Lead oxide-zinc oxide resistor sheet side insulation material composition, insulation material and its preparation method, and resistor sheet preparation method.

By using a composition of PbO, B2O3, ZnO, Al2O3, SiO2, and AgO to form an insulating glaze, the problems of side insulation flashover and moisture absorption of ZnO resistor sheets under lightning strikes are solved, improving insulation strength and moisture resistance, and ensuring the safety of power equipment.

CN117571267BActive Publication Date: 2026-11-17湖南防灾科技有限公司
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310068008.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-14
Publication Date
2026-11-17
Estimated Expiration
2043-01-14

AI Technical Summary

Technical Problem

Existing ZnO resistance sheets are prone to lateral insulation flashover under lightning strikes, and are susceptible to moisture absorption in the air, which leads to a decline in insulation performance and makes them unable to effectively protect electrical equipment.

Method used

A composition containing PbO, B2O3, ZnO, Al2O3, SiO2, and AgO is used as the insulating material, and an insulating glaze is formed by coating and sintering with an atomizing air compressor to improve the insulation strength.

Benefits of technology

The insulation strength of the side insulation material of the resistor sheet is improved, the moisture resistance is enhanced, side insulation flashover is prevented under lightning strikes, and the safe and stable operation of the power grid is ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117571267B_ABST
    Figure CN117571267B_ABST
Patent Text Reader

Abstract

This invention relates to the field of power, and discloses a lead oxide-zinc oxide resistor side insulation material composition, the insulation material, its preparation method, and a method for preparing the resistor sheet. The composition contains a binder and ingredients, wherein the ingredients contain the following components: based on the total mass of the ingredients, the content of PbO is 60-80 wt%, the content of B2O3 is 5-20 wt%, the content of ZnO is 5-10 wt%, the content of Al2O3 is 5-10 wt%, the content of SiO2 is 3-7 wt%, and the content of AgO is 1-3 wt%. This invention provides a resistor sheet side insulation material with high resistivity, which is not prone to side insulation flashover under lightning strikes and is not easily affected by moisture in air.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of electric power, specifically to a composition of side insulating material for lead oxide-zinc oxide resistor sheets, insulating materials and their preparation methods, and a method for preparing resistor sheets. Background Technology

[0002] Zinc oxide surge arresters are key devices in power systems used to suppress lightning overvoltages and protect power equipment from lightning strike damage. Their core component is a zinc oxide (ZnO) varistor. However, existing ZnO resistors are prone to side insulation flashover under lightning strikes due to poor side insulation, which can cause the ZnO surge arrester to explode and jeopardize the safe and stable operation of the power grid.

[0003] Existing ZnO resistor elements typically have silicone rubber or similar coatings applied to the sides, resulting in insufficient insulation strength and a high risk of side insulation flashover during lightning strikes. Furthermore, since surge arresters operate outdoors for extended periods, the side insulation of the zinc oxide resistor elements is prone to moisture absorption, leading to ZnO resistor element failure. Consequently, zinc oxide surge arresters are susceptible to side insulation flashover under lightning strikes, rendering them ineffective for lightning protection.

[0004] Scholars both at home and abroad have conducted relevant research on the side insulation problem of ZnO resistor sheets.

[0005] CN106587985A discloses a formula and process for a high-resistivity layer of a zinc oxide resistive sheet, but its high-resistivity layer material is thin and can only withstand 2ms square wave energy. It is prone to side insulation flashover under 4 / 10μs impact current.

[0006] CN113045203A discloses a formula for side insulating glaze, but its main components are substances such as Sb2O3, which will form spinel after sintering. Spindle is easily affected by moisture in the air, which leads to a reduction in side insulation.

[0007] Therefore, based on the current research status, it is of great significance to provide a side insulation material for resistor sheets that has high resistivity, is not prone to side insulation flashover under lightning strikes, is not easily affected by moisture in air, and has good side insulation performance. Summary of the Invention

[0008] The purpose of this invention is to overcome the problem in the prior art that the resistivity of the side insulation material of the resistor sheet is low, and side insulation flashover is prone to occur under lightning strike.

[0009] To achieve the above objectives, a first aspect of the present invention provides a composition for the side insulation material of lead oxide-zinc oxide resistor sheets, the composition comprising an adhesive and ingredients, said ingredients comprising the following components:

[0010] PbO, B2O3, ZnO, Al2O3, SiO2, AgO;

[0011] Based on the total mass of the ingredients, the content of PbO is 60-80 wt%, the content of B2O3 is 5-20 wt%, the content of ZnO is 5-10 wt%, the content of Al2O3 is 5-10 wt%, the content of SiO2 is 3-7 wt%, and the content of AgO is 1-3 wt%.

[0012] The weight ratio of the adhesive to the ingredients is 1:0.9-1.2.

[0013] A second aspect of the present invention provides a method for preparing a side insulating material for a resistor sheet, the method being carried out using the composition described in the first aspect, comprising:

[0014] (1) Mix the ingredients and the binder in the first mixing to obtain mixture I;

[0015] (2) Grind the mixture I to obtain the insulating material on the side of the resistor sheet;

[0016] Based on the total mass of the ingredients, the content of PbO is 60-80 wt%, the content of B2O3 is 5-20 wt%, the content of ZnO is 5-10 wt%, the content of Al2O3 is 5-10 wt%, the content of SiO2 is 3-7 wt%, and the content of AgO is 1-3 wt%.

[0017] The weight ratio of the adhesive to the ingredients is 1:0.9-1.2.

[0018] A third aspect of the present invention provides a side insulating material for a resistor sheet prepared by the method described in the second aspect.

[0019] A fourth aspect of the present invention provides a method for preparing a resistor sheet, the method being carried out using the side insulating material of the resistor sheet described in the third aspect, comprising:

[0020] SS1. Using an atomizing air compressor, the insulating material on the side of the resistor sheet is coated onto the side of the raw material resistor sheet to obtain resistor sheet I. The pressure of the atomizing air compressor is 3-5 MPa, and the coating thickness is 100-300 μm.

[0021] SS2. The resistor I is sintered at 20-550℃ to obtain a product resistor with insulating glaze on the side.

[0022] The resistor side insulation material provided by this invention has high insulation strength and stronger moisture resistance compared to traditional organic insulating adhesives. It solves the problems of insufficient side insulation strength of ZnO resistor sheets and easy side insulation flashover under lightning strikes in the prior art. Attached Figure Description

[0023] Figure 1 This is the microstructure inside the resistor chip provided by the present invention. Detailed Implementation

[0024] The endpoints and any values ​​of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of the various ranges, the endpoint values ​​of the various ranges and individual point values, and individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.

[0025] As previously described, a first aspect of the present invention provides a composition for the side insulation material of lead oxide-zinc oxide resistor sheets, the composition comprising an adhesive and ingredients, the ingredients comprising the following components:

[0026] PbO, B2O3, ZnO, Al2O3, SiO2, AgO;

[0027] Based on the total mass of the ingredients, the content of PbO is 60-80 wt%, the content of B2O3 is 5-20 wt%, the content of ZnO is 5-10 wt%, the content of Al2O3 is 5-10 wt%, the content of SiO2 is 3-7 wt%, and the content of AgO is 1-3 wt%.

[0028] The weight ratio of the adhesive to the ingredients is 1:0.9-1.2.

[0029] Preferably, the adhesive is selected from at least one of ethanol, butyl carbitol, and ethyl cellulose.

[0030] In a preferred embodiment, the adhesive is ethanol, butyl carbitol and ethyl cellulose in a weight ratio of 1:0.05-0.1:0.05-0.1.

[0031] As previously described, a second aspect of the present invention provides a method for preparing a side insulating material for a resistor sheet, the method being carried out using the composition described in the first aspect, comprising:

[0032] (1) Mix the ingredients and the binder in the first mixing to obtain mixture I;

[0033] (2) Grind the mixture I to obtain the insulating material on the side of the resistor sheet;

[0034] Based on the total mass of the ingredients, the content of PbO is 60-80 wt%, the content of B2O3 is 5-20 wt%, the content of ZnO is 5-10 wt%, the content of Al2O3 is 5-10 wt%, the content of SiO2 is 3-7 wt%, and the content of AgO is 1-3 wt%.

[0035] The weight ratio of the adhesive to the ingredients is 1:0.9-1.2.

[0036] According to a preferred embodiment, the method of the present invention further includes: in step (1), the adhesive is ethanol, butyl carbitol, and ethyl cellulose, and the method further includes preparing the adhesive using a step comprising the following operations:

[0037] S1. Under stirring conditions, ethanol and butylcarbidol are mixed for a second time for 30-60 minutes to obtain mixture II;

[0038] S2. Under stirring conditions, the mixture II is mixed with ethyl cellulose for a third time for 60-120 minutes to obtain an adhesive;

[0039] The weight ratio of the ethanol, the butyl carbitol, and the ethyl cellulose is 1:0.05-0.1:0.05-0.1.

[0040] Preferably, in step S1, the conditions for the second mixing are at least: rotation speed of 360-420 rpm and temperature of 80-90℃.

[0041] In a preferred embodiment, in step S2, the conditions for the third mixing are at least: a rotational speed of 360-420 rpm and a temperature of 80-90°C.

[0042] It should be noted that the present invention does not have specific requirements for the method of achieving the temperature conditions in the preparation of the adhesive; for example, a water bath can be used.

[0043] To ensure more complete dissolution of ethyl cellulose, preferably, in step S2 of preparing the adhesive, the ethyl cellulose is added to the mixture II in 3-5 batches for a third mixing.

[0044] According to a preferred embodiment, step S2 of preparing the adhesive further includes: mixing the mixture II with ethyl cellulose for the third time, letting it stand for 12-24 hours, and then taking the supernatant as the adhesive.

[0045] According to a preferred embodiment, in step (1), the conditions for the first mixing include: being carried out under stirring conditions, with a stirring speed of 360-420 rpm, a stirring time of 30-120 min, and a temperature of 80-90℃.

[0046] In a preferred embodiment, the first mixing operation includes: in step (1), first mixing and contacting each component in the ingredients for 30-60 minutes to obtain the ingredients, and then mixing the ingredients with the adhesive for 30-60 minutes to obtain mixture I.

[0047] Preferably, in step (2), the grinding conditions include: a rotation speed of 360-420 rpm, a grinding time of 24-72 h, and a mass ratio of the total mass of the grinding balls to the mass of the ingredients being 1:1-2, and the diameter of each grinding ball being 1-20 mm.

[0048] According to a preferred embodiment, the grinding ball is selected from at least one of agate and zirconium balls.

[0049] More preferably, the grinding ball is a zirconium ball.

[0050] Preferably, the diameter of the grinding balls is divided into 1-3 levels.

[0051] More preferably, the diameter of the grinding balls is divided into three levels: small (1-4 mm), medium (5-9 mm), and large (10-15 mm); and the ratio of the number of grinding balls of the three levels (large, medium, and small) is 10-30%: 20-30%: 50-70%.

[0052] Preferably, the grinding in this invention is performed using a ball mill.

[0053] As previously stated, the third aspect of the present invention provides a side insulating material for a resistor sheet prepared by the method described in the second aspect.

[0054] As previously described, a fourth aspect of the present invention provides a method for preparing a resistor sheet, the method being carried out using the resistor sheet side insulating material described in the third aspect, comprising:

[0055] SS1. Using an atomizing air compressor, the insulating material on the side of the resistor sheet is coated onto the side of the raw material resistor sheet to obtain resistor sheet I. The pressure of the atomizing air compressor is 3-5 MPa, and the coating thickness is 100-300 μm.

[0056] SS2. The resistor I is sintered at 20-550℃ to obtain a product resistor with insulating glaze on the side.

[0057] According to a preferred embodiment, the method of the present invention further includes: in step SS1, using an atomizing air compressor connected to a spray gun to coat the side insulating material of the resistor sheet onto the side of the raw material resistor sheet.

[0058] According to a preferred embodiment, the method further includes: the sintering operation in step SS2 further includes a heating process, including:

[0059] (1-1) After 100-150 minutes, the temperature is raised from 25±5℃ to 320±5℃;

[0060] (1-2) After 25-50 minutes, the temperature is raised from 320±5℃ to 375±5℃;

[0061] (1-3) Keep warm at 375±5℃ for 60-120 min;

[0062] (1-4) After 30-40 minutes, the temperature is raised from 375±5℃ to 490±5℃;

[0063] (1-5) After 20-30 minutes, the temperature is raised from 490±5℃ to 525±5℃;

[0064] (1-6) Keep warm at 525±5℃ for 60-120 min;

[0065] (1-7) After 1620-4200 min, the temperature was reduced from 525±5℃ to 120±5℃;

[0066] (1-8) Cool to 25±5℃ to obtain a product resistor sheet with insulating glaze on the side.

[0067] In the following examples, unless otherwise specified, the mass ratios are all based on the total mass of the substance as a solution, powder, or solid.

[0068] In the following examples, unless otherwise specified, room temperature refers to 25±5℃.

[0069] In the following examples, unless otherwise specified, each “part by weight” is 100g.

[0070] In the following examples, unless otherwise specified, all products used are commercially available.

[0071] raw material:

[0072] Raw material resistor: ZnO resistor, purchased from Hunan Power Grid Disaster Prevention Technology Co., Ltd., with parameters of 42mm diameter and 100kA current carrying capacity;

[0073] Butylcarbidol: analytical grade, purchased from Chengde Fu'an Electric Co., Ltd.;

[0074] Ethyl cellulose: purchased from Shanghai Yuanye Biotechnology Co., Ltd., brand name S14026-500g.

[0075] equipment:

[0076] Atomizing air compressor: purchased from Hunan Pinde Electric Co., Ltd.;

[0077] Ball mill: rated speed 0-720 rpm, purchased from Nanyang Zhongwei Electric Co., Ltd.

[0078] Preparation of adhesives:

[0079] S1. Place ethanol into the inner tank of a water bath and, under stirring conditions at 80°C, add butylcarbidol to the ethanol for a second mixing for 60 minutes to obtain mixture II; the stirring speed is 400 rpm.

[0080] S2. After raising the temperature to 85°C, under stirring conditions, ethyl cellulose is added to the mixture II in three portions for a third mixing of 100 min. After standing for 24 h, the supernatant is taken to obtain the adhesive; the rotation speed is 400 rpm.

[0081] The weight ratio of the ethanol, the butyl carbitol, and the ethyl cellulose is 1:0.05:0.05.

[0082] Example A-1

[0083] This embodiment illustrates the preparation method of the insulating material on the side of the resistor sheet provided by the present invention. Referring to the addition amount and process parameters in Table 1, the method is carried out according to the following steps:

[0084] (1) Mix and contact each component in the ingredients at 85°C for 30 minutes to obtain the ingredients, and then mix the adhesive with the ingredients at a weight ratio of 1:1 for 30 minutes to obtain mixture I; the rotation speed is 360 rpm;

[0085] (2) The mixture I was ground in a ball mill for 45 hours using zirconium balls to obtain the insulating material on the side of the resistor sheet; the rotation speed was 400 rpm.

[0086] The total mass of the grinding balls is 1:1 with the mass of the ingredients. The diameter of the grinding balls is divided into three levels: small (1 mm), medium (5 mm), and large (10 mm). The ratio of the number of grinding balls of the three levels is 10%: 20%: 70%.

[0087] The insulating material on the side of the resistor sheet is named a1.

[0088] Example A-2

[0089] This embodiment uses a method similar to that of Embodiment A-1, except that the amount of each component added in the ingredients is changed. See Table 1 for specific parameters.

[0090] The ratio of the total mass of the grinding balls to the mass of the ingredients is 1:2, and the ratio of the number of large, medium and small grinding balls is 20%:30%:50%.

[0091] The insulating material on the side of the resistor sheet is named a2.

[0092] Example A-3

[0093] This embodiment uses a method similar to that of embodiment A-1, except that the process parameters have been changed. See Table 1 for specific parameters.

[0094] The insulating material on the side of the resistor sheet is named a3.

[0095] Example B-1

[0096] This embodiment illustrates the following steps in the preparation method of the resistive sheet with insulating glaze on its side provided by the present invention:

[0097] SS1. Using an atomizing air compressor connected to a spray gun, the insulating material a1 on the side of the resistor sheet is coated onto the side of the raw material resistor sheet to obtain resistor sheet I. The pressure of the atomizing air compressor is 5MPa, and the coating thickness is 200μm.

[0098] SS2. The resistor I is sintered at 25-525℃ to obtain a product resistor with insulating glaze on the side. The specific heating process is as follows:

[0099] (1-1) After 100 minutes, the temperature was raised from 25℃ to 320℃;

[0100] (1-2) After 25 minutes, the temperature was raised from 320℃ to 375℃;

[0101] (1-3) Keep warm at 375℃ for 60 minutes;

[0102] (1-4) After 30 minutes, the temperature was raised from 375℃ to 490℃;

[0103] (1-5) After 30 minutes, the temperature was raised from 490℃ to 525℃;

[0104] (1-6) Keep warm at 525℃ for 120 min;

[0105] (1-7) After 1620 minutes, the temperature was reduced from 525℃ to 120℃;

[0106] (1-8) Cool to 25°C to obtain a product resistor sheet with insulating glaze on the side, named b1.

[0107] Figure 1 The microstructure of the resistor observed using a micro-electron microscope is shown. The outermost layer is an insulating side glaze with a thickness of about 200 μm. Between the side glaze and the body of the ZnO resistor, there is a high-resistivity layer composed of Zn2SiO4 and spinel, which is a glass phase. This high-resistivity layer can effectively fill the gap between the body of the ZnO resistor and the high-resistivity layer, and can effectively prevent side insulation flashover of the ZnO resistor during lightning strikes.

[0108] Example B-2

[0109] This embodiment uses a method similar to that of embodiment B-1, except that the side insulating material a2 of the resistor sheet is used instead of the side insulating material a1 of the resistor sheet in step SS1.

[0110] The resulting resistor sheet with insulating glaze on its sides is named b2.

[0111] Example B-3

[0112] This embodiment uses a method similar to that of Embodiment B-1, except that side insulating material a3 is used instead of side insulating material a1 for step SS1, and the specific heating process of sintering is as follows: sintering to obtain a product resistor sheet with insulating glaze on the side, specifically:

[0113] (1-1) After 150 minutes, the temperature was raised from 25℃ to 320℃;

[0114] (1-2) After 50 minutes, the temperature was raised from 320℃ to 375℃;

[0115] (1-3) Keep warm at 375℃ for 120 min;

[0116] (1-4) After 40 minutes, the temperature was raised from 375℃ to 490℃;

[0117] (1-5) After 30 minutes, the temperature was raised from 490℃ to 525℃;

[0118] (1-6) Keep warm at 525℃ for 120 min;

[0119] (1-7) After 4200 minutes, the temperature was reduced from 525℃ to 120℃;

[0120] (1-8) Cool to 25°C to obtain a product resistor sheet with insulating glaze on the side, named b3.

[0121] Comparative Example 1

[0122] This comparative example was carried out using a method similar to that of Example B-1, except that conventional ZnO side insulation material was used instead of the resistor sheet side insulation material a1 (purchased from Henan Nanyang Jinniu Co., Ltd., brand name CAS 1314-13-2) for step SS1.

[0123] The resulting resistor sheet with insulating glaze on its sides is named b4.

[0124] Test Example 1

[0125] For product resistors b1, b2, b3, and b4 with insulating glaze on the sides, a high-amplitude lightning impulse current test of the insulating glaze was conducted using an impulse voltage generator (model 35kV 100kA, purchased from Xi'an Dianyou Technology Co., Ltd.). The test conditions were as follows: the product resistor core was placed under the impulse high-current test device, an impulse high current was applied to the product resistor, and it was observed whether side insulation flashover occurred.

[0126] The results are shown in Table 2.

[0127] Table 1

[0128]

[0129]

[0130] Table 2

[0131] Parameter Items b1 b2 b3 b4 High current amplitude of lightning impulse causing side insulation flashover / kA 100 95 93 96

[0132] The results above show that the glass glaze formed on the side of the resistor sheet by the insulating material provided by the present invention has high resistivity and is not prone to side insulation flashover under lightning strike.

[0133] The preferred embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combinations of various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.

Claims

1. A method for preparing a resistor sheet, characterized in that, This method utilizes the insulating material on the side of the resistor sheet, including: SS1. Using an atomizing air compressor, the insulating material on the side of the resistor sheet is coated onto the side of the raw material resistor sheet to obtain resistor sheet I. The pressure of the atomizing air compressor is 3-5 MPa, and the coating thickness is 100-300 μm. SS2. The resistor sheet I is sintered at 20-550℃ to obtain a product resistor sheet with an insulating glaze on the side; there is a high-resistivity layer containing Zn2SiO4 and spinel between the insulating glaze and the raw material resistor sheet, and the high-resistivity layer is a glass phase; The sintering operation in step SS2 further includes a heating process, including: (1-1) After 100-150 minutes, the temperature is raised from 25±5℃ to 320±5℃; (1-2) After 25-50 minutes, the temperature is raised from 320±5℃ to 375±5℃; (1-3) Keep warm at 375±5℃ for 60-120 min; (1-4) After 30-40 minutes, the temperature is raised from 375±5℃ to 490±5℃; (1-5) After 20-30 minutes, the temperature is raised from 490±5℃ to 525±5℃; (1-6) Keep warm at 525±5℃ for 60-120 min; (1-7) After 1620-4200 min, the temperature was reduced from 525±5℃ to 120±5℃; (1-8) Cool to 25±5℃ to obtain a product resistor sheet with insulating glaze on the side; The method for preparing the insulating material on the side of the resistor sheet includes: (1) The ingredients and adhesive are first mixed to obtain mixture I; (2) Grind the mixture I to obtain the insulating material on the side of the resistor sheet; The ingredients contain the following components: PbO, B2O3, ZnO, Al2O3, SiO2, and AgO; based on the total mass of the ingredients, the content of PbO is 70-80 wt%, the content of B2O3 is 5-20 wt%, the content of ZnO is 5-10 wt%, the content of Al2O3 is 5-10 wt%, the content of SiO2 is 3-5 wt%, and the content of AgO is 1-3 wt%. The adhesive is composed of ethanol, butyl carbitol, and ethyl cellulose in a weight ratio of 1:0.05-0.1:0.05-0.

1. The weight ratio of the adhesive to the ingredients is 1:0.9-1.

2.

2. The method according to claim 1, wherein, The method further includes: in step (1), preparing the adhesive using a step comprising the following operations: S1. Under stirring conditions, ethanol and butylcarbidol are mixed for a second time for 30-60 minutes to obtain mixture II; S2. Under stirring conditions, the mixture II is mixed with ethyl cellulose for a third time for 60-120 minutes to obtain the adhesive.

3. The method according to claim 2, wherein, In step S1, the conditions for the second mixing must at least satisfy: rotation speed of 360-420 rpm and temperature of 80-90℃; And / or, in step S2, the conditions for the third mixing are at least: a rotation speed of 360-420 rpm and a temperature of 80-90°C.

4. The method according to any one of claims 1-3, wherein, In step (1), the conditions for the first mixing include: being carried out under stirring conditions, with a stirring speed of 360-420 rpm, a stirring time of 30-120 min, and a temperature of 80-90℃.

5. The method according to any one of claims 1-3, wherein, In step (2), the grinding conditions include: a rotation speed of 350-360 rpm, a grinding time of 24-72 h, and a mass ratio of the total mass of the grinding balls to the mass of the ingredients of 1:1-2, and the diameter of each grinding ball is 1-20 mm.

Citation Information

Patent Citations

  • Preparation method of high-gradient zinc oxide piezoresistor high-resistance layer with high through-flow capacity

    CN106587985A

  • Lightning arrester resistor disc side glaze formula

    CN113045203A

  • Inorganic galss insulating paint