A hydrophobic nylon composite material and preparation method thereof
By cross-linking PA12 with ethyl cyanoacrylate and silicon tetrachloride plasma surface treatment, the problem of strong water absorption of nylon materials is solved, and its hydrophobic performance is significantly improved, making it suitable for applications in water conservancy, ships and other fields.
Patent Information
- Application Number
- CN202311815183.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-27
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-12-27
AI Technical Summary
Nylon materials have strong water absorption, which limits their application in industrial fields such as water conservancy and ships, and it is difficult to effectively modify its hydrophobic properties with existing technology.
PA12 is used as the main material, cross-linked with ethyl cyanoacrylate to form an interpenetrating polymer network structure, and silicon tetrachloride plasma surface treatment is performed, including 6-aminocaproic acid grafting, to improve the hydrophobic properties of the material.
It achieves high hydrophobicity of nylon composite materials, reduces the hydrophilicity of surface amide functional groups, significantly improves the hydrophobic properties of the material, and is suitable for large-scale production.
Smart Images

Figure CN117567862B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nylon composite materials, and in particular to a hydrophobic nylon composite material and a preparation method thereof. Background Art
[0002] Nylon, also known as polyamide, is an engineering plastic with excellent performance and wide application. It is widely used in many manufacturing industries and chemical industries, such as automobiles, airplanes, ships, etc. There are many varieties of nylon (PA), which are divided into polylactamide nylon and polydiacid diamine nylon, including PA6, PA66, PA12, PA46, PA610, PA612, PA1010, PA1012 and high temperature resistant nylon. The comprehensive performance of nylon is very excellent. It has high strength and impact resistance. It also has very high heat resistance, wear resistance, chemical resistance and flame retardancy. The friction coefficient of nylon is very low, which is due to the good self-lubricating properties of nylon itself. Because nylon has amide groups, high polarity and strong water absorption, it greatly limits the application of nylon in industrial fields such as water conservancy and ships. It can be seen that it is of great significance to modify nylon to be wear-resistant and hydrophobic. Summary of the invention
[0003] In order to overcome the deficiencies of the prior art, one of the objectives of the present invention is to provide a hydrophobic nylon composite material, the surface of which has hydrophobic properties.
[0004] The second object of the present invention is to provide a method for preparing a hydrophobic nylon composite material, which is simple to prepare and can be produced on a large scale.
[0005] One of the purposes of the present invention is achieved by the following technical solution:
[0006] A hydrophobic nylon composite material is composed of the following raw materials in parts by weight: 45-60 parts of nylon 12 and 12-15 parts of ethyl cyanoacrylate, wherein the amide groups of the nylon 12 and the carbon groups of polyethyl cyanoacrylate formed by cross-linking the ethyl cyanoacrylate interact with each other through hydrogen bonds to form an interpenetrating polymer network structure, and the method for forming the interpenetrating polymer network structure comprises the following steps:
[0007] S1, nylon 12, and ethyl cyanoacrylate were dispersed in formic acid solution;
[0008] S2. After evaporating the formic acid solution, the ethyl cyanoacrylate monomer begins to cross-link into polyethyl cyanoacrylate. During the cross-linking process, hydrogen bonds between the amide groups of the nylon 12 and the carbon groups of the polyethyl cyanoacrylate interact to form an interpenetrating polymer network structure.
[0009] The present invention uses PA12 as the main material. PA12 is also called nylon 12. The density of PA12 is relatively low, only 1.02g / cm 3 , plays a very important role in the field of lightweight materials; and its carbon chain is long, the amide group content is low, and the water absorption rate is relatively low compared to other types of nylon materials, only 0.25%. PA12 has very good wear resistance, and the wear rate is only 2.8mg / 1000r, which is very low among nylon materials.
[0010] Furthermore, after obtaining the hydrophobic nylon composite material, the process further includes a step of surface treating the hydrophobic nylon composite material. The specific steps are as follows:
[0011] S1, treating the surface of the hydrophobic nylon composite material with silicon tetrachloride plasma to obtain a silicon tetrachloride plasma functionalized substrate;
[0012] S2. Under the condition of diethyl ether, 6-aminocaproic acid is reacted with the silicon tetrachloride plasma functionalized substrate, and 6-aminocaproic acid is grafted onto the silicon tetrachloride plasma functionalized substrate to complete the surface treatment of the hydrophobic nylon composite material.
[0013] Furthermore, before S1, a cleaning procedure using argon plasma (300 W, 300 mTorr) was performed for 10 minutes before the plasma experiment to remove possible contaminants generated by the early plasma reaction.
[0014] Further, in S1, the SiCl 4 The nylon 12 is subjected to plasma treatment by plasma, the parallel plate capacitor is coupled to a cylindrical stainless steel reactor, the cylindrical stainless steel reactor comprises a stainless steel disc electrode with a diameter of 20 cm, the stainless steel disc electrode comprises an upper electrode and a lower electrode, the gap between the upper electrode and the lower electrode is 3 cm, the lower electrode is grounded, and the cylindrical stainless steel reactor is equipped with a radio frequency power supply with a frequency of 40 KHz.
[0015] Further, after placing the nylon 12 on the lower electrode, the cylindrical stainless steel reactor was evacuated to a basic pressure level of 30 mTorr, and the SiCl 4 The liquid storage valve and pump control valve are used to build the required SiCl 4 Working pressure, the SiCl 4 The working pressure is 150 mtorr; then 100 W of radio frequency energy is applied to the upper electrode and the lower electrode to start the SiCl 4The plasma is maintained for 1 minute; at the end of the reaction, after obtaining the silicon tetrachloride plasma functionalized substrate, the chamber is evacuated to the base pressure, and then the argon gas in the system is pressurized to atmospheric conditions.
[0016] The second object of the present invention is achieved by adopting the following technical solution:
[0017] A method for preparing a hydrophobic nylon composite material comprises the following steps:
[0018] S1, weighing the nylon 12 and the ethyl cyanoacrylate according to the formula amount, and after weighing, dispersing the nylon 12 and the ethyl cyanoacrylate in the formic acid solution;
[0019] S2, after evaporating the formic acid solution, after the evaporation is completed, the ethyl cyanoacrylate monomer begins to cross-link into the polyethyl cyanoacrylate, and during the cross-linking process, the amide group of the nylon 12 and the carbon group of the polyethyl cyanoacrylate interact with each other through hydrogen bonds to form the interpenetrating polymer network structure;
[0020] S3, adding the interpenetrating polymer network structure into a high-speed mixer and dispersing it evenly, and then sending it into a twin-screw extruder for extrusion and granulation to obtain the hydrophobic nylon composite material.
[0021] Furthermore, in S3, during extrusion, the temperature of each section of the twin screw is 225-245° C., the screw speed is 300-320 rpm, the material feeding speed is 15-25 rpm, and the extruded material strips are cooled and pelletized to obtain the hydrophobic nylon composite material.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] (1) The present invention provides a hydrophobic nylon composite material. The solution casting method is used. The amide groups of the nylon 12 and the carbon groups of the polycyanoacrylate formed by cross-linking the ethyl cyanoacrylate interact with each other through hydrogen bonds to form an interpenetrating polymer network structure, which exhibits unexpectedly high hydrophobicity. The interaction between nylon 12 and polycyanoacrylate prevents the interaction between water and the surface hydrophilic amide functional groups of nylon 12. The amide functional groups on the surface of the nylon composite material prepared by the method are gradually covered by polycyanoacrylate, reducing the number of amide functional groups on the solid-air interface and lowering the hydrophilicity of the amide functional groups. Therefore, the nylon composite material has good hydrophobicity.
[0024] (2) The present invention provides a hydrophobic nylon composite material. After obtaining the hydrophobic nylon composite material, it also includes a step of surface treating the hydrophobic nylon composite material, wherein 6-aminocaproic acid is grafted onto the surface of the hydrophobic nylon composite material. 6-aminocaproic acid is an amino acid with hydrophobicity and flexible structure, which makes the nylon composite material have excellent hydrophobic properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying any creative work.
[0026] Figure 1 is a morphological diagram of a water drop dropped into the surface of the injection-molded sample provided in Example 1;
[0027] Figure 2 is a morphological diagram of a water drop dropped into the surface of the injection-molded sample provided in Example 2;
[0028] Figure 3 This is a morphological diagram of a water drop dropped onto the surface of the injection-molded sample provided by comparative example nylon 12. DETAILED DESCRIPTION
[0029] The present invention is further described below in conjunction with specific embodiments. It should be noted that, under the premise of no conflict, the embodiments or technical features described below can be arbitrarily combined to form a new embodiment.
[0030] The sources of the raw materials used in the following examples are as follows:
[0031] Nylon 12 (PA12) was purchased from Hubei Yongkuo Technology Co., Ltd.;
[0032] Ethyl cyanoacrylate (ECA) was purchased from Hubei Zhonglong Kangsheng Fine Chemical Co., Ltd.;
[0033] Silicon tetrachloride (SiCl 4 , purity 99%, nitrogen filling) was purchased from Shanghai MacLean Biochemical Technology Co., Ltd.
[0034] 6-Aminocaproic acid was purchased from Shenggong Biotechnology (Shanghai) Co., Ltd.
[0035] The structural formula of ethyl cyanoacrylate and 6-aminocaproic acid is as follows:
[0036]
[0037] Example 1
[0038] This embodiment provides a hydrophobic nylon composite material, comprising the following steps:
[0039] A hydrophobic nylon composite material is composed of the following raw materials in parts by weight: 45-60 parts of nylon 12 and 12-15 parts of ethyl cyanoacrylate. The carbon groups of polyethyl cyanoacrylate formed by cross-linking ethyl cyanoacrylate with amide groups of nylon 12 interact with each other through hydrogen bonds to form an interpenetrating polymer network structure. The interpenetrating polymer network structure is formed by a solvent casting method, which comprises the following steps:
[0040] S1, nylon 12, and ethyl cyanoacrylate were dispersed in formic acid solution;
[0041] S2. After the formic acid solution is evaporated, the ethyl cyanoacrylate monomer begins to cross-link into polyethyl cyanoacrylate (PECA). During the cross-linking process, hydrogen bonds between the amide groups of nylon 12 and the carbon groups of polyethyl cyanoacrylate interact to form an interpenetrating polymer network structure.
[0042] A method for preparing a hydrophobic nylon composite material comprises the following steps:
[0043] S1. Weigh nylon 12 and ethyl cyanoacrylate according to the formula, and disperse the nylon 12 and ethyl cyanoacrylate in a formic acid solution;
[0044] S2, after evaporating the formic acid solution, after the evaporation is completed, the ethyl cyanoacrylate monomer begins to cross-link into polyethyl cyanoacrylate, and during the cross-linking process, the amide groups of nylon 12 and the carbon groups of polyethyl cyanoacrylate interact with each other through hydrogen bonds to form an interpenetrating polymer network structure;
[0045] The formation process is as follows:
[0046]
[0047] S3. Add the interpenetrating polymer network structure into a high-speed mixer and disperse it evenly, then send it into a twin-screw extruder for extrusion and granulation to obtain a hydrophobic nylon composite material.
[0048] Furthermore, in S3, during extrusion, the temperature of each section of the twin screw is 225-245° C., the screw speed is 300-320 rpm, the feeding speed is 15-25 rpm, and the extruded material strips are cooled and pelletized to obtain a hydrophobic nylon composite material.
[0049] Example 2
[0050] This embodiment provides a hydrophobic nylon composite material. After the hydrophobic nylon composite material is prepared in Example 1, the step of surface treating the hydrophobic nylon composite material is further included. The specific steps are as follows:
[0051] S1, treating the surface of a hydrophobic nylon composite material with silicon tetrachloride plasma to obtain a silicon tetrachloride plasma functionalized substrate;
[0052] Specifically, before S1, a cleaning procedure with argon plasma (300 W, 300 mTorr) was performed for 10 minutes before the plasma experiment to remove contaminants that may be generated by the early plasma reaction.
[0053] Specifically, in S1, the SiCl 4 Plasma is used to treat nylon 12. A parallel plate capacitor is used to couple a cylindrical stainless steel reactor. The cylindrical stainless steel reactor includes a stainless steel disc electrode with a diameter of 20 cm. The stainless steel disc electrode includes an upper electrode and a lower electrode. The gap between the upper electrode and the lower electrode is 3 cm. The lower electrode is grounded. The cylindrical stainless steel reactor is equipped with a radio frequency power supply with a frequency of 40 KHz.
[0054] Specifically, the hydrophobic nylon composite material prepared in Example 1 was placed on the lower electrode, and the cylindrical stainless steel reactor was evacuated to a basic pressure level of 30 mTorr. 4 The liquid storage valve and pump control valve establish the required SiCl 4 Working pressure, SiCl 4 The working pressure is 150mtorr; then 100W of RF energy is applied to the upper and lower electrodes to start the SiCl 4 Plasma was maintained for 1 minute; after obtaining the silicon tetrachloride plasma functionalized substrate, at the end of the reaction, the chamber of the cylindrical stainless steel reactor was evacuated to base pressure, and then the argon gas in the system was pressurized to atmospheric conditions.
[0055] S2. Under the condition of ether, 6-aminocaproic acid is reacted with a substrate functionalized by silicon tetrachloride plasma, and 6-aminocaproic acid is grafted onto the substrate functionalized by silicon tetrachloride plasma, thereby completing the surface treatment of the hydrophobic nylon composite material.
[0056] The reaction process is as follows:
[0057]
[0058] Comparative Example
[0059] The comparative example is nylon 12.
[0060] Experimental Example 1
[0061] Water absorption test
[0062] Water absorption was tested with reference to GB / T1034-2008. First, the hydrophobic nylon composite material pellets obtained in Example 1, Example 2, and Comparative Example were placed in a vacuum oven at 100°C for drying for 8 hours, and then injection molded at 265°C to prepare samples with a sample size of 60mm×60mm×2mm. The injection molded samples were dried at 50°C for 96 hours, and weighed after cooling; then, the injection molded samples were immersed in distilled water at 23°C for 24 hours, and the water absorption mass fraction was measured, as shown in Table 1.
[0063] Table 1 Water absorption properties of injection molded samples of hydrophobic nylon composite materials obtained in Example 1 and Example 2
[0064]
[0065]
[0066] Through testing, it is found that the injection-molded samples of the hydrophobic nylon composite materials obtained in Examples 1 and 2 of the present invention have low water absorption and excellent hydrophobic effect; while the comparative example easily absorbs water.
[0067] Experimental Example 2
[0068] Hydrophobicity test
[0069] Drop water into the surface of the injection-molded samples of Example 1, Example 2, and Comparative Example. Figure 1 As shown, Figure 1 For the injection-molded sample of Example 1, the water droplet maintains good hydrophobicity; Figure 2 For the injection-molded sample of Example 2, the water droplet maintains excellent hydrophobicity; Figure 3 For the injection-molded sample of the comparative example, the water droplets are easily dispersed and the hydrophobicity is significantly reduced.
[0070] The above-mentioned embodiments are only preferred embodiments of the present invention and cannot be used to limit the scope of protection of the present invention. Any non-substantial changes and substitutions made by technicians in this field on the basis of the present invention shall fall within the scope of protection required by the present invention.
Claims
1. A hydrophobic nylon composite material, characterized in that: The invention is composed of the following raw materials in parts by weight: 45-60 parts of nylon 12 and 12-15 parts of ethyl cyanoacrylate, wherein the amide groups of the nylon 12 and the carbon groups of the polyethyl cyanoacrylate formed by cross-linking the ethyl cyanoacrylate interact with each other through hydrogen bonds to form an interpenetrating polymer network structure, and the method for forming the interpenetrating polymer network structure comprises the following steps: S1, nylon 12, and ethyl cyanoacrylate were dispersed in formic acid solution; S2. After evaporating the formic acid solution, the ethyl cyanoacrylate monomer begins to cross-link into polyethyl cyanoacrylate. During the cross-linking process, hydrogen bonds between the amide groups of the nylon 12 and the carbon groups of the polyethyl cyanoacrylate interact to form an interpenetrating polymer network structure.
2. A hydrophobic nylon composite material as claimed in claim 1, characterized in that: After obtaining the hydrophobic nylon composite material, the method further includes the step of surface treating the hydrophobic nylon composite material. The specific steps are as follows: S1, treating the surface of the hydrophobic nylon composite material with silicon tetrachloride plasma to obtain a silicon tetrachloride plasma functionalized substrate; S2. Under the condition of diethyl ether, 6-aminocaproic acid is reacted with the silicon tetrachloride plasma functionalized substrate, and 6-aminocaproic acid is grafted onto the silicon tetrachloride plasma functionalized substrate to complete the surface treatment of the hydrophobic nylon composite material.
3. A hydrophobic nylon composite material as claimed in claim 2, characterized in that: Before S1, a 10-min argon plasma cleaning procedure was performed before the plasma experiment to remove possible contaminants generated by the early plasma reaction.
4. A hydrophobic nylon composite material as claimed in claim 3, characterized in that: In S1, the SiCl4 plasma between the parallel plates is used to perform plasma treatment on the nylon 12. The parallel plates are capacitively coupled to a cylindrical stainless steel reactor. The cylindrical stainless steel reactor includes a stainless steel disc electrode with a diameter of 20 cm. The stainless steel disc electrode includes an upper electrode and a lower electrode. The gap between the upper electrode and the lower electrode is 3 cm. The lower electrode is grounded. The cylindrical stainless steel reactor is equipped with a radio frequency power supply with a frequency of 40 KHz.
5. The hydrophobic nylon composite material according to claim 4, characterized in that: After placing the nylon 12 on the lower electrode, the cylindrical stainless steel reactor is evacuated to a base pressure level of 30 mTorr, and the required SiCl4 working pressure in the cylindrical stainless steel reactor is established by operating the SiCl4 liquid storage valve and the pump control valve of the cylindrical stainless steel reactor, and the SiCl4 working pressure is 150 mtorr; then, radio frequency energy with a power of 100 W is applied to the upper electrode and the lower electrode to start the SiCl4 plasma and maintain it for 1 minute; at the end of the reaction, after obtaining the silicon tetrachloride plasma functionalized substrate, the chamber is evacuated to the base pressure, and then the argon gas in the system is pressurized to atmospheric conditions.
6. The method for preparing a hydrophobic nylon composite material according to any one of claims 1 to 5, characterized in that: The following steps are involved: S1, weighing the nylon 12 and the ethyl cyanoacrylate according to the formula amount, and after weighing, dispersing the nylon 12 and the ethyl cyanoacrylate in the formic acid solution; S2, after evaporating the formic acid solution, after the evaporation is completed, the ethyl cyanoacrylate monomer begins to cross-link into the polyethyl cyanoacrylate, and during the cross-linking process, the amide group of the nylon 12 and the carbon group of the polyethyl cyanoacrylate interact with each other through hydrogen bonds to form the interpenetrating polymer network structure; S3, adding the interpenetrating polymer network structure into a high-speed mixer and dispersing it evenly, and then sending it into a twin-screw extruder for extrusion and granulation to obtain the hydrophobic nylon composite material.
7. The method for preparing a hydrophobic nylon composite material according to claim 6, characterized in that: In S3, during extrusion, the temperature of each section of the twin screw is 225-245° C., the screw speed is 300-320 rpm, the material feeding speed is 15-25 rpm, and the extruded material strips are cooled and pelletized to obtain the hydrophobic nylon composite material.
Citation Information
Patent Citations
Fibre sheet reinforcement alpha-cyano acrylate molding article
JP1989228841A