(2H-benzotriazol-2-yl)-6-(1-methyl-1-phenylethyl)-4-(1,1,3,3-tetramethylbutyl)phenol, and 0.5g of yellow light absorber ketone phthalocyanine blue.

[0070] The preparation method includes the following steps:

[0071] (1) Ingredients: Mix the resin monomer with the ultraviolet absorber, yellow light absorber and initiator evenly;

[0072] (2) Casting: The material mixed evenly in step (1) is injected into the glass mold through a 1μm filter and sealed with tape;

[0073] (3) One-time curing: Set the initial temperature to 10-12℃ and keep it at that temperature for 8-10 hours; raise the temperature to 35℃ in 3-4 hours; raise the temperature to 45℃ in 3-4 hours and keep it at that temperature for 5-6 hours; raise the temperature to 80℃ in 3-4 hours; raise the temperature to 110℃ in 10-12 hours; raise the temperature to 120℃ in 3-4 hours and keep it at that temperature; after 2-3 hours, lower the temperature to 80℃ in 1 hour.

[0074] (4) Mold opening, edge machining, and cleaning;

[0075] (5) Dye the product in a dyeing bath at 90°C for 30 minutes, and then harden it by fixing the color at 120°C for 3 hours.

[0076] Comparative Example 3

[0077] A resin lens, comprising the following raw materials: 110g of resin monomer 2,5 (or 2,6)-bis(isocyanate-methyl)bicyclo[2.2.1]heptane, 135g of hexamethylene diisocyanate, 100g of pentaerythritol tetrakis(3-mercaptopropionic acid), 155g of 4-mercaptomethyl-3,6-dithia-1,8-octanedithiol, 0.4g of initiator dimethyl carbonate, and 0.3g of ultraviolet absorber 2'-(2'-hydroxy-3'-tert-butyl-5'-methylphenyl)-5-chlorobenzotriazole. The preparation method includes the following steps:

[0078] (1) After softening the PVA polarizing film, press it into 600W using a film presser and place it in the film warehouse to set naturally. Then cut the PVA polarizing film to size using a film cutting machine.

[0079] (2) Perform polarization mold assembly. The curvature of the upper bending mold used for mold assembly is also 600W. The polarization film is assembled between the two glass molds.

[0080] (3) Ingredients: Mix the resin monomer with the ultraviolet absorber and initiator evenly;

[0081] (4) Casting: The material mixed evenly in step (3) is injected into the glass mold through a 1μm filter and sealed with tape;

[0082] (5) One-time curing: Set the initial temperature to 10-12℃ and keep it at that temperature for 8-10 hours; raise the temperature to 35℃ in 3-4 hours; raise the temperature to 45℃ in 3-4 hours and keep it at that temperature for 5-6 hours; raise the temperature to 80℃ in 3-4 hours; raise the temperature to 110℃ in 10-12 hours; raise the temperature to 120℃ in 3-4 hours and keep it at that temperature; after 2-3 hours, lower the temperature to 80℃ in 1 hour.

[0083] (6) Mold opening, edge machining, and cleaning;

[0084] (7) Dye the product in a dyeing bath at 90°C for 30 minutes, and then harden it by fixing the color at 120°C for 3 hours.

[0085] Comparative Example 4

[0086] PC polarized lenses available on the market.

[0087] Comparative Example 5

[0088] MR-8 polarized lenses made from Mitsui MR-8 material are available on the market.

[0089] The performance of the lenses prepared in the above embodiments and comparative examples is shown in Table 1.

[0090] Table 1 Comparison of lens performance between the examples and the comparative examples

[0091]

[0092] Note: TM-8S instrument for testing blue light protection performance, anti-glare performance, and visible light transmittance; optical transmittance meter for testing dyeing depth.

[0093] As shown in the table above, the lenses prepared by the method described in this invention have excellent functionality and maintain a high level of visible light transmittance, meeting the requirements for night driving glasses. The lens pass rate is stable at a high level, and the lenses prepared by this invention also have good staining properties.

[0094] The various embodiments of the present invention have been described above. These descriptions are exemplary and not exhaustive, nor are they limited to the disclosed embodiments. Many modifications and variations will be apparent to those skilled in the art without departing from the scope and principles of the described embodiments, and these modifications and variations should also be considered within the scope of protection of the present invention.

Claims

1. A 1.60PLUS multi-functional polarized driving mirror, characterized in that, Including the lens substrate and polarizing film; The lens substrate is prepared from the following raw materials in parts by weight: 100 parts resin monomer, 0.03-0.06 parts initiator, 0.01-0.03 parts ultraviolet absorber, and 0.02-0.05 parts yellow light absorber; wherein the resin monomer is a mixture of 2,5-bis(isocyanate methyl)bicyclo[2.2.1]heptane or 2,6-bis(isocyanate methyl)bicyclo[2.2.1]heptane, hexamethylene diisocyanate, pentaerythritol tetrakis(3-mercaptopropionic acid) and 4-mercaptomethyl-3,6-dithia-1,8-octanedithiol, in a mass ratio of (25-34):(16-24):(24-32):(18-27); The yellow light absorber is one of ketophyll blue or anthocyanin dye; The polarizing film and the lens substrate form a sandwich structure of lens substrate-polarizing film-lens substrate.

2. The 1.60PLUS multi-functional polarized driving mirror according to claim 1, characterized in that, The initiator is one or more of dimethyl carbonate, diethyl carbonate, and dimethyl tin dichloride.

3. The 1.60PLUS multi-functional polarized driving mirror according to claim 1, characterized in that, The ultraviolet absorber is one or more of 2-(2H-benzotriazole-2-yl)-6-(1-methyl-1-phenylethyl)-4-(1,1,3,3-tetramethylbutyl)phenol, 2'-(2'-hydroxy-3'-tert-butyl-5'-methylphenyl)-5-chlorobenzotriazole, and 2-(2'-hydroxy-5'-tert-octylphenyl)benzotriazole.

4. The 1.60PLUS multi-functional polarized driving mirror according to claim 1, characterized in that, The polarizing film is a PVA film.

5. A method for manufacturing the 1.60PLUS multi-functional polarized driving mirror according to any one of claims 1-4, characterized in that, include: Prepare polarizing films with the required curvature and dimensions; The polarizing film is placed in the middle of the glass mold for casting the lens substrate, and the mold is closed. The resin monomer, ultraviolet absorber, yellow light absorber and initiator are mixed evenly to prepare a casting refractory; The casting material is poured into a glass mold with a polarizing film and then sealed. Curing and shaping.

6. The method for manufacturing the 1.60PLUS multi-functional polarized driving mirror according to claim 5, characterized in that, The method for preparing the polarizing film with the required curvature and size is as follows: After the polarizing film is softened, it is pressed into the required curvature by a film press and then placed in a film warehouse to set naturally. Finally, the polarizing film is cut to the required size by a film cutting machine.

7. The method for manufacturing the 1.60PLUS multi-functional polarized driving mirror according to claim 5, characterized in that, The curvature of the upper bending mold of the glass mold is consistent with the curvature of the polarizing film.

8. The method for manufacturing the 1.60PLUS multi-functional polarized driving mirror according to claim 5, characterized in that, The curing curve for the curing process is as follows: set the initial temperature to 10-12℃, hold for 8-10 hours; raise the temperature to 35℃ in 3-4 hours; raise the temperature to 45℃ in 3-4 hours and hold for 5-6 hours; raise the temperature to 80℃ in 3-4 hours; raise the temperature to 110℃ in 10-12 hours; raise the temperature to 120℃ in 3-4 hours and hold; after 2-3 hours, cool down to 80℃ in 1 hour.

9. The method for manufacturing the 1.60PLUS multi-functional polarized driving mirror according to claim 5, characterized in that, The preparation method further includes: dyeing the cured lens in a dyeing tank at 90°C for 30 minutes, then fixing the color at 120°C for 3 hours, and then applying a hardening coating.

Citation Information

Patent Citations

  • High-binding-force and anti-impact resin lens composition, and preparation method of polarizing lens

    CN107501499A

  • Composite polyester lens and preparation method thereof

    CN107828041A

  • Dyeable 1.74 resin lens and preparation method thereof

    CN113109894A