Liquid encapsulation composition, photovoltaic module and encapsulation method thereof
By using a liquid encapsulation composition, the problems of microcracks and PID in photovoltaic modules were solved, the crosslinking density and insulation performance of the encapsulation material were improved, the operation process was simplified, and the anti-PID performance and yield of photovoltaic modules were enhanced.
Patent Information
- Application Number
- CN202311522603.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-15
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-11-15
AI Technical Summary
Existing photovoltaic modules are prone to microcracks and PID (Potential Instability and Degradation) in high temperature and high humidity environments, and have poor resistance to PID.
A liquid encapsulation composition comprising a telechelic polymer and additives is used to form an encapsulation preform through mixing, degassing and curing. This solves the problem of microcracks in photovoltaic modules and improves the crosslinking density and insulation performance of the encapsulation material, while blocking the migration of metal ions.
It effectively prevents microcracks in solar cells, improves the anti-PID performance of photovoltaic modules, simplifies the operation process, and increases product yield and compatibility of encapsulation materials.
Smart Images

Figure CN117567943B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of optoelectronic technology, and more specifically, to a liquid encapsulation composition, a photovoltaic module, and an encapsulation method thereof. Background Technology
[0002] In crystalline silicon photovoltaic cells, reducing wafer thickness and increasing wafer size are ways to reduce costs and improve efficiency. Similarly, in crystalline silicon photovoltaic modules, improving the performance of various encapsulation materials and reducing their usage are also methods to reduce costs and improve efficiency. Currently, the development trend of crystalline silicon photovoltaic modules is towards larger and lighter designs. This trend presents increasing challenges to the mechanical strength of crystalline silicon photovoltaic modules. As crystalline silicon cells become thinner and larger, and as encapsulation materials become thinner, the problem of microcracks in crystalline silicon photovoltaic modules is becoming increasingly prominent.
[0003] Furthermore, in high-temperature and high-humidity environments, moisture enters the photovoltaic module and, through a series of chemical reactions, causes a large number of freely moving Na ions to precipitate from the glass protective layer. Under the influence of an external electric field, these ions migrate to the cell surface and accumulate in the anti-reflection layer, increasing leakage current. They also recombine with charge carriers in the cell, reducing the charge carrier concentration and ultimately leading to a decrease in module power output. Therefore, limiting the migration ability of metal ions in the encapsulant film and reducing the content of free ions in the module are both promising ways to avoid the PID phenomenon in solar modules. Summary of the Invention
[0004] The main objective of this invention is to provide a liquid encapsulation composition, a photovoltaic module, and an encapsulation method thereof to solve the problems of poor anti-PID performance and easy microcracks in the cells of existing photovoltaic modules.
[0005] To achieve the above objectives, according to one aspect of the present invention, a liquid encapsulation composition is provided, comprising, by weight parts: 80 to 99.9 parts by weight of a telechelic polymer and 0.1 to 20 parts by weight of an additive, wherein the telechelic polymer has the following general chemical formula: Where M is a C2~C2 bond containing carbon-carbon unsaturated bonds. 40 The alkylene group, The molecular weight is 5000 to 30000; R1 and R2 are each independently selected from any one of hydroxyl, carboxyl, epoxy, amino, amide, and hydroxylamine groups.
[0006] Furthermore, M is selected from any one or more of the following: groups containing vinylidene, groups represented by the formula CH2=C(Y1)-, and groups represented by the formula Y1CH=CH-, wherein Y1 is C1 to C2. 30 The hydrocarbon group, preferably Y1 is C2~C3. 30The olefinic group, further preferably Y1 is C3-C4. 15 The olefinic group; preferably, M also includes an olefinyl group obtained by removing two terminal hydrogen atoms from the molecular chain of the ethylene / α-olefin copolymer, wherein the α-olefin copolymer is C3~C4. 30 α-olefins, preferably α-olefin copolymers with C3 to C4 olefins. 10 The α-olefin, preferably the α-olefin copolymer, is selected from any one or more of propylene, isobutene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-heptene, 1-octene, 1-nonene, and 1-decene; preferably M also includes an olefinyl group obtained by removing two terminal hydrogen atoms from the molecular chain of the conjugated diene copolymer, preferably the conjugated diene copolymer is a C4 to C6 conjugated diene copolymer, preferably the conjugated diene copolymer is selected from any one or more of cis-1,4-polybutadiene, trans-1,4-polybutadiene, and 1,2-polybutadiene.
[0007] Furthermore, the total number of moles of R1 and R2 is n, and the ratio of n to the mass of the liquid encapsulation composition ranges from 0.4 to 0.8 mmol / g.
[0008] Furthermore, the melting enthalpy ΔHm of the aforementioned telechelic polymer is 5–210 J / g.
[0009] Furthermore, a silane coupling agent is grafted onto the molecular chain of M as a side chain, preferably with a grafting rate of 0.1% to 15%. The silane coupling agent is preferably selected from any one or more of allyltrimethoxysilane, allyltriethoxysilane, allyltriisopropoxysilane, vinylethyltrimethoxysilane, vinylethyltriethoxysilane, vinylpropyltrimethoxysilane, vinylbutyltrimethoxysilane, vinylbutyltriethoxysilane, vinylbutyltriisopropoxysilane, vinylpentyltrimethoxysilane, vinylhexyltrimethoxysilane, vinylheptyltrimethoxysilane, and vinyloctyltrimethoxysilane.
[0010] Furthermore, R1 and R2 are each independently selected from any one of hydroxyl, carboxyl, amino, amide, and hydroxylamine groups. By weight, the liquid encapsulation composition includes: 90 to 99.9 parts by weight of the telechelic polymer, 0.05 to 5 parts by weight of the crosslinking agent, and 0.05 to 5 parts by weight of the co-crosslinking agent.
[0011] Furthermore, both R1 and R2 are epoxy groups. By weight, the liquid encapsulation composition includes: 85 to 99.9 parts by weight of the telechelic polymer, 0.09 to 14.5 parts by weight of the curing agent, and 0.01 to 0.5 parts by weight of the crosslinking agent.
[0012] Furthermore, the viscosity of the above-mentioned liquid encapsulation composition at 25°C is 2000–8000 mPa·s.
[0013] According to another aspect of the present invention, a method for encapsulating a photovoltaic module is provided, the method comprising: step S1, mixing and degassing the components of an encapsulation composition to form an encapsulation liquid; step S2, disposing the encapsulation liquid between an upper substrate, a cell unit and a lower substrate to form an encapsulation preform; and step S3, degassing and curing the encapsulation preform to obtain a photovoltaic module, wherein the encapsulation composition is the aforementioned liquid encapsulation composition.
[0014] According to another aspect of the present invention, a photovoltaic module is provided, the photovoltaic module comprising a lower substrate, a cell unit and an upper substrate, wherein the pores between the lower substrate, the cell unit and the upper substrate are filled with an encapsulating adhesive, the encapsulating adhesive being cured from the aforementioned liquid encapsulation composition.
[0015] By applying the technical solution of this invention, on the one hand, this application is a liquid encapsulation method, which can solve the problem of microcracks in photovoltaic module cells caused by increasingly thinner and larger cell thicknesses and thinner encapsulation materials. On the other hand, compared with conventional encapsulation materials, the teleclaw polymer has a higher crosslinking density after curing, resulting in better insulation performance of the encapsulation material, which can better block the migration of metal ions to the cell and has better anti-PID performance. In addition, the teleclaw polymer has polar end groups, which have better compatibility with various additives, thereby avoiding the problem of additive overflow caused by incompatibility between conventional POE resin and additives.
[0016] also, The molecular weight is too high, the viscosity of the liquid encapsulation composition is too high, its flowability is too poor, and it is not easy to process later. The molecular weight is too low, and the viscosity of the liquid encapsulation composition is too low, which is not conducive to subsequent film formation. Detailed Implementation
[0017] It should be noted that, unless otherwise specified, the embodiments and features described in this application can be combined with each other. The present invention will now be described in detail with reference to the embodiments.
[0018] As analyzed in the background section, existing photovoltaic modules suffer from poor anti-PID performance and are prone to microcracks in the cells. To address this issue, the present invention provides a liquid encapsulation composition, a photovoltaic module, and an encapsulation method thereof.
[0019] In a typical embodiment of this application, a liquid encapsulation composition is provided, comprising, by weight, 80 to 99.9 parts of a telechelic polymer and 0.1 to 20 parts by weight of an additive, wherein the telechelic polymer has the following general chemical formula: Where M is a C2~C2 bond containing carbon-carbon unsaturated bonds. 40 The alkylene group, The molecular weight is 5000 to 30000; R1 and R2 are each independently selected from any one of hydroxyl, carboxyl, epoxy, amino, amide, and hydroxylamine groups.
[0020] On the one hand, this application utilizes liquid encapsulation, which can solve the problem of microcracks in photovoltaic module cells caused by increasingly thinner and larger cell thicknesses and thinner encapsulation materials. On the other hand, compared with conventional encapsulation materials, the telechelic polymer has a higher cross-linking density after curing, resulting in encapsulation materials with better insulation properties, better blocking of metal ion migration to the cell, and better anti-PID performance. Furthermore, the telechelic polymer has polar end groups, resulting in better compatibility with various additives, thus avoiding the problem of additive overflow caused by incompatibility between conventional POE resin and additives.
[0021] also, The molecular weight is too high, the viscosity of the liquid encapsulation composition is too high, its flowability is too poor, and it is not easy to process later. The molecular weight is too low, and the viscosity of the liquid encapsulation composition is too low, which is not conducive to subsequent film formation.
[0022] Preferred additives may include any one or more of crosslinking agents, co-crosslinking agents, and tackifiers. Among them, crosslinking agents help promote polymer crosslinking, thereby enabling the polymer to achieve a higher degree of crosslinking. In a preferred embodiment, the crosslinking agent in the above composition is preferably selected from those commonly used in the art. Further, the crosslinking agent is preferably one or more from the group consisting of tert-butyl peroxycarbonate, 2,5-dimethyl-2,5-(bis-tert-butylperoxy)hexane, tert-butyl peroxycarbonate-2-ethylhexyl ester, 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, 1,1-bis(tert-pentylperoxy)-3,3,5-trimethylcyclohexane, 1,1-bis(tert-pentylperoxy)cyclohexane, 1,1-bis(tert-butylperoxy)cyclohexane, 2,2-bis(tert-butylperoxy)butane, tert-pentyl peroxycarbonate, 2,5-dimethyl-2,5-dimethyl-2,5-dimethyl-2,5-bis(benzoylperoxy)-hexane, tert-pentyl peroxycarbonate, and tert-butyl peroxy 3,3,5-trimethylhexanoate. In a preferred embodiment, the co-crosslinking agent includes, but is not limited to, triallyl isocyanurate, triallyl cyanurate, trimethylolpropane triacrylate, trimethylolpropane trimethacrylate, pentaerythritol triacrylate, tri(2-hydroxyethyl)isocyanurate triacrylate, ethoxylated trimethylolpropane triacrylate, propionyl methylolpropane triacrylate, ethoxylated glycerol triacrylate, propionyl glycerol triacrylate, pentaerythritol tetraacrylate, ethoxylated pentaerythritol tetraacrylate, trimethylolpropane tetraacrylate, and bis(trimethylolpropane) The adhesive comprises any one or more of the following: propane tetraacrylate, bis(trimethylolpropane)tetramethacrylate, propoxylated pentaerythritol tetraacrylate, 2,4,6-tris(2-propenyloxy)-1,3,5-triazine, tricyclodecanedimethylethanol diacrylate, propoxylated neopentyl glycol diacrylate, ethoxylated bisphenol A diacrylate, ethoxylated bisphenol A dimethacrylate, 2-butyl-2-ethyl-1,3-propanediol diacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, and polyethylene glycol dimethacrylate. The addition of a tackifier is beneficial for improving the adhesion between the adhesive film and the substrate. In a preferred embodiment, the tackifier includes, but is not limited to, any one or more of the group consisting of γ-aminopropyltriethoxysilane, γ-methacryloxypropyltrimethoxysilane, γ-(2,3-epoxypropoxy)propyltrimethoxysilane, vinyltrimethoxysilane, N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, γ-glycidoxypropyltrimethylsilane, and 3-aminopropyltrimethylsilane.
[0023] Of course, skilled technicians may add other types of additives as needed, which will not be elaborated here.
[0024] In one embodiment of this application, M is selected from any one or more of the following: groups containing vinylidene, groups represented by the formula CH2=C(Y1)-, and groups represented by the formula Y1CH=CH-, wherein Y1 is C1 to C2. 30 The hydrocarbon group, preferably Y1 is C2~C3. 30 The olefinic group, further preferably Y1 is C3-C4. 15 The olefinic group; preferably, M also includes an olefinyl group obtained by removing two terminal hydrogen atoms from the molecular chain of the ethylene / α-olefin copolymer, wherein the α-olefin copolymer is C3~C4. 30 α-olefins, preferably α-olefin copolymers with C3 to C4 olefins. 10 The α-olefin, preferably the α-olefin copolymer, is selected from any one or more of propylene, isobutene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-heptene, 1-octene, 1-nonene, and 1-decene; preferably M also includes an olefinyl group obtained by removing two terminal hydrogen atoms from the molecular chain of the conjugated diene copolymer, preferably the conjugated diene copolymer is a C4 to C6 conjugated diene copolymer, preferably the conjugated diene copolymer is selected from any one or more of cis-1,4-polybutadiene, trans-1,4-polybutadiene, and 1,2-polybutadiene.
[0025] The preferred M above gives the telechelic polymer better water vapor permeability and insulation properties, thereby enabling the photovoltaic module obtained from the above liquid encapsulation composition to have anti-PID performance. In addition, the preferred M has a wide range of choices, such as M being an olefin group obtained by removing two terminal hydrogen atoms from the molecular chain of an ethylene / α-olefin copolymer or M being an olefin group obtained by removing two terminal hydrogen atoms from the molecular chain of a conjugated diene copolymer, thereby enabling the liquid encapsulation composition of this application to have a wider range of applications.
[0026] In one embodiment of this application, the total number of moles of R1 and R2 is n, and the ratio of n to the mass of the liquid encapsulation composition ranges from 0.4 to 0.8 mmol / g.
[0027] Both R1 and R2 are active groups. The preferred ratio range of n to the mass of the liquid encapsulation composition is beneficial for achieving a higher crosslinking density after curing, thereby improving its insulation performance and better preventing metal ions from migrating to the battery cell. Furthermore, the preferred content of active groups further enhances its compatibility with various additives.
[0028] In one embodiment of this application, the melting enthalpy ΔHm of the above-mentioned telechelic polymer is 5 to 210 J / g.
[0029] The aforementioned enthalpy of fusion is tested using DSC. The principle of DSC for measuring enthalpy of fusion is as follows: Since the enthalpy of a polymer changes significantly before and after melting, an endothermic peak (melting) is generated on the DSC curve. The area between the baselines of this melting peak (peak area) is measured, and then normalized to the sample mass to obtain the enthalpy of fusion of the sample. Currently, the standard for DSC determination of enthalpy in plastics is GB 19466-3, using nitrogen (analytical grade) as the test gas at a flow rate of 50 mL / min. The sample mass is 5 mg to 10 mg, accurate to 0.1 mg. Heating and cooling tests are performed at a rate of 20 °C / min. The enthalpy of fusion ΔHm of the aforementioned telechelic polymer is 5–210 J / g. This is due to the difference in crystallinity caused by the arrangement of flexible and rigid regions in the telechelic polymer of this invention, which is reflected in its cohesive strength. When the enthalpy of melting exceeds 210 J / g, sufficient bonding strength may not be obtained at temperatures below the melting temperature of the teleclaw polymer. Furthermore, the enthalpy of melting is positively correlated with the crystallinity of the teleclaw polymer. If the enthalpy of melting is too high, the crystallinity will be high, which may reduce the storage stability of the teleclaw polymer to some extent. Therefore, this application preferably has the enthalpy of melting of the teleclaw polymer ΔHm within the above range.
[0030] In one embodiment of this application, a silane coupling agent is grafted as a side chain onto the molecular chain of M, preferably with a grafting rate of 0.1% to 15%. The preferred silane coupling agent is selected from any one or more of allyltrimethoxysilane, allyltriethoxysilane, allyltriisopropoxysilane, vinylethyltrimethoxysilane, vinylethyltriethoxysilane, vinylpropyltrimethoxysilane, vinylbutyltrimethoxysilane, vinylbutyltriethoxysilane, vinylbutyltriisopropoxysilane, vinylpentyltrimethoxysilane, vinylhexyltrimethoxysilane, vinylheptyltrimethoxysilane, and vinyloctyltrimethoxysilane.
[0031] Grafting a silane coupling agent onto the molecular chain of M above, and controlling the grafting rate within the above range, helps to improve the cross-linking and curing effect of the telechelic polymer and improve its compatibility with additives.
[0032] In one embodiment of this application, R1 and R2 are each independently selected from any one of hydroxyl, carboxyl, amino, amide, and hydroxylamine groups. By weight, the liquid encapsulation composition includes: 90 to 99.9 parts by weight of a telechelic polymer, 0.05 to 5 parts by weight of a crosslinking agent, and 0.05 to 5 parts by weight of a co-crosslinking agent.
[0033] The liquid encapsulation composition having the above components and their contents is cross-linked and cured by thermosetting. Preferred contents of each component within the above ranges contribute to improved synergistic effects between the components, thereby enhancing the anti-PID performance of the photovoltaic module.
[0034] In one embodiment of this application, R1 and R2 are both epoxy groups. By weight, the liquid encapsulation composition includes: 85 to 99.9 parts by weight of a telechelic polymer, 0.09 to 14.5 parts by weight of a curing agent, and 0.01 to 0.5 parts by weight of a crosslinking agent.
[0035] The liquid encapsulation composition having the above components and their contents is cross-linked and cured by photocuring. Preferred content ranges for each component help improve the synergistic effect between the components, thereby enhancing the anti-PID performance of the photovoltaic module. Furthermore, it is preferred that the curing agent be an amine-based curing agent, thus helping to avoid contamination associated with using toluene diisocyanate curing systems.
[0036] In one embodiment of this application, the viscosity of the above-mentioned liquid encapsulation composition at 25°C is 2000-8000 mPa·s.
[0037] If the viscosity of the liquid encapsulation composition is too high, its flowability is poor and it is difficult to permeate. If the viscosity of the liquid encapsulation composition is too low, the flowability of the liquid encapsulation composition is too strong, making it difficult to encapsulate. The above-mentioned viscosity range is preferred and conducive to the successful encapsulation of photovoltaic modules.
[0038] In another typical embodiment of this application, a method for encapsulating a photovoltaic module is provided. The encapsulation method includes: step S1, mixing and degassing the components of an encapsulation composition to form an encapsulation liquid; step S2, disposing the encapsulation liquid between an upper substrate, a cell unit, and a lower substrate to form an encapsulation preform; and step S3, degassing and curing the encapsulation preform to obtain a photovoltaic module, wherein the encapsulation composition is the aforementioned liquid encapsulation composition.
[0039] By using the liquid encapsulation composition of this application for encapsulation, the operation process can be simplified, the production cost can be reduced, and the cell is less likely to break during curing compared to solid encapsulation methods. It is also relatively easy to remove air bubbles, which helps to improve the product yield and obtain photovoltaic modules with better anti-PID performance, which has a good application prospect.
[0040] In another typical embodiment of this application, a photovoltaic module is provided, which includes a lower substrate, a cell unit and an upper substrate, wherein the pores between the lower substrate, the cell unit and the upper substrate are filled with an encapsulating adhesive, which is formed by curing the above-mentioned liquid encapsulation composition.
[0041] Photovoltaic modules encapsulated using the liquid encapsulation composition of this application exhibit excellent anti-PID performance.
[0042] The beneficial effects of this application will be explained below with reference to specific embodiments and comparative examples.
[0043] Example 1
[0044] By weight, 99 parts of the telescopic polymer A liquid encapsulation composition was obtained by dispensing 0.1 parts by weight of crosslinking agent 2,5-dimethyl-2,5-di(tert-butylperoxide)hexane, 0.1 parts by weight of co-crosslinking agent triallyl isocyanurate, and 0.8 parts by weight of tackifier vinyltris(β-methoxyethoxy)silane, wherein M is a repeating unit of ethylene-1-octene copolymer. The molecular weight is approximately 10,000; R1 is an amide group, and R2 is an amide group. The total molar number of R1 and R2 is n, and the ratio of n to the mass of the liquid encapsulation composition is in the range of 0.5 mmol / g. The melting enthalpy ΔHm of the telechelic polymer is 150 J / g.
[0045] Example 2
[0046] By weight, 99 parts of the telescopic polymer 0.5 parts by weight of curing agent 593 (Sanmu) and 0.5 parts by weight of crosslinking agent triallyl isocyanurate were used to obtain a liquid encapsulation composition, wherein M is a repeating unit of ethylene-1-octene copolymer. The molecular weight is approximately 10,000; both R1 and R2 are epoxy groups.
[0047] Example 3
[0048] The difference from Example 1 is that M is a repeating unit of cis-1,4-polybutadiene. The molecular weight is approximately 30,000, ultimately yielding a liquid encapsulation composition.
[0049] Example 4
[0050] The difference from Example 1 is that M is a repeating unit of 1,2-polybutadiene. The molecular weight is approximately 5000, ultimately yielding a liquid encapsulation composition.
[0051] Example 5
[0052] The difference from Example 1 is that M is a repeating unit of the ethylene-1-octene copolymer. The molecular weight is approximately 5000, ultimately yielding a liquid encapsulation composition.
[0053] Example 6
[0054] The difference from Example 1 is that R1 is a carboxyl group and R2 is a hydroxyl group, resulting in a liquid encapsulation composition.
[0055] Example 7
[0056] The difference from Example 1 is that R1 is a carboxyl group and R2 is an amino group, resulting in a liquid encapsulation composition.
[0057] Example 8
[0058] The difference from Example 1 is that R1 is an amide group and R2 is a hydroxyl group, resulting in a liquid encapsulation composition.
[0059] Example 9
[0060] The difference from Example 1 is that the telechelic polymer The liquid encapsulation composition is obtained by using 80 parts by weight of the following ingredients: 2 parts by weight of the crosslinking agent 2,5-dimethyl-2,5-di(tert-butylperoxide)hexane, 2 parts by weight of the co-crosslinking agent triallyl isocyanurate, and 16 parts by weight of the tackifier vinyltris(β-methoxyethoxy)silane.
[0061] Example 10
[0062] The difference from Example 1 is that the telechelic polymer The liquid encapsulation composition is obtained by comprising 99.9 parts by weight of the crosslinking agent 2,5-dimethyl-2,5-di(tert-butylperoxide)hexane, 0.01 parts by weight of the co-crosslinking agent triallyl isocyanurate, and 0.08 parts by weight of the tackifier vinyltris(β-methoxyethoxy)silane.
[0063] Example 11
[0064] The difference from Example 1 is that the ratio of n to the mass of the liquid encapsulation composition is in the range of 0.4 mmol / g, and the liquid encapsulation composition is finally obtained.
[0065] Example 12
[0066] The difference from Example 1 is that the ratio of n to the mass of the liquid encapsulation composition is in the range of 0.8 mmol / g, and the liquid encapsulation composition is finally obtained.
[0067] Example 13
[0068] The difference from Example 1 is that the ratio of n to the mass of the liquid encapsulation composition is in the range of 0.3 mmol / g, and the liquid encapsulation composition is finally obtained.
[0069] Example 14
[0070] The difference from Example 1 is that the melting enthalpy ΔHm of the telechelic polymer is 5 J / g, resulting in a liquid encapsulation composition.
[0071] Example 15
[0072] The difference from Example 1 is that the melting enthalpy ΔHm of the telechelic polymer is 210 J / g, resulting in a liquid encapsulation composition.
[0073] Example 16
[0074] The difference from Example 1 is that the melting enthalpy ΔHm of the telechelic polymer is 2J / g, resulting in a liquid encapsulation composition.
[0075] Example 17
[0076] The difference from Example 1 is that vinylethyltrimethoxysilane is grafted onto the molecular chain of M in the telechelic polymer as a side chain, with a grafting rate of 0.1%, ultimately resulting in a liquid encapsulation composition.
[0077] Example 18
[0078] The difference from Example 1 is that vinylethyltrimethoxysilane is grafted onto the molecular chain of M in the telechelic polymer as a side chain, with a grafting rate of 10%, ultimately yielding a liquid encapsulation composition.
[0079] Example 19
[0080] The difference from Example 1 is that vinylethyltrimethoxysilane is grafted onto the molecular chain of M in the telechelic polymer as a side chain, with a grafting rate of 15%, ultimately resulting in a liquid encapsulation composition.
[0081] Example 20
[0082] The difference from Example 2 is that, by weight, 85 parts of the telescopic polymer are used. A liquid encapsulation composition was obtained by mixing 14.5 parts by weight of curing agent 650C (Miki) and 0.5 parts by weight of crosslinking agent triallyl isocyanurate, wherein M is a repeating unit of ethylene-1-octene copolymer. The molecular weight is approximately 10,000; both R1 and R2 are epoxy groups.
[0083] Example 21
[0084] The difference from Example 2 is that, by weight, 99.9 parts of the telechelicer polymer... A liquid encapsulation composition was obtained by dissolving 0.09 parts by weight of curing agent 650C (Miki) and 0.01 parts by weight of crosslinking agent triallyl isocyanurate, wherein M is a repeating unit of ethylene-1-octene copolymer. The molecular weight is approximately 10,000; both R1 and R2 are epoxy groups.
[0085] Comparative Example 1
[0086] The difference from Example 1 is that both R1 and R2 are H, resulting in a liquid encapsulation composition.
[0087] Comparative Example 2
[0088] The difference from Example 1 is that, The molecular weight is approximately 4000, ultimately yielding a liquid encapsulation composition.
[0089] Comparative Example 3
[0090] The difference from Example 1 is that, The molecular weight is approximately 35,000, ultimately yielding a liquid encapsulation composition.
[0091] Comparative Example 4
[0092] The difference from Example 1 is that 70 parts by weight of the remote claw polymer and 30 parts by weight of the additives ultimately yield a liquid encapsulation composition.
[0093] Comparative Example 5
[0094] The difference from Example 1 is that cis-1,4-polybutadiene is used instead of the telechelic polymer to obtain the liquid encapsulation composition.
[0095] Laminated photovoltaic modules were prepared using the liquid encapsulation compositions of the above embodiments and comparative examples, and volume resistivity and PID tests were performed. Volume resistivity was tested according to GB / T 1410-2006, and PID testing was conducted according to IEC TS 62804-1:2015. The test results are shown in Table 1.
[0096] Table 1
[0097]
[0098]
[0099] As can be seen from the above description, the embodiments of the present invention achieve the following technical effects:
[0100] On the one hand, this application utilizes liquid encapsulation, which can solve the problem of microcracks in photovoltaic module cells caused by increasingly thinner and larger cell thicknesses and thinner encapsulation materials. On the other hand, compared with conventional encapsulation materials, the telechelic polymer has a higher cross-linking density after curing, resulting in encapsulation materials with better insulation properties, better blocking of metal ion migration to the cell, and better anti-PID performance. Furthermore, the telechelic polymer has polar end groups, resulting in better compatibility with various additives, thus avoiding the problem of additive overflow caused by incompatibility between conventional POE resin and additives.
[0101] also, The molecular weight is too high, the viscosity of the liquid encapsulation composition is too high, its flowability is too poor, and it is not easy to process later. The molecular weight is too low, and the viscosity of the liquid encapsulation composition is too low, which is not conducive to subsequent film formation.
[0102] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A liquid encapsulation composition, characterized in that, The liquid encapsulation composition comprises, by weight, 80-99.9 parts of a telechelic polymer and 0.1-20 parts by weight of an additive, wherein the telechelic polymer has the following general chemical formula: Where M is a C2~C bond containing carbon-carbon unsaturated bonds. 40 The alkylene group, The molecular weight is 5000~30000; R1 and R2 are each independently selected from any one of hydroxyl, carboxyl, epoxy, amino, amide, and hydroxylamine groups; The ratio of the total molar number of R1 and R2 to the mass of the liquid encapsulation composition ranges from 0.4 to 0.8 mmol / g; The melting enthalpy ΔHm of the telechelic polymer is 5~210 J / g.
2. The liquid encapsulation composition according to claim 1, characterized in that, The M is selected from any one or more of the following: containing vinylidene groups, groups represented by the formula CH2=C(Y1)-, and groups represented by the formula Y1CH=CH-, wherein Y1 is C1~C1. 30 Hydrocarbon group.
3. The liquid encapsulation composition according to claim 2, characterized in that, Y1 is C2~C 30 olefin group.
4. The liquid encapsulation composition according to claim 3, characterized in that, Y1 is C3~C 15 olefin group.
5. The liquid encapsulation composition according to claim 1, characterized in that, The M further includes an olefinic group obtained by removing two terminal hydrogen atoms from the molecular chain of the ethylene / α-olefin copolymer, wherein the α-olefin copolymer is C3~C4. 30 α-olefins.
6. The liquid encapsulation composition according to claim 5, characterized in that, The α-olefin copolymer is C3~C 10 α-olefins.
7. The liquid encapsulation composition according to claim 6, characterized in that, The α-olefin copolymer is selected from any one or more of propylene, isobutylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-heptene, 1-octene, 1-nonene, and 1-decene.
8. The liquid encapsulation composition according to claim 1, characterized in that, The M also includes an olefinic group obtained by removing two terminal hydrogen atoms from the molecular chain of a conjugated diene copolymer.
9. The liquid encapsulation composition according to claim 8, characterized in that, The conjugated diene copolymer is a C4~C6 conjugated diene copolymer.
10. The liquid encapsulation composition according to claim 9, characterized in that, The conjugated diene copolymer is selected from any one or more of cis-1,4-polybutadiene, trans-1,4-polybutadiene, and 1,2-polybutadiene.
11. The liquid encapsulation composition according to claim 1, characterized in that, A silane coupling agent is grafted onto the molecular chain of M as a side chain, with a grafting rate of 0.1-15%.
12. The liquid encapsulation composition according to claim 11, characterized in that, The silane coupling agent is selected from any one or more of allyltrimethoxysilane, allyltriethoxysilane, allyltriisopropoxysilane, vinylethyltrimethoxysilane, vinylethyltriethoxysilane, vinylpropyltrimethoxysilane, vinylbutyltrimethoxysilane, vinylbutyltriethoxysilane, vinylbutyltriisopropoxysilane, vinylpentyltrimethoxysilane, vinylhexyltrimethoxysilane, vinylheptyltrimethoxysilane, and vinyloctyltrimethoxysilane.
13. The liquid encapsulation composition according to claim 1, characterized in that, R1 and R2 are each independently selected from any one of hydroxyl, carboxyl, amino, amide, and hydroxylamine groups. The liquid encapsulation composition comprises, by weight, the following: 90-99.9 parts by weight of the aforementioned telescopic polymer; 0.05 to 5 parts by weight of crosslinking agent; and 0.05 to 5 parts by weight of crosslinking agent.
14. The liquid encapsulation composition according to claim 1, characterized in that, Both R1 and R2 are epoxy groups. The liquid encapsulation composition comprises, by weight, the following components: 85-99.9 parts by weight of the aforementioned telechelic polymer; 0.09 to 14.5 parts by weight of curing agent; and 0.01~0.5 parts by weight of crosslinking agent.
15. The liquid encapsulation composition according to claim 1, characterized in that, The viscosity of the liquid encapsulation composition at 25°C is 2000~8000 mPa·s.
16. A method for encapsulating a photovoltaic module, the encapsulation method comprising: Step S1: Mix the components of the encapsulation composition and degas them to prepare an encapsulation solution; Step S2 involves disposing the encapsulation liquid between the upper substrate, the battery cell unit, and the lower substrate to form an encapsulation pre-form. And step S3, degassing and curing the encapsulation preform to obtain a photovoltaic module, characterized in that the encapsulation composition is the liquid encapsulation composition according to any one of claims 1 to 15.
17. A photovoltaic module, the photovoltaic module comprising a lower substrate, a solar cell unit, and an upper substrate, wherein the pores between the lower substrate, the solar cell unit, and the upper substrate are filled with encapsulating adhesive, characterized in that, The encapsulating adhesive is formed by curing the liquid encapsulating composition according to any one of claims 1 to 15.
Citation Information
Patent Citations
Photovoltaic packaging adhesive film
CN106366986A
A liquid rubber photovoltaic encapsulation composition, encapsulation method, and photovoltaic module.
CN114933873A
Pressure sensitive structural adhesives and sealants based on telechelic / heterotelechelic polymers with dual cure systems
CN1160416A