A thioctic acid-based bioadhesive and its preparation and application
By preparing a thioctic acid-based bioadhesive, combining thioctic acid and aminothioctic acid and adding zinc chloride, the problems of poor adhesion and biocompatibility of bioadhesives in humid environments were solved, achieving rapid wound repair and promoting healing.
Patent Information
- Application Number
- CN202311527212.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-16
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-11-16
AI Technical Summary
Existing bioadhesives have poor adhesion in humid environments, are highly irritating to the human body, have poor biocompatibility, and are complex to prepare, making it difficult to meet the needs of rapid wound repair.
A bioadhesive was prepared by combining lipoic acid and aminolipoic acid through electrostatic interaction, and zinc chloride was added to promote wound healing, forming a lipoic acid-based bioadhesive with antibacterial and anti-inflammatory effects.
It offers excellent adhesion, good biocompatibility, and promotes wound healing, simplifying the operation process and making it suitable for emergency and surgical scenarios.
Smart Images

Figure CN117563037B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of bioadhesives, and in particular to a thioctic acid-based bioadhesive and its preparation and application. Background Technology
[0002] Trauma includes damage to normal skin (body tissue) caused by external factors such as surgery, external force, heat, electric current, chemicals, and low temperature, as well as internal factors such as local blood supply disorders. For all types of trauma, closing the wound as soon as possible is the best way to slow bleeding and prevent further infection. Traditional first aid methods use gauze, cotton, or sutures, or employ binding or plugging to urgently close the wound site. However, these materials do not have anti-inflammatory or antibacterial effects, which is not conducive to wound repair. Often, problems such as wound inflammation, bacterial infection, and surface necrosis will arise later. Furthermore, due to the characteristics of the materials themselves, they are prone to adhering to the wound surface, causing secondary damage when removed.
[0003] To address the shortcomings of traditional dressings, various adhesive hydrogels and bio-adhesives have been developed in recent years, making them ideal for rapid wound closure. Currently, commercially available adhesives mainly include natural biological tissue adhesives and synthetic adhesives. Natural biological adhesives, such as fibrin glue, are highly safe, contain no harmful substances, and are relatively safe for humans and the environment. They often have good biocompatibility, exhibiting low irritation and immune response to human tissues and cells. Natural biological adhesives are easily degraded and metabolized in the body, leaving no residue for tissue repair and reducing the risk of secondary surgery. However, natural biological adhesives also have unavoidable drawbacks, such as lower strength, making them unsuitable for bonding structures with heavy loads. Their bonding performance is poor in humid environments, and they are highly sensitive to water. Furthermore, their storage stability is relatively poor, easily affected by factors such as temperature and humidity. In addition, they are more expensive, have more complex application methods, and are not suitable for wound adhesive repair.
[0004] Synthetic adhesives, such as cyanoacrylate adhesives, typically possess high bonding strength and are suitable for bonding structures requiring heavy loads. Furthermore, their application scenarios are broader than those of natural biological adhesives. Synthetic biological adhesives can be used for bonding various materials, such as skin, bone, and soft tissue. However, synthetic adhesives also have some unavoidable drawbacks. For example, their safety is relatively low, their manufacturing processes are complex, and the safety of the catalysts and other chemicals used in their synthesis remains to be assessed, with potential risks to humans and the environment unclear. Secondly, commercially available liquid bandages and other synthetic adhesives often have strong irritant properties to human tissues and cells, resulting in a poor user experience and potentially causing severe inflammatory reactions. In addition, some synthetic adhesives have poor biocompatibility, with chemicals degrading slowly or not completely in the body, which may adversely affect tissue repair. Summary of the Invention
[0005] The purpose of this invention is to overcome the shortcomings of the existing technology and provide a thioctic acid-based bioadhesive with strong adhesion, good biocompatibility, and wound-healing effects, as well as its preparation and application. This invention utilizes a gel-forming method based on the tight electrostatic interaction between two small molecules, thioctic acid and aminothioctic acid, to prepare the thioctic acid-based bioadhesive material. Zinc chloride is added to provide zinc ions, thereby promoting wound healing.
[0006] The objective of this invention can be achieved through the following technical solutions: A method for preparing a thioctic acid-based bioadhesive, comprising: S1: Preparation of aminolipoic acid: Lipoic acid is dissolved in an organic solvent, and then a carboxyl activating reagent is added and stirred. N-tert-butoxycarbonylethylenediamine is added, stirred, and purified to obtain an intermediate product. The intermediate product is dissolved in an organic solvent, and a de-BOC protection reagent is added. The mixture is stirred and washed to obtain the aminolipoic acid. S2: Preparation of thioctic acid-based bioadhesive: First, mix the aminolipoic acid prepared above with zinc chloride, adjust the pH, and then add thioctic acid and stir to coagulate into a gel, thus obtaining the thioctic acid-based bioadhesive.
[0007] Further, in step S1, the molar ratio of the carboxyl activating reagent to lipoic acid is (1-1.1):1, the molar ratio of N-tert-butoxycarbonyl ethylenediamine to lipoic acid is (1-1.1):1, and the molar ratio of the deboc protecting reagent to the intermediate product is (1-5):1.
[0008] Further, in step S1, the organic solvent includes one of toluene, ethane, dichlorotoluene, dichlorobenzene, or chlorobenzene.
[0009] Further, in step S1, the carboxyl activating agent includes one or more of N,N' carbonyl diimidazole, (1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride), bis(2-oxo-3-oxazolidinyl) hypophosphite chloride, or dicyclohexylcarbodiimide.
[0010] Furthermore, in step S1, the deboc protection agent includes trifluoroacetic acid or hydrochloric acid.
[0011] Further, in step S2, the molar ratio of lipoic acid to aminolipoic acid is (0.2-5):1.
[0012] Furthermore, the zinc chloride content in the thioctic acid-based bioadhesive is 2-100 mg / mL.
[0013] Furthermore, in step S2, the time for gelation is 5-120 seconds.
[0014] A thioctic acid-based bioadhesive is prepared using the method described above.
[0015] Application of a thioctic acid-based bioadhesive in medical dressings to achieve effective wound closure.
[0016] Compared with the prior art, the present invention has the following advantages and beneficial effects: (1) Excellent adhesion properties: The present invention uses thioctic acid as a raw material, which can combine with the wound surface to form a strong adhesive layer, with excellent adhesion properties, effectively connecting tissues and providing a reliable wound closure effect.
[0017] (2) Biocompatibility: The present invention uses lipoic acid as a raw material. Lipoic acid is a natural compound with good biocompatibility. It will not cause serious local irritation or allergic reactions, and it will gradually degrade in tissues without leaving harmful residues.
[0018] (3) Adjustable gel morphology: Lipoic acid can control the morphology and rheological properties of the gel by adjusting its concentration and pH value. Therefore, it can be customized according to different wound needs, from soft gel to hard gel.
[0019] (4) Promote wound healing: The present invention incorporates zinc chloride, which works synergistically with lipoic acid to activate platelets and fibrin, promote angiogenesis and tissue regeneration, and help accelerate the wound healing process.
[0020] (5) Easy to operate: Thioctic acid bioadhesive can be applied directly to the wound surface without the need for additional special equipment or complicated operating steps, which makes it highly practical and operable in scenarios such as first aid and surgery.
[0021] (6) The thioctic acid-based bioadhesive provided by this invention has good biocompatibility, high viscosity, and the addition of zinc ions gives it certain antibacterial and anti-inflammatory effects. Furthermore, the preparation method of the thioctic acid-based bioadhesive provided by this invention is simple, easy to operate, requires no complex or expensive equipment, and is easy to industrialize. The thioctic acid-based bioadhesive provided by this invention can achieve rapid wound repair with quick and obvious effects. The thioctic acid-based bioadhesive material provided by this invention has good application prospects as a biomedical material. Attached Figure Description
[0022] Figure 1 The infrared spectrum of the thioctic acid-based bioadhesive in Example 1 is shown below. Figure 2 NMR comparison of BOC-aminolipoic acid, aminolipoic acid, and raw material lipoic acid prepared in Example 1; Figure 3 This is a diagram illustrating the bonding effect of the thioctic acid-based bio-adhesive in Example 1. Figure 4 The compressive stress-strain curve of the thioctic acid-based bioadhesive in Example 1 is shown. Figure 5 This is a diagram illustrating the bonding effect of the thioctic acid-based bio-adhesive in Example 1 on different substrates underwater. Figure 5 Figure labels: 1- Macroscopic schematic diagram of underwater adhesion of glass with lipoic acid-based bio-adhesive; 2- Macroscopic schematic diagram of underwater adhesion of Teflon sheet with lipoic acid-based bio-adhesive; 3- Macroscopic schematic diagram of underwater adhesion of rubber with lipoic acid-based bio-adhesive. Detailed Implementation
[0023] The present invention will now be described in detail with reference to the accompanying drawings and specific embodiments.
[0024] The following embodiments are implemented based on the above-described technical solution of the present invention, and provide detailed implementation methods and specific operation processes. However, the scope of protection of the present invention is not limited to the following embodiments.
[0025] The following are more detailed implementation examples, which further illustrate the technical solution of the present invention and the technical effects that can be obtained.
[0026] In the following embodiments, unless otherwise specified, the raw materials, reagents or processing techniques are all conventional commercial products or conventional processing techniques in the art.
[0027] Example 1 This embodiment provides a lipoic acid-based bioadhesive and its preparation method: (1) Preparation of aminolipoic acid: Under light-protected conditions at room temperature, 3.2 g (16 mmol) of thioctic acid was dissolved in 20 ml of dichloromethane, and then 2.5 g (16 mmol) of N,N'-carbonyldiimidazole (CDI) was added. The mixture was activated by magnetic stirring for 30 min, and then 2.7 g (17 mmol) of N-tert-butoxycarbonylethylenediamine (BOC-ethylenediamine) was slowly added at 450 r / min. The mixture was stirred magnetically for 12 h. After the reaction was completed, the mixture was washed with saturated sodium chloride solution and dried over anhydrous sodium sulfate. The product was then purified by column chromatography to obtain BOC-aminolipoic acid, which was a pale yellow powder crystal. Under light-protected conditions at room temperature, 3.7 g (10.7 mmol) of BOC-aminolipoic acid was dissolved in 25 ml of dichloromethane, and then 2.5 g (20 mmol) of trifluoroacetic acid was added dropwise. The mixture was magnetically stirred for 12 h. After the reaction was completed, the mixture was distilled under reduced pressure and washed with anhydrous diethyl ether. This process was repeated 5 times to obtain the product aminolipoic acid. (2) Preparation of thioctic acid-based bioadhesives: At room temperature, 8 mg of zinc chloride powder was dissolved in 0.5 ml of deionized water, and 0.5 g of the prepared aminolipoic acid was added. After mixing thoroughly, tris-hydroxymethylaminomethane (tris base) at a concentration of 0.25 g / ml was added to adjust the pH of the mixture to 8. Then, 0.5 g of lipoic acid powder was added, and the mixture was stirred thoroughly for 2 min. After coagulation for 40 s, a gel was formed, yielding an lipoic acid-based bioadhesive. Its infrared spectrum is shown below. Figure 1 As shown, the appearance of the NH peak confirms the synthesis of aminolipoic acid, and the shift of the infrared absorption peaks of NH and C=O proves the electrostatic interaction between lipoic acid and aminolipoic acid. Labeled as AC 0.5 -N 0.5 -Zn 1% ,like Figure 2 The figure shows the NMR comparison of BOC-aminolipoic acid, aminolipoic acid and raw material lipoic acid. The figure shows that BOC-aminolipoic acid and aminolipoic acid were successfully synthesized.
[0028] Among them, such as Figure 3 As shown in the figure, the thioctic acid-based bio-adhesive prepared in the example was tested for adhesion. As can be seen from the figure, the thioctic acid-based bio-adhesive has strong adhesion.
[0029] like Figure 4 As shown, the thioctic acid-based bioadhesive prepared in this embodiment was subjected to mechanical testing. The stress-strain curve shows that the thioctic acid-based bioadhesive has a certain mechanical strength. Combined with its adhesive properties, it can effectively ensure that the wound remains closed, prevent external bacterial contamination, and promote wound repair.
[0030] like Figure 5As shown, the thioctic acid-based bio-adhesive prepared in this embodiment is used to adhere to different substrates underwater. 1 is a macroscopic schematic diagram of underwater adhesion of glass by the thioctic acid-based bio-adhesive; 2 is a macroscopic schematic diagram of underwater adhesion of Teflon sheet by the thioctic acid-based bio-adhesive; 3 is a macroscopic schematic diagram of underwater adhesion of rubber by the thioctic acid-based bio-adhesive. As can be seen from the figures, the present invention has a certain underwater adhesion capability and can adhere to and lift a variety of materials underwater.
[0031] Example 2 This embodiment provides a lipoic acid-based bioadhesive and its preparation method: The procedure is the same as in Example 1, except that the amount of zinc chloride used is replaced with 25 mg instead of 8 mg in Example 1, to prepare a thioctic acid-based bioadhesive, labeled as: AC. 0.5 -N 0.5 -Zn 3% .
[0032] Example 3 This embodiment provides a lipoic acid-based bioadhesive and its preparation method: The steps are the same as in Example 1, except that zinc chloride is not added to prepare a thioctic acid-based bioadhesive, labeled as: AC. 0.5 -N 0.5 .
[0033] Example 4: This embodiment provides a lipoic acid-based bioadhesive and its preparation method: The steps are the same as in Example 1, except that in step (2), the amount of lipoic acid added is 0.3 g and the amount of aminolipoic acid added is 0.7 g. A lipoic acid-based bioadhesive is prepared and labeled as: AC. 0.3 -N 0.7 -Zn 1% .
[0034] Example 5: This embodiment provides a lipoic acid-based bioadhesive and its preparation method: The procedure is the same as in Example 1, except that the amount of lipoic acid added is 0.7 g and the amount of aminolipoic acid added is 0.3 g. A lipoic acid-based bioadhesive is prepared and labeled as: AC. 0.7 -N 0.3 -Zn 1% .
[0035] Testing and experimentation: 1. Adhesion strength test: Adhesion strength tests were conducted on the above-described embodiments and a comparative group of commercially available clinical fibrin adhesives (Guangzhou Beixiu Biotechnology Co., Ltd., porcine fibrin adhesive). Test reference standard: ASTM F2255-05 Specific implementation process: A 0.05 g / ml gelatin solution was applied to one side of two 2.5 cm × 5 cm glass slides and allowed to dry to simulate pigskin. Then, 0.3 g of the thioctic acid-based bio-adhesive prepared in Examples 1-5 was applied to the interlayer between the two slides to form an overlap area of 2.5 cm × 1 cm. After pressing by hand for 15 seconds, the slides were sheared apart using a universal tensile testing machine (Shenzhen Xin Sansi). The maximum force required was recorded, and then divided by the overlap area to obtain the adhesive strength. The specific results are shown in the table below. As can be seen from the table, the prepared thioctic acid-based bio-adhesive has better adhesive strength compared to the previous group.
[0036] Table 1: Adhesion strength tests of Examples 1-5 and comparative examples 2. Biocompatibility testing: The biocompatibility of this coating was evaluated according to the extraction solution test in GB / T 16886. The specific steps are as follows: (1) Extraction The thioctic acid-based bioadhesives prepared in Examples 1-5 were sterilized by radiation and then extracted with 10% fetal bovine serum DMEM medium at 37°C for 24 h to obtain the extract.
[0037] (2) Cell culture L929 cells in the exponential growth phase were digested with trypsin, counted using a counting chamber, and 100 μL of 1×10⁻⁶ cells were collected. 5 Cells at a concentration of 1 cell / mL were seeded in 96-well plates, with 6 parallel wells for each control group (cells cultured in cell culture medium) and experimental samples, and cultured in a 37°C, 5% CO2 incubator for 24 h.
[0038] After 24 hours, the culture medium of the experimental group was replaced with an equal volume of the extract, while the culture medium of the control group was replaced normally, and the culture was continued for another 24 hours.
[0039] (3) Detection After culturing for another 24 hours, 10 μL of CCK-8 (BET Biotech) was added to each well, and after incubation for 4 hours, the absorbance was measured at 450 nm using a microplate reader.
[0040] The relative cell proliferation rate of the experimental group was calculated with the absorbance of the control group as 100%.
[0041] Relative cell proliferation rate = As / Ac × 100% As: Absorbance of experimental wells (including cells, culture medium, CCK-8 solution, and thioctic acid binder extract); Ac: Absorbance of the control well (containing cells, culture medium, and CCK-8 solution); The biological properties of the lipoic acid-based adhesives prepared in Examples 1 to 5 are judged in combination with the relative cell proliferation grading table, and a relative proliferation degree (calculated based on the cell concentration on day 7) of grade 0 or grade 1 is judged as qualified, Table 2: Relative Cell Proliferation Degree Grading Table The experimental results are shown in the following table: Table 3: Biological Property Results of the Lipoic Acid-based Adhesives Prepared in Examples 1 to 5 The foregoing description of the embodiments is provided to enable any person skilled in the art to make and use the present invention. It will be apparent to those skilled in the art that various modifications can be readily made to these embodiments, and the general principles defined herein may be applied to other embodiments without inventive effort. Therefore, the present invention is not limited to the above-described embodiments, and all improvements and modifications made by those skilled in the art in light of the disclosure of the present invention without departing from the scope of the present invention shall fall within the protection scope of the present invention.
Claims
1. A method for preparing a thioctic acid-based bioadhesive, characterized in that, include: S1: Preparation of aminolipoic acid: Under the conditions of room temperature and protection from light, lipoic acid was dissolved in an organic solvent, and then a carboxyl activating reagent was added and stirred. N-tert-butoxycarbonylethylenediamine was added, stirred, and purified to obtain an intermediate product. The intermediate product was dissolved in an organic solvent, and a Boc deprotection reagent was added. After stirring and washing, the aminolipoic acid was obtained. S2: Preparation of thioctic acid-based bioadhesive: At room temperature, the aminolipoic acid prepared above is first mixed with zinc chloride, the pH is adjusted, and then thioctic acid is added and stirred to coagulate into a gel, thus obtaining the thioctic acid-based bioadhesive.
2. The method for preparing the thioctic acid-based bioadhesive according to claim 1, characterized in that, In step S1, the molar ratio of the carboxyl activating reagent to lipoic acid is (1-1.1):1, the molar ratio of N-tert-butoxycarbonylethylenediamine to lipoic acid is (1-1.1):1, and the molar ratio of the deBoc protecting reagent to the intermediate product is (1-5):
1.
3. The method for preparing the thioctic acid-based bioadhesive according to claim 1, characterized in that, In step S1, the organic solvent is selected from toluene, dichloromethane, dichlorobenzene, or chlorobenzene.
4. The method for preparing the thioctic acid-based bioadhesive according to claim 1, characterized in that, In step S1, the carboxyl activating agent includes one or more of N,N'-carbonyldiimidazole, 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride, bis(2-oxo-3-oxazolidinyl)phosphine chloride, or dicyclohexylcarbodiimide.
5. The method for preparing the thioctic acid-based bioadhesive according to claim 1, characterized in that, In step S1, the deBoc protection agent includes trifluoroacetic acid or hydrochloric acid.
6. The method for preparing the thioctic acid-based bioadhesive according to claim 1, characterized in that, In step S2, the molar ratio of lipoic acid to aminolipoic acid is (0.2-5):
1.
7. The method for preparing the thioctic acid-based bioadhesive according to claim 1, characterized in that, The zinc chloride content in the thioctic acid-based bioadhesive is 2-100 mg / mL.
8. The method for preparing the thioctic acid-based bioadhesive according to claim 1, characterized in that, In step S2, the time for gelation is 5-120 seconds.
9. A thioctic acid-based bioadhesive, characterized in that, It is prepared by the method described in any one of claims 1-8.
10. The use of a thioctic acid-based bioadhesive as described in claim 9 in the preparation of medical dressings.
Citation Information
Patent Citations
Lipoic acid hydrogel as well as preparation method and application thereof
CN115232329A
Composite hydrogel as well as preparation method and application thereof
CN116637234A