Double-sided heat dissipation SiC MOSFET packaging structure and its connection method between heat sink and ceramic substrate
By employing a double-sided heat dissipation structure and high-efficiency connection materials, the low heat dissipation efficiency and reliability issues of SiC MOSFET packaging structures are solved, achieving multi-path heat dissipation and high thermal conductivity connections, thereby improving the heat dissipation performance and reliability of the device.
Patent Information
- Application Number
- CN202311324814.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-13
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-10-13
AI Technical Summary
Existing SiC MOSFET packaging structures have low heat dissipation efficiency and small heat dissipation area. Traditional connection materials have poor thermal conductivity and thermal reliability, resulting in insufficient device reliability.
It adopts a double-sided heat dissipation structure, uses Sn3.5Ag4Ti solder to connect the graphite heat sink and the ceramic substrate, and combines cylindrical chip molybdenum pads and supporting molybdenum pads to provide multi-path heat dissipation. The connection strength and stability are improved by a nano-silver sintering layer.
This improves the heat dissipation performance and thermal reliability of the SiC MOSFET package structure, enhances the mechanical rigidity of the device, and extends its service life.
Smart Images

Figure CN117577599B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of chip packaging technology, and specifically to a double-sided heat dissipation SiC MOSFET packaging structure and a method for connecting its heat sink to a ceramic substrate. Background Technology
[0002] SiC MOSFETs are widely used in high-voltage, high-frequency, and high-power applications due to their advantages such as high switching frequency, low switching loss, and high voltage resistance. During the operation of a SiC MOSFET module, a significant amount of heat is generated at the chip. If this heat cannot be dissipated in time, it will seriously threaten the reliability of the device. As modules become smaller and denser in packaging, the heat flux density inside the package structure increases. The mismatch in the thermal expansion coefficients of different materials will generate significant thermal stress, leading to strain within the package structure sufficient to compromise its structural integrity. Therefore, a SiC MOSFET package structure with excellent heat dissipation performance is crucial for improving device reliability.
[0003] Traditional SiC MOSFET packaging structures are mainly single-sided heat dissipation structures, with a single heat dissipation path and a small heat dissipation area. Moreover, the thermal grease and adhesives used to connect the heat sink and the ceramic substrate have low thermal conductivity and thermal reliability. Therefore, how to develop a SiC MOSFET package that can both expand the heat dissipation surface and achieve multi-path heat dissipation is an urgent problem to be solved. Summary of the Invention
[0004] The main objective of this invention is to overcome the shortcomings and deficiencies of the prior art and provide a double-sided heat dissipation SiC MOSFET package structure and its heat sink and ceramic substrate connection method, thereby improving the heat dissipation efficiency of the SiC MOSFET package structure and achieving high thermal conductivity bonding interconnection, thus meeting the requirements of higher reliability and longer service life of power devices.
[0005] To achieve the above objectives, the present invention adopts the following technical solution:
[0006] In a first aspect, the present invention provides a double-sided heat dissipation SiC MOSFET package structure, the structure comprising an upper heat sink, an upper heat sink bonding layer, an upper ceramic substrate, a bonding layer on a supporting molybdenum pad, a supporting molybdenum pad, a lower bonding layer on a supporting molybdenum pad, a bonding layer on a chip molybdenum pad, a chip molybdenum pad, a lower bonding layer on a chip molybdenum pad, a SiC chip, a chip bonding layer, a lower ceramic substrate, a lower heat sink bonding layer, and a lower heat sink;
[0007] The upper heat sink is connected to the upper ceramic substrate through an upper heat sink welding layer;
[0008] The upper ceramic substrate is connected to the supporting molybdenum pad via an upper welding layer, and the supporting molybdenum pad is connected to the lower ceramic substrate via a lower welding layer. A chip molybdenum pad and a SiC chip are disposed below the upper ceramic substrate. The upper ceramic substrate is connected to one side of the chip molybdenum pad via an upper welding layer, and the other side of the chip molybdenum pad is connected to the SiC chip via a lower welding layer. The terminals of the SiC chip are connected to the lower ceramic substrate via a chip welding layer.
[0009] The lower heat sink and the lower ceramic substrate are connected by a lower heat sink welding layer.
[0010] As a preferred technical solution, the upper heat sink and the lower heat sink have the same structure, both including heat dissipation fins and a base plate, and the heat dissipation fins and the base plate are in contact; the heat dissipation fins include a plurality of parallel rectangular sheet-like heat dissipation fins.
[0011] As a preferred technical solution, the upper heat sink welding layer and the lower heat sink welding layer are welding layers of Sn3.5Ag4Ti active solder.
[0012] As a preferred technical solution, both the upper welding layer and the lower welding layer of the supporting molybdenum pad are made of nano-silver sintered layer.
[0013] As a preferred technical solution, the upper welding layer of the chip molybdenum pad, the lower welding layer of the chip molybdenum pad, and the chip welding layer all adopt nano-silver sintering layers.
[0014] As a preferred technical solution, the upper ceramic substrate and the lower ceramic substrate are made of aluminum nitride ceramic, and the aluminum nitride ceramic is provided with a copper plating layer.
[0015] As a preferred technical solution, the molybdenum pad for the chip adopts a cylindrical structure.
[0016] As a preferred technical solution, the supporting molybdenum pad adopts a cylindrical structure.
[0017] As a preferred technical solution, the molybdenum chip pads and SiC chips are provided in multiple groups and distributed in a matrix on the lower ceramic substrate.
[0018] Secondly, the present invention also provides a method for connecting a heat sink to a ceramic substrate, applied to a double-sided heat dissipation SiCMOSFET package structure, comprising the following steps:
[0019] S1. The base plate of the polished heat sink to be welded, wherein the heat sink includes an upper heat sink and a lower heat sink;
[0020] S2. Clean and polish the heat sink;
[0021] S3. Preheat the heat sink on a heating platform at a set temperature, then place the solder of the upper heat sink welding layer and the lower heat sink welding layer on the surface of the heat sink to be welded. When the solder of the upper heat sink welding layer and the lower heat sink welding layer begins to melt, mechanically stir to ensure that the molten solder wets the surface of the heat sink to be welded.
[0022] S4. Place the ceramic substrate on the molten solder from step S3, rub the ceramic substrate and the surface to be soldered of the heat sink together, and then apply a certain pressure in the direction perpendicular to the soldering surface to ensure the tightness of the connection.
[0023] S5. After welding, heat-insulate the connected parts for a preset time, and then allow them to cool naturally to room temperature. The connection is now complete.
[0024] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0025] (1) The double-sided heat dissipation structure and graphite heat sink of the present invention overcome the shortcomings of low heat transfer efficiency and small heat dissipation area of existing SiC MOSFET devices, thereby making the structure of the present invention have stronger heat exchange capability and improving the heat dissipation performance and thermal reliability of the device.
[0026] (2) The present invention uses Sn3.5Ag4Ti solder to connect graphite heat sink and ceramic substrate. Sn3.5Ag4Ti solder has excellent bonding ability to both graphite heat sink and ceramic substrate, overcoming the shortcomings of poor thermal reliability and low thermal conductivity of traditional thermal interface materials. Thus, the present invention can achieve low thermal resistance connection between graphite heat sink and ceramic substrate.
[0027] (3) The present invention uses a cylindrical chip molybdenum pad and a supporting molybdenum pad, which can effectively relieve the stress and pressure on the chip, increase the mechanical rigidity of the internal structure of the chip package, and prevent the mismatch of thermal expansion coefficients of different materials due to thermal expansion and thermal compression during operation, thereby improving the reliability of the device. Attached Figure Description
[0028] Figure 1 This is a schematic diagram of the main structure of the overall structure in an embodiment of the present invention;
[0029] Figure 2 This is an exploded structural diagram of the main view of the overall structure in an embodiment of the present invention;
[0030] Figure 3 This is an exploded structural diagram of the right view of the overall structure in an embodiment of the present invention;
[0031] Figure 4 This is a schematic diagram of the overall chip layout in an embodiment of the present invention;
[0032] Figure 5This is a three-dimensional structural diagram of the overall structure in an embodiment of the present invention.
[0033] Explanation of reference numerals: 1-Upper heat sink; 2-Upper heat sink solder layer; 3-Upper ceramic substrate; 4-Upper solder layer of supporting molybdenum pad; 5-Supporting molybdenum pad; 6-Lower solder layer of supporting molybdenum pad; 7-Upper solder layer of chip molybdenum pad; 8-Chip molybdenum pad; 9-Lower solder layer of chip molybdenum pad; 10-SiC chip; 11-Chip solder layer; 12-Lower ceramic substrate; 13-Lower heat sink solder layer; 14-Lower heat sink. Detailed Implementation
[0034] The present invention will be further described in detail below with reference to the embodiments and accompanying drawings, but the embodiments of the present invention are not limited thereto.
[0035] Example
[0036] Please see Figure 1-5 This embodiment provides a double-sided heat dissipation SiC MOSFET package structure, including an upper heat sink 1, an upper heat sink bonding layer 2, an upper ceramic substrate 3, a bonding layer 4 on a supporting molybdenum pad, a supporting molybdenum pad 5, a bonding layer 6 on a supporting molybdenum pad, a bonding layer 7 on a chip molybdenum pad, a chip molybdenum pad 8, a bonding layer 9 on a chip molybdenum pad, a SiC chip 10, a chip bonding layer 11, a lower ceramic substrate 12, a lower heat sink bonding layer 13, and a lower heat sink 14.
[0037] Furthermore, the upper heat sink 1 is connected to the upper ceramic substrate 3 via the upper heat sink solder layer 2; the upper ceramic substrate 3 is connected to the supporting molybdenum pad 5 via the upper solder layer 4, and the supporting molybdenum pad 5 is connected to the lower ceramic substrate 14 via the lower solder layer 6; a chip molybdenum pad 8 and a SiC chip 10 are disposed below the upper ceramic substrate 3, the upper ceramic substrate 3 is connected to one side of the chip molybdenum pad 8 via the upper solder layer 7, and the other side of the chip molybdenum pad 8 is connected to the SiC chip 10 via the lower solder layer 9, and the terminals of the SiC chip 10 are connected to the lower ceramic substrate 12 via the chip solder layer 11; the lower heat sink 14 and the lower ceramic substrate 12 are connected via the lower heat sink solder layer 13.
[0038] In this embodiment, both the upper heat sink 1 and the lower heat sink 14 are graphite heat sinks, with structures including heat dissipation fins and a graphite base plate. The heat dissipation fins include 21 parallel rectangular sheet-like heat dissipation fins, which are in contact with the base plate. Because graphite has a low density and excellent thermal conductivity, this invention reduces the weight of the device and improves its heat dissipation efficiency. Therefore, in this embodiment, both the heat dissipation fins and the base plate use graphite as the main material.
[0039] Furthermore, in this embodiment, the upper ceramic substrate 3 and the lower ceramic substrate 12 have a two-layer structure, comprising an aluminum nitride ceramic layer and a copper plating layer. The aluminum nitride ceramic layer in this embodiment utilizes aluminum nitride ceramic material, which, on the one hand, possesses excellent thermal conductivity—generally six times that of alumina and twice that of silicon nitride—and on the other hand, exhibits stable mechanical and thermal properties, providing good support and stability for the device and improving its heat dissipation capabilities. In this embodiment, the alumina ceramic is copper-plated to form a copper plating layer, which can replace bonding wires for chip-to-chip connections, improving signal transmission efficiency and reliability.
[0040] It should also be noted that wire bonding is a process that uses thin metal wires and employs heat, pressure, and ultrasonic energy to tightly bond the metal wires to the substrate pads. However, because the metal wires are longer and have a smaller diameter than bumps, they result in high impedance. This leads to longer signal transmission times, affecting circuit performance and speed, and also causes signal distortion. Copper itself has excellent conductivity, and due to the large surface area of the component, copper plating on alumina ceramic results in a lower impedance on the alumina ceramic layer. Compared to wire bonding, this improves conductivity, further enhancing signal transmission performance and efficiency.
[0041] In this embodiment, Sn3.5Ag4Ti active solder was used for both the upper heat sink soldering layer 2 and the lower heat sink soldering layer 13. Sn3.5Ag4Ti solder has excellent adhesion to both graphite heat sinks and ceramic substrates, reducing the thermal resistance caused by non-smooth surfaces and air gaps at the connection interface, and can efficiently transfer heat from inside the device to the heat dissipation channel. Therefore, Sn3.5Ag4Ti solder is the optimal soldering material in this embodiment.
[0042] In this embodiment, the upper welding layer 4 of the supporting molybdenum pad, the lower welding layer 6 of the supporting molybdenum pad, the upper welding layer 7 of the chip molybdenum pad, the lower welding layer 9 of the chip molybdenum pad, and the chip welding layer 11 all adopt nano-silver sintering layers. Nano-silver sintering has the advantages of low-temperature sintering and high-temperature use, and has good high-temperature working characteristics, which can effectively avoid damage to the chip caused by high-temperature welding during device manufacturing.
[0043] like Figure 2-3As is clearly understood, in this embodiment, both the chip molybdenum pad 8 and the supporting molybdenum pad 5 adopt a cylindrical structure. For the chip molybdenum pad, during manufacturing, it effectively alleviates the stress and pressure on the chip, thereby improving device reliability. The supporting molybdenum pad primarily serves as a buffer layer, increasing the mechanical rigidity of the chip package's internal structure and preventing mismatches in the thermal expansion coefficients of different materials due to thermal expansion and compression during operation.
[0044] Based on the double-sided heat dissipation SiC MOSFET package structure disclosed in this embodiment, there are two heat dissipation paths: the first is from the chip bonding layer 11, through the lower ceramic substrate 12 and the lower heat sink bonding layer 13 to the lower heat sink 14; the second is from the lower bonding layer 9 of the chip molybdenum pad, through the chip molybdenum pad 8, the upper bonding layer 7 of the chip molybdenum pad, the upper ceramic substrate 3, and the upper heat sink bonding layer 2 to the upper heat sink 1. Therefore, the present invention has stronger heat exchange capability and improves the heat dissipation performance and thermal reliability of the device.
[0045] In addition, this embodiment also provides a method for connecting a heat sink to a ceramic substrate, including the following steps:
[0046] S1. Polish the graphite substrate of the graphite heat sink to be welded using diamond polishing paste;
[0047] S2. Use ethanol to ultrasonically clean the polished graphite heat sink.
[0048] S3. Preheat the graphite heat sink on a heating platform at 300℃ for one minute, then place the Sn3.5Ag4Ti solder on the surface of the graphite heat sink to be welded. When the Sn3.5Ag4Ti solder begins to melt, mechanically stir to ensure that the molten solder wets the surface of the graphite heat sink to be welded.
[0049] S4. Place the ceramic substrate on the molten solder from step S3, rub the ceramic substrate and the surface to be welded of the graphite heat sink against each other for thirty seconds, and then apply a certain pressure in the direction perpendicular to the welding surface to ensure the tightness of the connection.
[0050] S5. Keep the connector warm for 30 minutes, then let it cool naturally to room temperature. The connection is complete.
[0051] Finally, the directional terms "up," "down," "one side," and "the other side" mentioned above can be found in the appendix. Figure 1-5To facilitate understanding of the structure of this invention, this embodiment uses the chip soldering position as a reference system, with the chip soldering substrate vertically upward as the "lower" of this embodiment, and the opposite as the "upper"; while "one side" and "the other side" are a pair, which will change with the shape and method of the pad. For example, the cylindrical chip molybdenum pad and the supporting molybdenum pad mentioned in this embodiment, the supporting side can be obviously understood as the upper and lower bottom surfaces.
[0052] The above embodiments are preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the above embodiments. Any changes, modifications, substitutions, combinations, or simplifications made without departing from the spirit and principle of the present invention shall be considered equivalent substitutions and shall be included within the protection scope of the present invention.
Claims
1. A double-sided heat dissipation SiC MOSFET package structure, characterized in that, It includes an upper heat sink, an upper heat sink welding layer, an upper ceramic substrate, a welding layer on a supporting molybdenum pad, a supporting molybdenum pad, a welding layer on a supporting molybdenum pad, a welding layer on a chip molybdenum pad, a chip molybdenum pad, a welding layer on a chip molybdenum pad, a SiC chip, a chip welding layer, a lower ceramic substrate, a lower heat sink welding layer, and a lower heat sink. The upper heat sink is connected to the upper ceramic substrate through an upper heat sink welding layer; The upper ceramic substrate is connected to the supporting molybdenum pad via an upper welding layer, and the supporting molybdenum pad is connected to the lower ceramic substrate via a lower welding layer. A chip molybdenum pad and a SiC chip are disposed below the upper ceramic substrate. The upper ceramic substrate is connected to one side of the chip molybdenum pad via an upper welding layer, and the other side of the chip molybdenum pad is connected to the SiC chip via a lower welding layer. The terminals of the SiC chip are connected to the lower ceramic substrate via a chip welding layer. The lower heat sink and the lower ceramic substrate are connected by a lower heat sink welding layer; The upper and lower heat sink welding layers are welding layers made of Sn3.5Ag4Ti active solder.
2. The SiC MOSFET package structure with double-sided heat dissipation according to claim 1, characterized in that, The upper and lower heat sinks have the same structure, both including heat dissipation fins and a base plate, with the heat dissipation fins in contact with the base plate; the heat dissipation fins include multiple parallel rectangular sheet-like heat dissipation fins.
3. The SiC MOSFET package structure with double-sided heat dissipation according to claim 1, characterized in that, Both the upper welding layer and the lower welding layer of the supporting molybdenum pad are made of nano-silver sintered layer.
4. The SiC MOSFET package structure with double-sided heat dissipation according to claim 1, characterized in that, The upper welding layer, lower welding layer, and chip welding layer of the chip molybdenum pad are all made of nano-silver sintered layer.
5. The SiC MOSFET package structure with double-sided heat dissipation according to claim 1, characterized in that, The upper and lower ceramic substrates are made of aluminum nitride ceramic, and the aluminum nitride ceramic is provided with a copper plating layer.
6. The SiC MOSFET package structure with double-sided heat dissipation according to claim 1, characterized in that, The molybdenum pad for the chip has a cylindrical structure.
7. The SiC MOSFET package structure with double-sided heat dissipation according to claim 1, characterized in that, The supporting molybdenum pad has a cylindrical structure.
8. The SiC MOSFET package structure with double-sided heat dissipation according to claim 1, characterized in that, The chip molybdenum pads and SiC chips are arranged in multiple groups and distributed in a matrix on the lower ceramic substrate.
9. A method for connecting a heat sink to a ceramic substrate, used in the double-sided heat dissipation SiC MOSFET package structure according to any one of claims 1-8, characterized in that, Includes the following steps: S1. The base plate of the polished heat sink to be welded, wherein the heat sink includes an upper heat sink and a lower heat sink; S2. Clean and polish the heat sink; S3. Preheat the heat sink on a heating platform at a set temperature, then place the solder of the upper heat sink welding layer and the lower heat sink welding layer on the surface of the heat sink to be welded. When the solder of the upper heat sink welding layer and the lower heat sink welding layer begins to melt, mechanically stir to ensure that the molten solder wets the surface of the heat sink to be welded. S4. Place the ceramic substrate on the molten solder from step S3, rub the ceramic substrate and the surface to be soldered of the heat sink together, and then apply a certain pressure in the direction perpendicular to the soldering surface to ensure the tightness of the connection. S5. After welding, heat-insulate the connected parts for a preset time, and then allow them to cool naturally to room temperature. The connection is now complete.
Citation Information
Patent Citations
Double-bridge-arm double-sided heat dissipation IGBT power module packaging structure in high-power environment
CN116666325A
Oxidation resistance tin-based no-lead solder capable of proceeding welding without welding flux in air
CN1907636A