Niobium oxide composite energy storage materials, their preparation methods and applications
By preparing a multilayer sheet-like niobium oxide composite energy storage material, the problems of low energy density in traditional lithium-ion batteries, poor cycle stability in sodium-ion batteries, and dissolution shuttle effect in lithium-sulfur batteries have been solved, achieving high energy density and low cost energy storage effect.
Patent Information
- Application Number
- CN202311579359.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-24
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-11-24
AI Technical Summary
Traditional lithium-ion batteries have low energy density and high cost, sodium-ion batteries have poor cycle stability, and lithium-sulfur batteries have severe dissolution shuttle effect. Existing energy storage systems cannot meet the requirements of high energy density and low cost for large-scale energy storage.
Niobium oxide composite energy storage materials are used, including composite particles of niobium oxide matrix and non-metallic carbon materials. Multilayer sheet-like niobium oxide is prepared by oxidation and carbonization treatment to form effective lithium ion adsorption surface capacitance and diffusion path, alleviate volume expansion and suppress shuttle effect.
It improves the energy storage performance of lithium-ion batteries, reduces costs, improves the cycle stability of sodium-ion batteries, effectively suppresses the dissolution shuttle effect of lithium-sulfur batteries, and ensures electrochemical stability.
Smart Images

Figure CN117577844B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of electrochemical energy, specifically relating to a niobium oxide composite energy storage material, its preparation method, and its application. Background Technology
[0002] Lithium-ion batteries (LIBs) are among the most promising and commercially viable energy storage power sources, boasting advantages such as high specific energy, low self-discharge, excellent cycle performance, no memory effect, and environmental friendliness. However, with economic globalization and the widespread use of irreversible fossil fuels, environmental pollution and energy shortages are becoming increasingly prominent, leading to a surge in market demand for lithium. The relatively limited and unevenly distributed lithium resources in the Earth's crust contribute to the high price of lithium. Currently, however, lithium-ion batteries cannot meet the high energy density and low cost requirements of large-scale energy storage systems, nor can they match the driving range of electric vehicles (500km / charge). Therefore, developing a new generation of energy storage systems that are high in energy density, low in cost, long-life, and environmentally friendly is of paramount importance.
[0003] Sodium-ion batteries possess a lithium storage mechanism similar to that of lithium-ion batteries, and the advantages of abundant sodium resources and low cost make rechargeable sodium-ion batteries an important supplement to lithium-ion batteries, attracting widespread attention. However, sodium-ion batteries also have certain problems, such as poor conductivity of the negative electrode material, poor reaction kinetics of sodium ions, large sodium ion radius, rapid volume change of the buffer material during insertion / extraction processes that cannot guarantee its structural and electrochemical stability, and a limited number of electrode materials that can stably accommodate the insertion and extraction of sodium ions.
[0004] Lithium-sulfur batteries consist of a sulfur cathode and a lithium metal anode, boasting a theoretical energy density of 2600 Wh / kg. Sulfur is abundant in nature, possessing a high theoretical specific capacity of 1675 mAh / g, and is inexpensive and environmentally friendly. Therefore, lithium-sulfur batteries are considered one of the next-generation battery candidates and have received widespread research attention. Despite the significant advantages of Li-S batteries, the sulfur cathode still faces several serious problems: both the active material sulfur (S) and the final product lithium sulfide (Li₂S) are insulators with poor electronic conductivity; the large density difference between S and Li₂S leads to a significant volume change (approximately 80%) in the electrode during charge and discharge; and, in particular, the polysulfides generated during charge and discharge have extremely high solubility in ether-based electrolytes, resulting in a "shuttle effect." The shuttle effect leads to low utilization of active materials, low coulombic efficiency, and short cycle life. Therefore, the dissolution and shuttle of polysulfide intermediates is one of the key challenges that urgently needs to be addressed in lithium-sulfur batteries.
[0005] Therefore, developing a system that is compatible with lithium-ion batteries, sodium-ion batteries, and lithium-sulfur batteries, and can store energy quickly and stably, is an urgent problem to be solved. Summary of the Invention
[0006] The technical problem to be solved by this invention is how to effectively improve the energy storage performance of traditional lithium-ion batteries, reduce costs, and solve the poor cycle stability of sodium-ion batteries and effectively suppress the dissolution shuttle effect of lithium-sulfur batteries. In order to overcome the shortcomings and defects mentioned in the background technology, this invention provides a niobium oxide composite energy storage material, its preparation method and application.
[0007] The technical solution adopted by the present invention to solve its technical problem is: a niobium oxide composite energy storage material, comprising composite particles, wherein the composite particles comprise a niobium oxide matrix and a non-metallic carbon material; wherein the non-metallic carbon material is dispersed and loaded on the surface of the niobium oxide matrix.
[0008] The molecular formula of the above niobium oxide matrix is Nb x O y It has a multi-layered sheet-like structure.
[0009] The aforementioned non-metallic carbon materials are at least one of carbon nanotubes, Super P, graphene, ethylene glycol, and glucose carbonization.
[0010] The preparation method of the above-mentioned niobium oxide composite energy storage material includes the following steps:
[0011] a. Directly calcining and oxidizing niobium-containing MXene materials in air or an oxygen atmosphere to obtain niobium-containing oxides after complete oxidation;
[0012] b. Mix the non-metallic carbon material with the niobium-containing oxide obtained in step a, and fully carbonize it under a carbon dioxide atmosphere to obtain a niobium oxide composite energy storage material.
[0013] In step a above, the niobium-containing MXene material is niobium carbide (Nb2CT). x Any one of MXene, niobium aluminum carbide (Nb4AlC3)MAX phase ceramic materials and niobium aluminum carbide (Nb2AlC)MAX phase ceramic materials.
[0014] In step a above, the calcination oxidation temperature is 350-1000℃, the time is 1-10h, and the heating rate is 1-10℃ / min.
[0015] In step b above, the non-metallic carbon material is at least one of carbon nanotubes, Super P, graphene, ethylene glycol, and glucose carbonization.
[0016] In step b above, the mass ratio of the non-metallic carbon material to the niobium oxide is 1-10:1.
[0017] In step b above, the carbonization is carried out in a tube furnace at a temperature of 400-1000℃ for a time of 0.5-6 hours.
[0018] The aforementioned niobium oxide composite energy storage material can be applied to sodium-ion batteries, lithium-ion batteries, and lithium-sulfur batteries.
[0019] The beneficial effects of this invention are as follows: The niobium oxide composite energy storage material of this invention has a multi-layered structure, which can effectively adsorb lithium ions, form surface capacitance, and effectively improve the theoretical capacity. It is a binary transition metal sulfide, which effectively improves the conductivity of the electrode material and buffers the rapid volume change of the material during sodium ion insertion / extraction, thus ensuring its structural and electrochemical stability. The niobium oxide composite energy storage material of this invention provides an effective diffusion path for electrons and ions, alleviates the volume expansion during the material insertion / extraction process, effectively suppresses the shuttle effect, and ensures structural and electrochemical stability.
[0020] The niobium oxide composite energy storage material of the present invention can be prepared in one step. The method is simple, the material is readily available, the reproducibility is high, it is pollution-free, and the product structure is easy to control. It can be applied in sodium-ion batteries, lithium-ion batteries and lithium-sulfur batteries, and has a very broad application prospect. Attached Figure Description
[0021] Figure 1 Niobium carbide (Nb2CT) was provided for Example 1. x SEM image of MXene material;
[0022] Figure 2 Niobium carbide (Nb2CT) provided in Example 1 x Field emission diagram of Nb2O5 after oxidation of MXene material;
[0023] Figure 3 Niobium carbide (Nb2CT) provided in Example 1 x Field emission diagram of Nb2O5 after oxidation of MXene material;
[0024] Figure 4 Niobium carbide (Nb2CT) provided in Example 1 x )Elemental mapping diagram of Nb2O5 after oxidation of MXene material;
[0025] Figure 5 SEM image of the niobium aluminum carbide (Nb4AlC3) MAX phase ceramic material provided in Example 2;
[0026] Figure 6 The niobium aluminum carbide (Nb4AlC3) MAX phase ceramic material oxide Nb provided in Example 2 x O y SEM image;
[0027] Figure 7 SEM image of the niobium aluminum carbide (Nb2AlC) MAX phase ceramic material provided in Example 3;
[0028] Figure 8 The niobium aluminum carbide (Nb2AlC) MAX phase ceramic material oxide Nb provided in Example 3 x O y SEM image;
[0029] Figure 9 Niobium carbide (Nb2CT) provided in Example 1 x Thermogravimetric curves of MXene material;
[0030] Figure 10 Thermogravimetric curve of the niobium aluminum carbide (Nb4AlC3) MAX phase ceramic material provided in Example 2;
[0031] Figure 11 Thermogravimetric curve of the niobium aluminum carbide (Nb2AlC) MAX phase ceramic material provided in Example 3;
[0032] Figure 12 Niobium carbide (Nb2CT) provided in Example 1 x )Nb2O5xrd after oxidation of MXene material;
[0033] Figure 13 The charge-discharge curve of Nb2O5 as the negative electrode of lithium battery provided in Example 1;
[0034] Figure 14 The charge-discharge curves of S@Nb2O5 as a lithium-sulfur cathode provided in Example 1;
[0035] Figure 15 Charge-discharge curves of Nb2O5 as a sodium electrode provided in Example 1;
[0036] Figure 16 The niobium aluminum carbide (Nb4AlC3) MAX phase ceramic material oxide Nb provided in Example 2 x O y As the charge-discharge curve of the lithium battery negative electrode;
[0037] Figure 17 S@Nb provided for Example 2 x O y Charge-discharge curves of (Nb4AlC3 oxide) as a lithium-sulfur cathode;
[0038] Figure 18 The niobium aluminum carbide (Nb4AlC3) MAX phase ceramic material oxide Nb provided in Example 3 x O y As the charge-discharge curve of the lithium battery negative electrode;
[0039] Figure 19 S@Nb provided in Example 3x O y (Nb2AlC oxide) as lithium-sulfur cathode charge-discharge curve. Detailed Implementation
[0040] The technical solution of the present invention can be implemented in the following manner.
[0041] A niobium oxide composite energy storage material includes composite particles, the composite particles comprising a niobium oxide matrix and a non-metallic carbon material; the non-metallic carbon material is dispersed and loaded on the surface of the niobium oxide.
[0042] Preferably, the molecular formula of the niobium oxide matrix is Nb x O y It also exhibits a multi-layered, sheet-like structure.
[0043] Traditional lithium-ion batteries typically suffer from low energy density and high cost, sodium-ion batteries exhibit poor cycle stability, and lithium-sulfur batteries suffer from severe dissolution shuttle effects. Niobium oxide composite energy storage materials possess a multilayered structure, which effectively adsorbs lithium ions, forming surface capacitance and significantly increasing theoretical capacity. Furthermore, the layered structure provides efficient diffusion pathways for electrons and ions, mitigating volume expansion during material insertion / extraction, effectively suppressing the shuttle effect, and ensuring structural and electrochemical stability.
[0044] Preferably, the non-metallic carbon material is at least one of carbon nanotubes, SuperP, graphene, ethylene glycol, and glucose carbonization.
[0045] As a general technical concept, the present invention also provides a method for preparing the niobium oxide composite energy storage material as described above, characterized in that the method includes the following steps:
[0046] Step (1): Oxidize niobium-containing MXene materials to synthesize niobium oxide through oxidation;
[0047] Step (2): Add an appropriate amount of non-metallic carbon material to niobium oxide, stir and mix evenly, and then use a tube furnace under a carbon dioxide atmosphere to fully carbonize and obtain niobium oxide composite energy storage material.
[0048] Preferably, the oxidation synthesis method in step (1) is: directly oxidizing the niobium-containing MXene material in air or an oxygen atmosphere, and obtaining the niobium-containing oxide after full oxidation.
[0049] Preferably, the niobium-containing MXene material is niobium carbide (Nb2CT). xMXene or niobium aluminum carbide (Nb4AlC3)MAX phase ceramic materials or niobium aluminum carbide (Nb2AlC)MAX phase ceramic materials, calcined at a temperature of 350-1000℃, calcined for 1-10 hours, and heated at a rate of 1-10℃ / min.
[0050] Preferably, in step (2), the carbon material is at least one of carbon nanotubes, Super P, graphene, ethylene glycol and glucose carbonization; the carbonization temperature is 400-1000℃, the carbonization time is 0.5-6h, and the carbonization gas is carbon dioxide.
[0051] Preferably, the mass ratio of the non-metallic carbon material to niobium oxide is 1-10:1.
[0052] Preferably, the mixing and stirring time of the non-metallic carbon material and niobium oxide is 1-24 hours.
[0053] Preferably, the present invention also provides sodium-ion batteries, lithium-ion batteries, and lithium-sulfur batteries, comprising the above-mentioned niobium oxide composite energy storage material.
[0054] The technical solution and effects of the present invention will be further explained below through practical examples.
[0055] Example
[0056] Example 1
[0057] I. Preparation of Niobium Oxide Composite Energy Storage Materials
[0058] The product in this embodiment is the niobium oxide composite energy storage material of the present invention, and the non-metallic carbon material is selected from ethylene glycol high-temperature carbonization.
[0059] This embodiment prepares niobium oxide composite energy storage material according to the following method:
[0060] (1) Synthesis of niobium oxide: Niobium carbide (Nb2CT) is synthesized into niobium oxide. x Thermogravimetric analysis (TGA) was performed on MXene material, and the oxidation temperature was determined based on the TGA curves. Niobium carbide (Nb2CT) was subjected to oxidation in an oxygen atmosphere. x MXene material was placed in a tube furnace and heated at a rate of 2℃ / min to 750℃, and held for 4 hours to oxidize and synthesize niobium oxide.
[0061] Figure 1 This embodiment provides niobium carbide (Nb2CT) x SEM image of MXene material. Figure 2 , 3 Niobium carbide (Nb2CT) xThe field emission diagram of niobium oxide (Nb2O5) after oxidation of MXene material shows that the synthesized oxide has a multilayered sheet structure with good morphology. The morphology did not change after high-temperature oxidation, and the structure is relatively stable. Figure 9 Niobium carbide (Nb2CT) x The thermogravimetric curve of MXene material shows that the curve flattens out after oxidation to 750℃, and the material weight does not continue to increase. Figure 12 Niobium carbide (Nb2CT) x MXene material oxide xrd , The figure shows that the diffraction peaks correspond to the diffraction peaks of Nb₂O₅ and NbAlO₄. The formation of NbAlO₄ is due to the synthesis of niobium carbide (Nb₂CT). x It is difficult to completely remove Al elements when etching MXene materials with hydrofluoric acid. Figure 4 Niobium carbide (Nb2CT) x The elemental mapping diagram of Nb2O5 after oxidation of MXene material shows that the synthesized oxide contains Nb, O and a small amount of Al.
[0062] (2) Add an appropriate amount of ethylene glycol to niobium oxide (ethylene glycol and niobium oxide are in a mass ratio of 10:1), stir and mix evenly for 3 hours, place the mixture in a tube furnace, and carbonize at 800°C for 2 hours under a carbon dioxide atmosphere to obtain niobium oxide composite energy storage material.
[0063] II. Performance Testing
[0064] (1) Assembling lithium-ion batteries: The Nb2O5 composite energy storage material prepared in the example was used as the active material, PVDF as the binder, and conductive agents (SuperP and carbon nanotubes) were added. After stirring and slurry preparation, the mixture was coated onto copper foil and finally dried and rolled to obtain the negative electrode sheet. The ratio of active material: conductive agent: binder was 75:10:5:10. A lithium metal sheet was used as the counter electrode, a Celgard 2400 separator (Celgard Corporation, USA), and a 1M LiPF6 solution of ethylene carbonate (EC) + dimethyl carbonate (DMC) + diethyl carbonate (DEC) (VEC∶VDMC:VDEC=1∶1∶1) as the electrolyte to assemble lithium-ion batteries. Simulated batteries were assembled in an argon-filled glove box.
[0065] The test method for evaluating electrochemical performance is as follows:
[0066] 1. The surface morphology and particle size of the samples were observed using a Hitachi S4800 scanning electron microscope.
[0067] 2. Button battery charge / discharge performance test: Figure 13The figure shows the 25-cycle charge-discharge curve of the Nb2O5 composite anode material provided in this embodiment. As can be seen from the figure, the first-cycle discharge specific capacity of the composite material is 478.258 mAh / g, the 25-cycle charge specific capacity is 191.866 mAh / g, the discharge specific capacity is 191.874 mAh / g, and the charge-discharge rate after 25 cycles is 99.996%.
[0068] (2) Assembling a sodium-ion battery: The Nb2O5 composite energy storage material prepared in the example was used as the active material, PVDF as the binder, and conductive agents (SuperP and carbon nanotubes) were added. After stirring and slurry preparation, the mixture was coated onto copper foil and finally dried and rolled to obtain a negative electrode sheet. The ratio of active material: conductive agent: binder was 75:10:5:10. A lithium metal sheet was used as the counter electrode, a Celgard 2400 separator (Celgard Corporation, USA), and a 1 mol / L NaPF6 solution of ethylene carbonate (EC) + diethyl carbonate (DEC) (VEC:VDEC = 1:1) as the electrolyte to assemble a sodium-ion battery. A simulated battery was assembled in an argon-filled glove box.
[0069] The test method for evaluating electrochemical performance is as follows:
[0070] 1. The surface morphology and particle size of the samples were observed using a Hitachi S4800 scanning electron microscope.
[0071] 2. Button battery charge / discharge performance test: Figure 15 The figure shows the three-cycle charge-discharge curves of the Nb2O5 composite anode material provided in this embodiment. As can be seen from the figure, the first-cycle charge specific capacity of the composite material is 79.3 mAh / g, and the discharge specific capacity is 82.8 mAh / g.
[0072] (3) Assembling a lithium-sulfur battery: The Nb2O5 composite energy storage material prepared in the example was compounded with S in a ratio of 7:3, with S@Nb2O5 as the active material and PVDF as the binder. After adding a conductive agent (Super P), the mixture was stirred and slurried, then coated onto a carbon foil. Finally, the positive electrode was obtained by drying and rolling. The ratio of active material: conductive agent: binder was 7:2:1. A lithium metal sheet was used as the counter electrode, a Celgard 2400 separator (Celgard Corporation, USA), a 1M lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) mixed solution of ethylene glycol dimethyl ether (DME) and dioxolane (DOL) (volume ratio 1:1), and an electrolyte containing LiNO3 additive with a LiNO3 concentration of 2% were used to assemble a simulated lithium-sulfur battery in an argon-filled glove box.
[0073] The test method for evaluating electrochemical performance is as follows:
[0074] 1. The surface morphology and particle size of the samples were observed using a Hitachi S4800 scanning electron microscope.
[0075] 2. Button battery charge / discharge performance test: Figure 14 This figure shows the 25-cycle charge-discharge curves of the Nb2O5 composite anode material provided in this embodiment. As can be seen from the figure, the specific capacity of the composite material in the first charge cycle is 775.078 mAh / g, and the specific capacity in the second discharge cycle is 803.991 mAh / g. After 25 cycles, the specific capacity in the first charge cycle is 595.039 mAh / g, and the specific capacity in the second discharge cycle is 593.072 mAh / g. The charge-discharge rate remains close to 100% after 25 cycles.
[0076] Example 2
[0077] I. Preparation of Niobium Oxide Composite Energy Storage Materials
[0078] The product in this embodiment is the niobium oxide composite energy storage material of the present invention, and the non-metallic carbon material is selected from ethylene glycol high-temperature carbonization.
[0079] This embodiment prepares niobium oxide composite energy storage material according to the following method:
[0080] (1) Synthesis of niobium oxide: Thermogravimetric analysis (TGA) was performed on niobium aluminum carbide (Nb4AlC3)MAX phase ceramic material, and the oxidation temperature was determined based on the TGA curve. Under an oxygen atmosphere, the niobium aluminum carbide (Nb4AlC3)MAX phase ceramic material was placed in a tube furnace and heated at a rate of 1℃ / min until it reached 750℃. The temperature was maintained for 2 hours to oxidize and synthesize niobium oxide.
[0081] Figure 5 This embodiment provides SEM images of niobium aluminum carbide (Nb4AlC3)MAX phase ceramic materials. Figure 6 The image shows a SEM image of niobium oxide after oxidation of niobium aluminum carbide (Nb4AlC3)MAX phase ceramic material. As can be seen from the image, the synthesized oxide has a multilayer lamellar structure with good morphology. The morphology did not change after high-temperature oxidation, and the structure is relatively stable. Figure 10 The thermogravimetric curve of niobium aluminum carbide (Nb4AlC3)MAX phase ceramic material is shown in the figure. It can be seen from the figure that the curve flattens out after oxidation to 750℃, and the weight of the material does not continue to increase.
[0082] (2) Add an appropriate amount of ethylene glycol to niobium oxide (ethylene glycol and niobium oxide are in a mass ratio of 8:1), stir and mix evenly for 2 hours, place the mixture in a tube furnace, and carbonize at 700°C for 2 hours in a carbon dioxide atmosphere to obtain niobium oxide composite energy storage material.
[0083] II. Performance Testing
[0084] (1) Assembling lithium-ion batteries: The Nb prepared in the example was used to assemble lithium-ion batteries. x O yThe composite energy storage material was used as the active material, and the remaining steps were the same as in Example 1. The coin cell charge-discharge performance test was performed following the same steps as in Example 1, and the results are as follows: Figure 16 Niobium aluminum carbide (Nb4AlC3) MAX phase ceramic material oxide Nb x O y The charge-discharge curves of the lithium battery negative electrode are shown.
[0085] (2) Assembling lithium-sulfur batteries: The Nb prepared in the examples... x O y The composite energy storage material was compounded with S in a 7:3 ratio, with S@Nb2O5 as the active material. The remaining steps were the same as in Example 1. The coin cell charge-discharge performance was tested, following the same steps as in Example 1, and the results are as follows: Figure 17 S@Nb x O y The charge-discharge curves of (Nb4AlC3 oxide) as a lithium-sulfur cathode are shown.
[0086] Example 3
[0087] I. Preparation of Niobium Oxide Composite Energy Storage Materials
[0088] The product in this embodiment is the niobium oxide composite energy storage material of the present invention, and the non-metallic carbon material is selected from ethylene glycol high-temperature carbonization.
[0089] This embodiment prepares niobium oxide composite energy storage material according to the following method:
[0090] (1) Synthesis of niobium oxide: Thermogravimetric analysis (TGA) was performed on niobium aluminum carbide (Nb2AlC)MAX phase ceramic material, and the oxidation temperature was determined based on the TGA curve. Under an oxygen atmosphere, the niobium aluminum carbide (Nb2AlC)MAX phase ceramic material was placed in a tube furnace and heated at a rate of 5℃ / min to 750℃, and held for 1 hour to oxidize and synthesize niobium oxide.
[0091] Figure 7 This embodiment provides a SEM image of a niobium aluminum carbide (Nb2AlC) MAX phase ceramic material. Figure 8 The image shows the SEM image of niobium oxide after oxidation of niobium aluminum carbide (Nb2AlC)MAX phase ceramic material. As can be seen from the image, the synthesized oxide has a multilayer lamellar structure with good morphology. The morphology did not change after high-temperature oxidation, and the structure is relatively stable. Figure 11 The thermogravimetric curve of niobium aluminum carbide (Nb2AlC)MAX phase ceramic material is shown in the figure. It can be seen from the figure that the curve flattens out after oxidation to 750℃, and the weight of the material does not continue to increase.
[0092] (2) Add an appropriate amount of ethylene glycol to niobium oxide (ethylene glycol and niobium oxide are in a mass ratio of 6:1), stir and mix evenly for 1 hour, place the mixture in a tube furnace, and carbonize at 600°C for 1 hour in a carbon dioxide atmosphere to obtain niobium oxide composite energy storage material.
[0093] II. Performance Testing
[0094] (1) Assembling lithium-ion batteries: The Nb prepared in the example was used to assemble lithium-ion batteries. x O y The composite energy storage material was used as the active material, and the remaining steps were the same as in Example 1. The coin cell charge-discharge performance test was performed following the same steps as in Example 1, and the results are as follows: Figure 18 Niobium aluminum carbide (Nb4AlC3) MAX phase ceramic material oxide Nb x O y The charge-discharge curves of the lithium battery negative electrode are shown.
[0095] (2) Assembling lithium-sulfur batteries: The Nb prepared in the examples... x O y The composite energy storage material was compounded with S in a 7:3 ratio, with S@Nb2O5 as the active material. The remaining steps were the same as in Example 1. The coin cell charge-discharge performance was tested, following the same steps as in Example 1, and the results are as follows: Figure 19 S@Nb x O y The charge-discharge curves of (Nb4AlC oxide) as a lithium-sulfur cathode are shown.
Claims
1. A niobium oxide composite energy storage material, characterized in that: The composite particles include a niobium oxide matrix and a non-metallic carbon material; the non-metallic carbon material is dispersed and loaded on the surface of the niobium oxide matrix; the molecular formula of the niobium oxide matrix is Nb. x O y It has a multi-layered sheet structure; the non-metallic carbon material is at least one of carbon nanotubes, Super P, graphene, ethylene glycol and glucose carbonization.
2. The preparation method of the niobium oxide composite energy storage material as described in claim 1, characterized in that, Includes the following steps: a. Directly calcining and oxidizing niobium-containing MXene materials in air or an oxygen atmosphere to obtain niobium-containing oxides after complete oxidation; b. Mix the non-metallic carbon material with the niobium-containing oxide obtained in step a, and fully carbonize it under a carbon dioxide atmosphere to obtain a niobium oxide composite energy storage material; the non-metallic carbon material is at least one of carbon nanotubes, Super P, graphene, ethylene glycol and glucose carbonization.
3. The method for preparing the niobium oxide composite energy storage material according to claim 2, characterized in that: In step a, the niobium-containing MXene material is niobium carbide (Nb2CT). x Any one of MXene, niobium aluminum carbide (Nb4AlC3) MAX phase ceramic materials, and niobium aluminum carbide (Nb2AlC) MAX phase ceramic materials.
4. The method for preparing the niobium oxide composite energy storage material according to claim 2, characterized in that: In step a, the calcination oxidation temperature is 350-1000℃, the time is 1-10h, and the heating rate is 1-10℃ / min.
5. The method for preparing the niobium oxide composite energy storage material according to claim 2, characterized in that: In step b, the mass ratio of the non-metallic carbon material to the niobium oxide is 1-10:
1.
6. The method for preparing the niobium oxide composite energy storage material according to claim 2, characterized in that: In step b, the carbonization is carried out in a tube furnace at a temperature of 400-1000℃ for a time of 0.5-6 hours.
7. The application of niobium oxide composite energy storage materials, characterized by: Sodium-ion batteries, lithium-ion batteries, and lithium-sulfur batteries include the niobium oxide composite energy storage material as described in claim 1 and the niobium oxide composite energy storage material prepared by the preparation method of the niobium oxide composite energy storage material as described in any one of claims 2-6.
Citation Information
Patent Citations
Single crystal NaNbO3 cube as well as preparation method and application thereof
CN112251812A
Bimetallic niobium oxide and carbon composite material thereof, and preparation method and application thereof