A AlCrVTiSiCN / AlCrN / CrN multilayer composite coating and preparation method thereof and tool
Through the design of AlCrVTiSiCN/AlCrN/CrN multi-layer composite coating, the problem of insufficient hardness and wear resistance of traditional cutting tools is solved, and the improvement of high hardness, toughness and thermal stability is achieved, which is suitable for modern high-precision machining needs.
Patent Information
- Application Number
- CN202311647514.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-04
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-12-04
AI Technical Summary
Traditional cutting tools have problems with insufficient hardness, toughness and wear resistance in terms of machining accuracy and handling of difficult-to-machine materials. Although the AlCrTiSiN coating is excellent, its hardness, toughness and friction resistance still need to be improved.
The AlCrVTiSiCN/AlCrN/CrN multi-layer composite coating is used to form a nanocomposite structure by alternately depositing CrN transition layers and AlCrN and AlCrVTiSiCN layers. V and C elements are introduced to improve hardness and toughness, and the high adhesion and thermal properties of the CrN layer are used. Stability and enhanced membrane-based bonding force.
It achieves higher hardness, elastic modulus, toughness and film-based bonding force, improves the thermal stability and anti-friction performance of the coating, and enhances the overall performance of the tool.
Smart Images

Figure CN117568747B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of tool coatings, and in particular to an AlCrVTiSiCN / AlCrN / CrN multilayer composite coating and a preparation method thereof and a tool. Background Art
[0002] With the continuous innovation in the modern industrial field and the continuous iteration of mechanical parts, the market's requirements for the hardness, toughness, life, and processing accuracy of mechanical parts are gradually increasing. Traditional tools have gradually been unable to meet the existing processing accuracy requirements and the processing requirements of difficult-to-process materials. With the rapid development of dry cutting, the emergence of PVD hard coatings has greatly made up for this deficiency. Tool coating technology can be divided into multi-element coatings, gradient coatings, nano-composite coatings, nano-multilayer coatings, etc. over time, and the performance of its coatings has also steadily improved and is used in various cutting processing environments.
[0003] AlCrTiSiN coating is also one of the coatings with better mechanical properties in all aspects, but its hardness, toughness, friction resistance and bonding strength need to be further improved.
[0004] In view of this, the present invention is proposed. Summary of the invention
[0005] The object of the present invention is to provide an AlCrVTiSiCN / AlCrN / CrN multilayer composite coating and a preparation method and a cutting tool thereof. The multilayer composite coating has good hardness and elastic modulus, strong toughness, film-base bonding strength and thermal stability.
[0006] In order to achieve the above object, the present invention provides the following technical solutions:
[0007] The present invention provides an AlCrVTiSiCN / AlCrN / CrN multilayer composite coating, comprising a CrN transition layer and a wear-resistant layer deposited in sequence on a substrate, wherein the wear-resistant layer is formed by alternately cyclically depositing an AlCrN layer and an AlCrVTiSiCN layer, and the topmost surface of the wear-resistant layer is an AlCrVTiSiCN layer.
[0008] Furthermore, in the CrN transition layer, in terms of atomic percentage, Cr: 45-50%; N: 50-55%;
[0009] And / or, in the AlCrN layer, by atomic percentage, Al: 26-28%, Cr: 12-14%, N: 58-60%;
[0010] And / or, in the AlCrVTiSiCN layer, calculated by atomic percentage, Al: 13.5-14.5%; Cr: 2-3%; V: 12.5-13.5%; Ti: 13-14%; Si: 2.5-3.5%; C: 12.5-13.5%; N: 35-45%.
[0011] Further, the CrN coating is a transition layer, and the modulation ratio of the AlCrN layer and the AlCrVTiSiCN layer is 1:1;
[0012] And / or, the modulation period of the AlCrN layer and the AlCrVTiSiCN layer is 180-200nm, and the number of periods is ≥15.
[0013] Furthermore, the AlCrVTiSiCN / AlCrN / CrN multilayer composite coating forms a nanocomposite structure coating in which the amorphous phase Si3N4 wraps the nanocrystalline phase; preferably, the nanocrystalline phase includes (Al, Cr)N phase, (Ti, Al)CN phase, VN phase, and TiN phase.
[0014] In addition, the present invention also provides a method for preparing the above-mentioned AlCrVTiSiCN / AlCrN / CrN multilayer composite coating, which is characterized by comprising the following steps:
[0015] S1. Vacuuming: The pre-treated substrate is placed on the rotating table of the coating machine, and the coating chamber is evacuated to 3×10 ﹣ 3 pa~4×10 ﹣3 Pa below, the temperature in the coating chamber is heated to 460-500℃;
[0016] S2, etching and cleaning: introduce argon gas, control the pressure in the coating chamber to 0.3-1 Pa, turn on the Ti target, and perform particle etching for 100-150 minutes;
[0017] S3, depositing a CrN transition layer: opening an argon channel and a nitrogen channel, opening a Cr target, and depositing a CrN transition layer on the surface of the substrate;
[0018] S4, depositing a wear-resistant layer: closing the Cr target and the argon channel, opening the acetylene channel, alternately introducing nitrogen and acetylene, alternately opening the AlCr target, the AlCrTiSi target and the V target, and alternately depositing an AlCrN layer and an AlCrVTiSiCN layer on the surface of the CrN transition layer;
[0019] S5. End deposition: turn off the V target, AlCrTiSi target, and AlCr target currents, turn off the nitrogen and acetylene gas channels, turn off the bias voltage, turn off the heating module, and allow the coating chamber to stand to room temperature.
[0020] Furthermore, in step S1, the pretreatment includes sequentially grinding and polishing, ultrasonic cleaning, ultrapure water cleaning and anhydrous ethanol cleaning on the surface of the substrate;
[0021] Preferably, the grinding and polishing includes first grinding the surface of the substrate with sandpaper until it is smooth and flat and then grinding it with a metallographic polishing agent.
[0022] And / or, the substrate includes any one of cemented carbide, high speed steel and corundum.
[0023] Furthermore, in step S2, the etching and cleaning process includes the following process parameters: the flow rate of the argon gas is 450 to 500 sccm, the Ti target current is 80 to 100 A, and the etching negative bias voltage is -120 to -180 V.
[0024] Furthermore, in step S3, depositing the CrN transition layer includes the following process parameters: the argon flow rate is 50-60sccm, the nitrogen flow rate is 400-500sccm, the Cr target current is 80-100A, the deposition time is 20-25min, and the thickness of the CrN transition layer is 400-500nm.
[0025] Further, in step S4, depositing the wear-resistant layer includes the following process parameters: alternating nitrogen flow rate of 400-500 sccm, acetylene flow rate of 100-120 sccm, AlCr target current of 80-100 A, AlCrTiSi target current of 80-100 A, V target current of 80-100 A;
[0026] And / or, in the step S4, the bias voltage is turned on to -80 to -120 V, the pressure in the coating chamber is adjusted to 0.8 to 1.0 Pa, and the AlCrN layer and the AlCrVTiSiCN layer are alternately deposited;
[0027] And / or, the total deposition time of the wear-resistant layer is 180-200 min.
[0028] In addition, the present invention also provides a tool, including a tool substrate and the above-mentioned AlCrVTiSiCN / AlCrN / CrN multilayer composite coating deposited on the surface of the substrate or the AlCrVTiSiCN / AlCrN / CrN multilayer composite coating prepared by the above-mentioned preparation method.
[0029] Compared with the prior art, the technical solution of the present invention has at least the following technical effects:
[0030] (1) The AlCrVTiSiCN / AlCrN / CrN multilayer composite coating of the present invention has good hardness and elastic modulus;
[0031] (2) The AlCrVTiSiCN / AlCrN / CrN multilayer composite coating of the present invention has strong toughness and film-base bonding strength;
[0032] (3) The AlCrVTiSiCN / AlCrN / CrN coating of the present invention is a nanocomposite coating. The amorphous phase contained in the coating has the ability to prevent cracks from occurring, inhibit the movement of dislocations, and greatly improve the toughness of the coating.
[0033] (4) The present invention combines the hardness and toughness of the AlCrN coating with the high adhesion of the CrN coating on the basis of the high wear resistance and thermal stability of the AlCrVTiSiCN coating, thereby improving both the thermal stability and the bonding strength between the film layers;
[0034] (5) The present invention introduces two elements, C and V, on the basis of the AlCrTiSiN coating. The V element is introduced because the vanadium-containing nitride has excellent high-temperature friction resistance. The addition of V inhibits the growth of columnar crystals, and generates a VO2 lubricating phase during the friction process to reduce the wear rate, while showing good hardness; the C element (C2H2) is introduced because some carbon atoms have the property of being dissolved in the nitride lattice, thereby playing a role of solid solution strengthening and improving the hardness of the coating;
[0035] (6) The AlCrVTiSiCN / AlCrN / CrN coating process of the present invention has high process repeatability and good self-lubricating effect, which plays an important role in protecting the ecological environment. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. Among them:
[0037] Figure 1 It is a schematic structural diagram of the AlCrVTiSiCN / AlCrN / CrN multilayer composite coating of the present invention;
[0038] Figure 2 XRD spectrum of the AlCrVTiSiCN / AlCrN / CrN multilayer composite coating prepared in Example 1;
[0039] Figure 3 This is a surface morphology of the AlCrVTiSiCN / AlCrN / CrN multilayer composite coating prepared in Example 1;
[0040] Figure 4 This is a graph of the average friction coefficient of the AlCrVTiSiCN / AlCrN / CrN multilayer composite coating prepared in Example 1.
[0041] Explanation of the reference numerals: 1. substrate; 2. CrN transition layer; 3. AlCrN layer; 4. AlCrVTiSiCN layer. DETAILED DESCRIPTION
[0042] In order to make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme in the embodiment of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention. The process parameters of the following embodiments that do not specify specific conditions are usually based on conventional conditions.
[0043] The endpoints and any values of the ranges disclosed in the present invention are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in the present invention.
[0044] According to a first aspect of the present invention, there is provided an AlCrVTiSiCN / AlCrN / CrN multilayer composite coating, comprising a CrN transition layer 2 and a wear-resistant layer sequentially deposited on a substrate 1, wherein the wear-resistant layer is formed by alternatingly cyclically depositing an AlCrN layer 3 and an AlCrVTiSiCN layer 4, and the topmost surface of the wear-resistant layer is the AlCrVTiSiCN layer 4.
[0045] Adding C and V elements on the basis of AlCrVTiSiCN coating can form a small amount of vanadium-containing nitride, which increases the hardness, toughness, and friction resistance of the coating, but the strength of the bonding between it and the substrate is relatively low. The AlCrN coating prepared by cathode arc ion plating technology has the advantages of high hardness and strong toughness, but its thermal stability is poor and it cannot support long-term operation in an environment above 800°C. CrN, as a transition layer of many nitride coatings, has good bonding with the substrate. The present invention introduces two elements, C and V, on the basis of AlCrTiSiN coating. The introduction of V element is due to the fact that vanadium-containing nitride has excellent high-temperature friction resistance. The addition of V inhibits the growth of columnar crystals, and generates VO2 lubricating phase during the friction process to reduce the wear rate, while showing good hardness; the introduction of C element (C2H2) is due to the fact that some carbon atoms have the characteristics of solid solution in the nitride lattice, thereby playing a role of solid solution strengthening and improving the hardness of the coating. At the same time, the high wear resistance and thermal stability of AlCrVTiSiCN and the excellent hardness and toughness of AlCrN coating are fully utilized. AlCrN coating can also provide sufficient Al element in high temperature environment to generate Al2O3 film to protect the coating surface from further oxidation and maintain the hardness and thermal properties of the coating. In addition, combined with the high adhesion and other characteristics of CrN, a multi-layer composite coating structure is set up, and the obtained AlCrVTiSiCN / AlCrN / CrN multi-layer composite coating has good hardness and elastic modulus, strong toughness, film-base bonding and thermal stability.
[0046] As a preferred embodiment of the present invention, in the CrN transition layer, by atomic percentage, Cr: 45-50%; N: 50-55%;
[0047] Preferably, in the AlCrN layer, by atomic percentage, Al: 26-28%, Cr: 12-14%, N: 58-60%;
[0048] Preferably, in the AlCrVTiSiCN layer, by atomic percentage, Al: 13.5-14.5%; Cr: 2-3%; V: 12.5-13.5%; Ti: 13-14%; Si: 2.5-3.5%; C: 12.5-13.5%; N: 35-45%.
[0049] As a preferred embodiment of the present invention, the modulation ratio of the CrN coating layer, the AlCrN layer and the AlCrVTiSiCN layer is 1:1;
[0050] Preferably, the modulation period of the AlCrN layer and the AlCrVTiSiCN layer is 180-200 nm, and the number of periods is ≥ 15. More preferably, the modulation period of the AlCrN layer and the AlCrVTiSiCN layer is 200 nm, and the number of periods is 15.
[0051] As a preferred embodiment of the present invention, the AlCrVTiSiCN / AlCrN / CrN multilayer composite coating forms a nanocomposite structure coating in which an amorphous phase Si3N4 wraps a nanocrystalline phase; preferably, the nanocrystalline phase includes (Al, Cr)N phase, (Ti, Al)CN phase, VN phase, TiN phase, etc.
[0052] According to a second aspect of the present invention, there is also provided a method for preparing the above-mentioned AlCrVTiSiCN / AlCrN / CrN multilayer composite coating, comprising the following steps:
[0053] S1. Vacuuming: The pre-treated substrate is placed on the rotating table of the coating machine, and the coating chamber is evacuated to 3×10 ﹣ 3 pa~4×10 ﹣3 Pa below, the temperature in the coating chamber is heated to 460-500℃;
[0054] S2, etching and cleaning: introduce argon gas, control the pressure in the coating chamber to 0.3-1 Pa, turn on the Ti target, and perform particle etching for 100-150 minutes;
[0055] S3, depositing a CrN transition layer: opening an argon channel and a nitrogen channel, opening a Cr target, and depositing a CrN transition layer on the surface of the substrate;
[0056] S4, depositing a wear-resistant layer: closing the Cr target and the argon channel, opening the acetylene channel, alternately introducing nitrogen and acetylene, alternately opening the AlCr target, the AlCrTiSi target and the V target, and alternately depositing an AlCrN layer and an AlCrVTiSiCN layer on the surface of the CrN transition layer;
[0057] S5. End deposition: turn off the V target, AlCrTiSi target, and AlCr target currents, turn off the nitrogen and acetylene gas channels, turn off the bias voltage, turn off the heating module, and allow the coating chamber to stand to room temperature.
[0058] In the above technical solution, in step S1, the vacuuming step specifically includes: starting the roughing pump and the roughing valve to pump the pressure in the coating chamber to below 3 Pa, then starting the molecular pump, and after the molecular pump speed stabilizes, starting the fine pump and the fine valve to pump to 3×10 -3 ~4×10 -3 Turn on the heating module and raise the temperature in the coating chamber to 480°. Wait until the vacuum pressure in the furnace stabilizes at 3×10-3 ~4×10 -3 Pa, coating can begin.
[0059] As a preferred embodiment of the present invention, in step S1, the pretreatment includes polishing, ultrasonic cleaning, ultrapure water cleaning and anhydrous ethanol cleaning of the substrate surface in sequence;
[0060] Preferably, the grinding and polishing includes first grinding the surface of the substrate with sandpaper until it is smooth and flat and then grinding it with a metallographic polishing agent.
[0061] And / or, the substrate includes any one of cemented carbide, high speed steel and corundum.
[0062] As a preferred embodiment of the present invention, in step S2, the etching and cleaning includes the following process parameters: the argon gas flow rate is 450 to 500 sccm, the Ti target current is 80 to 100 A, and the etching negative bias voltage is -120 to -180 V.
[0063] As a preferred embodiment of the present invention, in step S3, depositing the CrN transition layer includes the following process parameters: the flow rate of the argon gas is 50-60sccm, the flow rate of the nitrogen gas is 400-500sccm, the Cr target current is 80-100A, the deposition time is 20-25min, and the thickness of the CrN transition layer is 400-500nm. More preferably, the deposition time is 20min, and the thickness of the CrN transition layer is 400nm.
[0064] As a preferred embodiment of the present invention, in step S4, depositing the wear-resistant layer includes the following process parameters: alternating nitrogen flow rate of 400-500sccm, acetylene flow rate of 100-120sccm, AlCr target current of 80-100A, AlCrTiSi target current of 80-100A, V target current of 80-100A;
[0065] Optionally, in step S4, the bias voltage is turned on to -80 to -120 V, the pressure in the coating chamber is adjusted to 0.8 to 1.0 Pa, and the AlCrN layer and the AlCrVTiSiCN layer are deposited alternately.
[0066] Optionally, the total deposition time of the wear-resistant layer is 180-200 min. More preferably, the total deposition time of the wear-resistant layer is 180 min.
[0067] According to the third aspect of the present invention, there is also provided a tool, comprising a tool substrate and the above-mentioned AlCrVTiSiCN / AlCrN / CrN multilayer composite coating deposited on the surface of the substrate or the AlCrVTiSiCN / AlCrN / CrN multilayer composite coating prepared by the above-mentioned preparation method.
[0068] The present invention will be further described in detail below with reference to specific embodiments and comparative examples.
[0069] Example 1
[0070] This embodiment provides a method for preparing an AlCrVTiSiCN / AlCrN / CrN multilayer composite coating, comprising the following steps:
[0071] (1) Pretreatment: Before the experiment, the substrate needs to be ground and polished. Use sandpaper (300 mesh, 600 mesh, 850 mesh, 1200 mesh, 1500 mesh) to grind the surface of the cemented carbide until it is smooth and flat without obvious defects. Then, use a metallographic polishing machine with the assistance of diamond powder to polish it to a mirror surface. After the treatment, the surface of the substrate sample must be neat and mirror-like, without obvious scratches and pits. Place the treated sample in an acetone solution for ultrasonic cleaning for 20 minutes to ensure that there is no oil stains, stains, etc. on the surface of the sample, and then clean it in ultrapure water and anhydrous ethanol for 10 minutes. Hang the treated sample on the turntable of the coating machine, wipe the dust with anhydrous ethanol again, close the furnace door, and perform vacuum treatment.
[0072] (2) Vacuuming: Open the roughing pump and roughing valve to pump the pressure in the coating chamber to below 3 Pa, then turn on the molecular pump. After the molecular pump speed stabilizes, open the fine pump and fine valve to pump to 3×10 -3 Turn on the heating module and raise the temperature in the coating chamber to 480°. Wait until the vacuum pressure in the furnace stabilizes at 3×10 -3 Pa before the coating test can be started.
[0073] (3) Etching and cleaning: the argon flow rate is 450 sccm, the pressure in the coating chamber is controlled to be 0.3 Pa, the etching target (Ti target) is turned on, the Ti target current is 80 A, the etching negative bias voltage is -120 V, and the particle etching is carried out for 120 min.
[0074] (4) Deposition of CrN transition layer: Open the argon channel and introduce 50 sccm of argon; open the nitrogen channel and introduce 500 sccm of nitrogen; turn on the Cr target and set the target current to 100 A to deposit a CrN coating on the substrate surface with a coating thickness of 400 nm;
[0075] (5) AlCrVTiSiCN / AlCrN deposition: close the Cr target and argon channel, open the acetylene channel, alternately introduce nitrogen with a flow rate of 500 sccm and acetylene with a flow rate of 120 sccm, alternately open the AlCr target with a target current of 100A, the AlCrTiSi target with a target current of 100A, and the V target with a target current of 100A. Turn on the bias voltage of -120V, adjust the throttle valve to make the pressure in the coating chamber 0.8Pa, alternately deposit AlCrVTiSiCN / AlCrN coatings, the last coating is the AlCrVTiSiCN layer, the number of alternating cycles is 15 times, the single tempering cycle is 200nm, and the total thickness of the alternating coating is 3μm.
[0076] (6) End of deposition: turn off the V, AlCrTiSi, and AlCr target currents, turn off the nitrogen and acetylene gas channels, turn off the bias voltage, turn off the heating module, and allow the coating chamber to stand to room temperature.
[0077] The XRD pattern of the AlCrVTiSiCN / AlCrN / CrN multilayer composite coating prepared in this embodiment is as follows: Figure 2 As shown in the figure, the layer is polycrystalline, mostly face-centered cubic structure, and the phase composition is mainly (Al, Cr) N phase, TiN phase, VN phase, (Al, Cr) CN phase. There is no Si3N4 phase in the spectrum, which may be due to the crystallization temperature of silicon nitride is above 1000℃, while the temperature of the experimental preparation coating is 480℃, and Si3N4 is not crystallized. It may be that Si3N4 exists in the form of amorphous phase inside the coating. The phases in the spectrum all grow preferentially along the (211) crystal plane. The coating is a nanocomposite structure, the nanocrystals are wrapped by Si3N4 amorphous, and the grain size is small, which will inhibit the generation of dislocations and prevent the crack propagation caused by grain boundary enhancement and grain boundary sliding inhibition. It has a good effect on the hardness, toughness and thermal stability of the coating, and is suitable for tools, mechanical molds and parts.
[0078] The surface morphology of the AlCrVTiSiCN / AlCrN / CrN multilayer composite coating prepared in this embodiment is shown in FIG. Figure 3 As shown in the figure, the surface of the multi-layer composite coating is relatively flat and dense, but there are still some large particles and pits, which are caused by the arc ion plating equipment. When the target is energized, the sputtered particles are supported by the bias voltage, and a large number of droplets are sputtered to the surface of the substrate for deposition, thereby forming large particles, and the unevenly distributed surface stress promotes the formation of pits.
[0079] Example 2
[0080] This embodiment provides a method for preparing an AlCrVTiSiCN / AlCrN / CrN multilayer composite coating, comprising the following steps:
[0081] (1) Pretreatment: Before the experiment, the substrate needs to be ground and polished. Use sandpaper (300 mesh, 600 mesh, 850 mesh, 1200 mesh, 1500 mesh) to grind the surface of the high-speed steel until it is smooth and flat without obvious defects. Then, use a metallographic polishing machine with the assistance of diamond powder to polish it to a mirror surface. After the treatment, the surface of the substrate sample must be neat and mirror-like, without obvious scratches and pits. Place the treated sample in an acetone solution for ultrasonic cleaning for 20 minutes to ensure that there is no oil stains, stains, etc. on the surface of the sample, and then clean it in ultrapure water and anhydrous ethanol for 10 minutes. Hang the treated sample on the turntable of the coating machine, wipe the dust with anhydrous ethanol again, close the furnace door, and perform vacuum treatment.
[0082] (2) Vacuuming: Open the roughing pump and roughing valve to pump the pressure in the coating chamber to below 3 Pa, then turn on the molecular pump. After the molecular pump speed stabilizes, open the fine pump and fine valve to pump to 3×10 -3 Turn on the heating module and raise the temperature in the coating chamber to 460°. Wait until the vacuum pressure in the furnace stabilizes at 3×10 -3 Pa before the coating test can be started.
[0083] (3) Etching and cleaning: the argon flow rate is 500 sccm, the pressure in the coating chamber is controlled to be 0.3 Pa, the etching target (Ti target) is turned on, the Ti target current is 80 A, the etching negative bias voltage is -150 V, and the particle etching is carried out for 100 min.
[0084] (4) Deposition of CrN transition layer: Open the argon channel and introduce 60 sccm of argon; open the nitrogen channel and introduce 400 sccm of nitrogen; open the Cr target and set the target current to 80 A to deposit a CrN coating on the substrate surface with a coating thickness of 500 nm;
[0085] (5) AlCrVTiSiCN / AlCrN deposition: close the Cr target and argon gas channel, open the acetylene channel, alternately introduce nitrogen with a flow rate of 400 sccm and acetylene with a flow rate of 100 sccm, alternately open the AlCr target with a target current of 80A, the AlCrTiSi target with a target current of 80A, and the V target with a target current of 80A. Turn on the bias voltage of -120V, adjust the throttle valve to make the pressure in the coating chamber 1.0Pa, and alternately deposit AlCrVTiSiCN / AlCrN coatings. The last coating is the AlCrVTiSiCN layer. The number of alternating cycles is 18 times, the single tempering cycle is 180nm, and the total thickness of the alternating coating is 3.24μm.
[0086] (6) End of deposition: turn off the V, AlCrTiSi, and AlCr target currents, turn off the nitrogen and acetylene gas channels, turn off the bias voltage, turn off the heating module, and allow the coating chamber to stand to room temperature.
[0087] Example 3
[0088] This embodiment provides a method for preparing an AlCrVTiSiCN / AlCrN / CrN multilayer composite coating, comprising the following steps:
[0089] (1) Pretreatment: Before the experiment, the substrate needs to be ground and polished. Use sandpaper (300 mesh, 600 mesh, 850 mesh, 1200 mesh, 1500 mesh) to grind the surface of the corundum until it is smooth and flat without obvious defects. Then, use a metallographic polishing machine with the assistance of diamond powder to polish it to a mirror surface. After the treatment, the surface of the substrate sample must be neat and mirror-like, without obvious scratches and pits. Place the treated sample in an acetone solution for ultrasonic cleaning for 20 minutes to ensure that there is no oil stains, stains, etc. on the surface of the sample, and then clean it in ultrapure water and anhydrous ethanol for 10 minutes. Hang the treated sample on the turntable of the coating machine, wipe the dust with anhydrous ethanol again, close the furnace door, and perform vacuum treatment.
[0090] (2) Vacuuming: Open the roughing pump and roughing valve to pump the pressure in the coating chamber to below 3 Pa, then turn on the molecular pump. After the molecular pump speed stabilizes, open the fine pump and fine valve to pump to 4×10 -3 Turn on the heating module and raise the temperature in the coating chamber to 500°. Wait until the vacuum pressure in the furnace stabilizes at 4×10 -3 Pa before the coating test can be started.
[0091] (3) Etching and cleaning: the argon flow rate is 480 sccm, the pressure in the coating chamber is controlled to be 1 Pa, the etching target (Ti target) is turned on, the Ti target current is 80 A, the etching negative bias voltage is -150 V, and the particle etching is carried out for 150 min.
[0092] (4) Deposition of CrN transition layer: Open the argon channel and introduce 55 sccm of argon; open the nitrogen channel and introduce 450 sccm of nitrogen; turn on the Cr target and set the target current to 90 A to deposit a CrN coating on the substrate surface with a coating thickness of 450 nm;
[0093] (5) AlCrVTiSiCN / AlCrN deposition: close the Cr target and argon gas channel, open the acetylene channel, alternately introduce nitrogen with a flow rate of 450sccm and acetylene with a flow rate of 110sccm, alternately open the AlCr target with a target current of 90A, the AlCrTiSi target with a target current of 90A, and the V target with a target current of 90A. Turn on the bias voltage of -120V, adjust the throttle valve to make the pressure in the coating chamber 0.8Pa, and alternately deposit AlCrVTiSiCN / AlCrN coatings. The last coating is the AlCrVTiSiCN layer. The number of alternating cycles is 20 times, the single tempering cycle is 200nm, and the total thickness of the alternating coating is 4μm.
[0094] (6) End of deposition: turn off the V, AlCrTiSi, and AlCr target currents, turn off the nitrogen and acetylene gas channels, turn off the bias voltage, turn off the heating module, and allow the coating chamber to stand to room temperature.
[0095] Comparative Example 1
[0096] This comparative example provides a method for preparing an AlCrVTiSiCN / AlCrN / CrN composite coating, comprising the following steps:
[0097] 1. Pretreatment: The surface of the substrate sample was polished with sandpaper (300 mesh, 600 mesh, 850 mesh, 1200 mesh, 1500 mesh) in sequence, and then polished to a mirror surface on a metallographic grinder. Ultrasonic cleaning was performed in acetone, ultrapure water, and anhydrous ethanol solutions.
[0098] 2. Vacuuming: Turn on the rough pump and rough valve, pump the pressure in the coating chamber to below 3Pa, then turn on the molecular pump, wait until the molecular pump speed is stable, then turn on the fine pump and fine valve, and pump to below 4×10-3Pa. Turn on the heating module, raise the temperature in the coating chamber to 500°, and wait until the vacuum pressure in the furnace is stable below 4×10-3Pa before starting the coating test.
[0099] 3. Etching and cleaning: the argon flow rate is 480sccm, the pressure in the coating chamber is controlled to be 1Pa, the etching target (Ti target) is turned on, the Ti target current is 80A, the etching negative bias voltage is -150V, and the particle etching is carried out for 150min.
[0100] 4. Deposition of CrN transition layer and AlCrN coating: the argon flow rate is 40sccm, the nitrogen flow rate is 250sccm, the throttle valve is adjusted to ensure that the deposition pressure in the coating chamber is 0.8Pa, the pulse bias is set to -80V, the Cr target current is 80A, the deposition time is 20min, the coating thickness is 400nm, the Cr target is turned off, the AlCr target is turned on, the target current is 90A, the nitrogen flow rate is 500sccm, and the AlCrN coating is deposited for 90min.
[0101] 5. Deposition of AlCrVTiSiCN: The nitrogen flow rate is 500sccm, the acetylene flow rate is 120sccm, and the throttle valve is adjusted to ensure that the deposition pressure in the coating chamber is 2.2Pa. Set the pulse bias voltage to -120V, the AlCrTiSi target current to 100A, the V target current to 100A, and the deposition time of AlCrVTiSiCN to 90min, so that the total thickness of the AlCrVTiSiCN layer and the AlCrN layer is 3μm.
[0102] Comparative Example 2
[0103] The parameters of the remaining steps are consistent with those of Example 1, except that the AlCrN layer is missing. The specific steps are:
[0104] (5) AlCrVTiSiCN deposition: close the Cr target and argon channel, open the acetylene channel, AlCrTiSi target, target current is 100A, V target, target current is 100A. Turn on the bias voltage to -120V, adjust the throttle valve so that the pressure in the coating chamber is 2.2Pa, the deposition time is 120min, and the coating thickness is 3μm.
[0105] Comparative Example 3
[0106] The parameters of the remaining steps are consistent with those of Example 1, except that an AlCrTiSiN layer is used to replace the AlCrVTiSiCN layer. The specific steps are as follows:
[0107] (5) AlCrTiSiN / AlCrN deposition: close the Cr target and argon gas channel, and alternately open the AlCr target with a target current of 100 A and the AlCrTiSi target with a target current of 100 A. Turn on the bias voltage of -120 V, adjust the throttle valve to make the pressure in the coating chamber 0.8 Pa, and alternately deposit AlCrTiSiN / AlCrN coatings. The last coating is the AlCrTiSiN layer. The number of alternating cycles is 15 times, the single tempering cycle is 200 nm, and the total thickness of the alternating coating is 3 μm.
[0108] Comparative Example 4
[0109] The parameters of the remaining steps are consistent with those of Example 1, except that an AlCrTiSiCN layer is used instead of an AlCrVTiSiCN layer. The specific steps are:
[0110] (5) AlCrTiSiCN / AlCrN deposition: The Cr target and the argon channel were closed, and the acetylene channel was opened. Nitrogen with a flow rate of 500 sccm and acetylene with a flow rate of 120 sccm were alternately introduced. The AlCr target was alternately opened with a target current of 100 A and the AlCrTiSi target was alternately opened with a target current of 100 A. The bias voltage was turned on to -120 V, and the throttle valve was adjusted to make the pressure in the coating chamber 0.8 Pa. AlCrTiSiCN / AlCrN coatings were alternately deposited. The last coating was the AlCrTiSiCN layer. The number of alternating cycles was 15 times, and the single tempering cycle was 200 nm. The total thickness of the alternating coatings was 3 μm.
[0111] Comparative Example 5
[0112] The parameters of the remaining steps are consistent with those of Example 1, except that an AlCrVTiSiN layer is used to replace the AlCrVTiSiCN layer. The specific steps are as follows:
[0113] (5) AlCrTiSiCN / AlCrN deposition: close the Cr target and argon gas channel, and alternately open the AlCr target with a target current of 100 A, the AlCrTiSi target with a target current of 100 A, and the V target with a target current of 100 A. Turn on the bias voltage of -120 V, adjust the throttle valve to make the pressure in the coating chamber 0.8 Pa, and alternately deposit AlCrVTiSiN / AlCrN coatings. The last coating is the AlCrVTiSiN layer. The number of alternating cycles is 15 times, the single tempering cycle is 200 nm, and the total thickness of the alternating coatings is 3 μm.
[0114] The coatings obtained in Examples 1-3 and Comparative Examples 1-5 were subjected to performance tests, wherein the bonding force was measured by a large load scratch tester, and the elastic modulus and hardness were measured by a nanoindentation method. The specific test results are shown in Table 1:
[0115] Table 1
[0116]
[0117]
[0118] It can be seen from Table 1 that the AlCrVTiSiCN / AlCrN / CrN multilayer composite coatings prepared in Examples 1-3 have greatly improved hardness and elastic modulus compared with the coatings prepared in Comparative Examples 1-5, and the ratio of hardness to elastic modulus can characterize the toughness of the coating material to a certain extent. The larger the ratio, the better the toughness of the coating material. The H / E value of the AlCrVTiSiCN / AlCrN / CrN coatings prepared in Examples 1-3 is higher than that of Comparative Examples 1-5, indicating that the AlCrVTiSiCN / AlCrN / CrN nanocomposite coatings prepared in the present invention have improved hardness while taking into account the coordination of toughness; the bonding strength of the AlCrVTiSiCN / AlCrN / CrN coatings prepared in Examples 1-3 is also higher than that of Comparative Examples 1-5, which is due to the strong film-base bonding strength between the CrN layer and the substrate.
[0119] In addition, the friction coefficients of the multilayer composite coatings obtained in Example 1 and Comparative Example 3 are compared (measured by a high temperature friction and wear tester). Figure 4 As shown, the AlCrVTiSiCN / AlCrN / CrN multilayer composite coating prepared in Example 1 has much higher anti-friction ability than that in Comparative Example 3. This is because the addition of the V element enables the nano-coating system to continuously generate a lubricating phase during the friction test, thereby reducing the friction coefficient and improving thermal stability.
[0120] In summary, the present invention uses arc ion plating technology to deposit AlCrVTiSiCN / AlCrN / CrN coating on the surface of the substrate, and the coating surface is more dense and smooth; the structure of the composite coating causes co-epitaxial growth between the coatings, and the organizational structure of nanocrystals embedded in amorphous Si3N4 in the AlCrVTiSiCN / AlCrN / CrN coating enables the coating to have excellent hardness, bonding strength, thermal stability, and resistance to friction and wear. The addition of V element in the AlCrVTiSiCN coating allows the coating to react with oxygen in the air to generate VO phase oxide during the friction and wear process. This structure has a sliding plane and has an excellent lubrication effect. The addition of the CrN layer makes the bonding between the coating and the substrate tighter, greatly improving the film-base bonding strength.
[0121] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. An AlCrVTiSiCN / AlCrN / CrN multilayer composite coating, characterized in that: It includes a CrN transition layer and a wear-resistant layer deposited in sequence on a substrate, wherein the wear-resistant layer is formed by alternately depositing an AlCrN layer and an AlCrVTiSiCN layer, and the topmost surface of the wear-resistant layer is an AlCrVTiSiCN layer; In the AlCrVTiSiCN layer, by atomic percentage, Al: 13.5-14.5%; Cr: 2-3%; V: 12.5-13.5%; Ti: 13-14%; Si: 2.5-3.5%; C: 12.5-13.5%; N: 35-45%; the sum of the above elements is 100%; The AlCrVTiSiCN / AlCrN / CrN multilayer composite coating forms a nano-composite structure coating in which an amorphous phase Si3N4 wraps a nano-crystalline phase; the nano-crystalline phase includes an (Al, Cr)N phase, a (Ti, Al)CN phase, a VN phase, and a TiN phase.
2. The AlCrVTiSiCN / AlCrN / CrN multilayer composite coating according to claim 1, characterized in that: In the CrN transition layer, in terms of atomic percentage, Cr: 45-50%; N: 50-55%; And / or, in the AlCrN layer, calculated by atomic percentage, Al: 26-28%, Cr: 12-14%, N: 58-60%.
3. The AlCrVTiSiCN / AlCrN / CrN multilayer composite coating according to claim 1, characterized in that: The CrN coating is a transition layer, and the modulation ratio of the AlCrN layer and the AlCrVTiSiCN layer is 1:1; And / or, the modulation period of the AlCrN layer and the AlCrVTiSiCN layer is 180-200nm, and the number of periods is ≥15.
4. A method for preparing the AlCrVTiSiCN / AlCrN / CrN multilayer composite coating according to any one of claims 1 to 3, characterized in that: The following steps are involved: S1. Vacuuming: The pre-treated substrate is placed on the rotating table of the coating machine, and the coating chamber is evacuated to 3×10 ﹣3 pa~4×10 ﹣3 Pa below, the temperature in the coating chamber is heated to 460~500℃; S2, etching and cleaning: introduce argon gas, control the pressure in the coating chamber to 0.3~1pa, turn on the Ti target, and perform particle etching for 100-150min; S3, depositing a CrN transition layer: opening an argon channel and a nitrogen channel, opening a Cr target, and depositing a CrN transition layer on the surface of the substrate; S4, depositing a wear-resistant layer: closing the Cr target and the argon channel, opening the acetylene channel, alternately introducing nitrogen and acetylene, alternately opening the AlCr target, the AlCrTiSi target and the V target, and alternately depositing an AlCrN layer and an AlCrVTiSiCN layer on the surface of the CrN transition layer; S5. End deposition: turn off the V target, AlCrTiSi target, and AlCr target currents, turn off the nitrogen and acetylene gas channels, turn off the bias voltage, turn off the heating module, and allow the coating chamber to stand to room temperature.
5. The preparation method according to claim 4, characterized in that: In the step S1, the pretreatment includes polishing, ultrasonic cleaning, ultrapure water cleaning and anhydrous ethanol cleaning of the substrate surface in sequence; And / or, the substrate includes any one of cemented carbide, high speed steel and corundum.
6. The preparation method according to claim 5, characterized in that: The grinding and polishing includes first grinding the surface of the substrate with sandpaper until it is smooth and flat and then grinding it with a metallographic polishing agent.
7. The preparation method according to claim 4, characterized in that: In the step S2, the etching and cleaning process includes the following process parameters: the flow rate of the argon gas is 450-500 sccm, the Ti target current is 80-100 A, and the etching negative bias voltage is -120--180 V.
8. The preparation method according to claim 4, characterized in that: In the step S3, the deposition of the CrN transition layer includes the following process parameters: the flow rate of the argon gas is 50-60 sccm, the flow rate of the nitrogen gas is 400-500 sccm, the Cr target current is 80-100 A, the deposition time is 20-25 min, and the thickness of the CrN transition layer is 400-500 nm.
9. The preparation method according to claim 4, characterized in that: In the step S4, the deposition of the wear-resistant layer includes the following process parameters: the flow rate of nitrogen gas is 400-500 sccm, the flow rate of acetylene is 100-120 sccm, the target current of AlCr is 80-100A, the target current of AlCrTiSi is 80-100A, and the target current of V is 80-100A; And / or, in the step S4, the bias voltage is turned on to -80~-120V, the pressure in the coating chamber is adjusted to 0.8~1.0Pa, and the AlCrN layer and the AlCrVTiSiCN layer are alternately deposited; And / or, the total deposition time of the wear-resistant layer is 180-200 min.
10. A cutting tool, characterized in that: It comprises a tool substrate and an AlCrVTiSiCN / AlCrN / CrN multilayer composite coating as described in any one of claims 1 to 3 deposited on the surface of the substrate, or an AlCrVTiSiCN / AlCrN / CrN multilayer composite coating prepared by the preparation method as described in any one of claims 4 to 9.
Citation Information
Cited By
Silicon-selective modulation thick-period multilayer nitride coating, and preparation method and application thereof