A polyimide slurry, a polyimide film, a method for preparing the same, and their applications.
By using polyimide slurry with aromatic rigid structure and fluorine-containing groups and a four-step polycondensation reaction, the problems of high thermal expansion coefficient and low tensile strength of transparent polyimide films were solved, and high-performance polyimide films suitable for flexible display devices were prepared.
Patent Information
- Application Number
- CN202311557835.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-22
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-11-22
AI Technical Summary
Existing transparent polyimide films have a high coefficient of thermal expansion and low tensile strength, which cannot meet the requirements of flexible display technology.
A polyimide slurry containing aromatic rigid structure and fluorine-containing groups is used. The properties of polyimide are controlled through a four-step polycondensation reaction. The aromatic structure enhances the intermolecular forces, the fluorine-containing structure reduces the charge transfer within the molecular chain, and trimellitic anhydride is combined as a crosslinking end-capping agent to reduce the coefficient of thermal expansion and improve the tensile strength.
The prepared polyimide film has a lower coefficient of thermal expansion and higher tensile strength, meeting the performance requirements of flexible display technology.
Smart Images

Figure CN117586503B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of polymer materials technology, specifically relating to a polyimide slurry, a polyimide film, its preparation method, and its application. Background Technology
[0002] Flexible display devices refer to flexible electronic products with lightweight, bendable, and even foldable characteristics, including flexible thin-film transistor liquid crystal displays (TFT-LCDs) and flexible organic light-emitting diode (OLED) displays. Flexible display technology requires materials with high glass transition temperatures, low coefficients of thermal expansion, excellent mechanical properties, and high optical properties. During the fabrication of flexible display devices, annealing temperatures exceeding 350°C are necessary to improve film performance. During annealing, the device and substrate must not warp, crack, or delaminate. Therefore, the polyimide film needs to have a low coefficient of thermal expansion and a high glass transition temperature. Simultaneously, to improve the impact resistance of flexible displays, the polyimide film also needs to possess excellent mechanical properties.
[0003] In the prior art, polyimides prepared from monomers containing alicyclic structures and fluorinated monomers are commonly used as flexible substrate materials. For example, the prior art [J.Appl.Polym.Sci.2022,139(44),e53082] reported that the transparent polyimide film prepared using fluorinated dianhydride and fluorinated diamine has a glass transition temperature of 347℃, a coefficient of thermal expansion of 51ppm / K, a tensile strength of 109MPa, and a transmittance of 89% at 450nm. The prior art [ACSAppl.Polym.Mater.2023,5,602-613] reported that the transparent polyimide film prepared using alicyclic monomers and fluorinated monomers has a glass transition temperature of 406℃, a coefficient of thermal expansion of 29ppm / K, a tensile strength of 56.5MPa, and a transmittance of 88% at 450nm. Currently, most transparent polyimide films have a transmittance greater than 85% and a glass transition temperature exceeding 350°C. Their optical transmittance and glass transition temperature can meet the requirements of flexible display technology, but they still have defects such as a high coefficient of thermal expansion (>10ppm / k) and low tensile strength (<250MPa), which cannot meet the current technical requirements. Summary of the Invention
[0004] The purpose of this invention is to provide a polyimide slurry, a polyimide film, a method for preparing the same, and its applications. The polyimide film prepared using the polyimide slurry of this invention has a lower coefficient of thermal expansion and higher tensile strength.
[0005] To achieve the objectives of this invention, the following technical solutions are provided:
[0006] A polyimide slurry comprising a polyimide and an organic solvent, wherein the polyimide has the structure shown in Formula I:
[0007]
[0008] Where x is 0.85 to 0.95, y is 0.15 to 0.05, and n is the degree of polymerization of the polyimide.
[0009] Preferably, the organic solvent includes one or more of N-methylpyrrolidone, N,N-dimethylacetamide, and N,N-dimethylformamide; the polyimide slurry contains 18-20% polyimide by mass.
[0010] The present invention also provides a method for preparing the polyimide slurry described in the above technical solution, characterized by comprising the following steps:
[0011] 2,2'-bis(trifluoromethyl)benzidine, pyromellitic dianhydride and organic solvent were mixed and subjected to the first polycondensation reaction to obtain the first polycondensation product system.
[0012] The first polycondensation product system was mixed with hexafluorodianhydride to carry out a second polycondensation reaction, thereby obtaining the second polycondensation product system.
[0013] The second polycondensation product is heated to carry out a third polycondensation reaction, resulting in a third polycondensation product system.
[0014] The third polycondensation product system is mixed with trimellitic anhydride and subjected to a fourth polycondensation reaction to obtain the polyimide slurry.
[0015] Preferably, the molar ratio of 2,2'-bis(trifluoromethyl)benzidine, pyromellitic dianhydride, hexafluorodianhydride and trimellitic anhydride is 1.0-1.02:0.85-0.95:0.05-0.15:0.02-0.04.
[0016] Preferably, the temperatures of the first, second, and fourth polycondensation reactions are independently 15–35°C; the temperature of the third polycondensation reaction is 60–70°C; and the first, second, third, and fourth polycondensation reactions are carried out under stirring conditions, wherein the stirring rate is independently 100–250 rpm.
[0017] Preferably, the first polycondensation reaction takes 1.5 to 2 hours; the second polycondensation reaction takes 20 to 30 hours; the third polycondensation reaction takes 1 to 2 hours; and the fourth polycondensation reaction takes 1.5 to 2 hours.
[0018] The present invention also provides a polyimide film, which is prepared by coating a polyimide slurry onto a substrate and then drying and annealing it in sequence; wherein the polyimide slurry is the polyimide slurry described in the above technical solution or the polyimide slurry prepared by the preparation method described in the above technical solution.
[0019] Preferably, the drying temperature is 100-110°C and the time is 1-1.5 hours; the annealing temperature is 50-400°C and the holding time is 4-5 hours.
[0020] Preferably, the coating method is spin coating; the spin coating speed is 500-1000 rpm and the time is 80-100 s.
[0021] The present invention also provides the application of the polyimide film described in the above technical solution in flexible display devices.
[0022] This invention provides a polyimide slurry comprising a polyimide and an organic solvent, wherein the polyimide has the structure shown in Formula I:
[0023]
[0024] Where x is 0.85–0.95, y is 0.15–0.05, and n is the degree of polymerization of the polyimide. This invention utilizes the synergistic regulation of the properties of polyimide by its aromatic rigid structure and fluorinated groups. The conjugation effect of the aromatic structure strengthens the intermolecular forces, thereby improving the tensile strength of the polyimide; and the fluorinated structure reduces intramolecular charge transfer, thus improving the optical transmittance of the polyimide.
[0025] This invention also provides a method for preparing a polyimide film. By employing an annealing process, the tensile strength of the film is effectively improved to meet the requirements of flexible display technology. Furthermore, this invention uses trimellitic anhydride for a fourth polycondensation reaction. Triellitic anhydride, as a crosslinking end-capping agent, can partially crosslink the molecular chain segments, thereby reducing the coefficient of thermal expansion of the polyimide film. Attached Figure Description
[0026] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0027] Figure 1 This is a flowchart illustrating the preparation process of the polyimide slurry in this invention.
[0028] Figure 2 This is a flowchart illustrating the preparation process of the polyimide film in this invention. Detailed Implementation
[0029] This invention provides a polyimide slurry comprising a polyimide and an organic solvent, wherein the polyimide has the structure shown in Formula I:
[0030]
[0031] Where x is 0.85 to 0.95, y is 0.15 to 0.05, and n is the degree of polymerization of the polyimide.
[0032] In this invention, x is 0.85 to 0.95, preferably 0.90; y is 0.15 to 0.05, preferably 0.10; and n is the degree of polymerization of the polyimide. In this invention, n is preferably 10 to 10000.
[0033] In this invention, the organic solvent preferably includes one or more of N-methylpyrrolidone (NMP), N,N-dimethylacetamide (DMAC), and N,N-dimethylformamide (DMF), more preferably N-methylpyrrolidone. In this invention, the mass percentage of polyimide in the polyimide slurry is preferably 18-20%, more preferably 19%.
[0034] The present invention also provides a method for preparing the polyimide slurry described in the above technical solution, comprising the following steps:
[0035] 2,2'-bis(trifluoromethyl)benzidine, pyromellitic dianhydride and organic solvent were mixed and subjected to the first polycondensation reaction to obtain the first polycondensation product system.
[0036] The first polycondensation product system was mixed with hexafluorodianhydride to carry out a second polycondensation reaction, thereby obtaining the second polycondensation product system.
[0037] The second polycondensation product is heated to carry out a third polycondensation reaction, resulting in a third polycondensation product system.
[0038] The third polycondensation product system is mixed with trimellitic anhydride and subjected to a fourth polycondensation reaction to obtain the polyimide slurry.
[0039] In this invention, unless otherwise specified, all raw materials used in the preparation are preferably commercially available products.
[0040] This invention prepares polyimide using 2,2'-bis(trifluoromethyl)benzidine (TFMB), pyromellitic dianhydride (PMDA), hexafluorodianhydride (6FDA), and trimellitic anhydride (TMA) as monomers. The preferred molar ratio of 2,2'-bis(trifluoromethyl)benzidine, pyromellitic dianhydride, hexafluorodianhydride, and trimellitic anhydride is 1.0–1.02:0.85–0.95:0.05–0.15:0.02–0.04, more preferably 1:0.88:0.0986:0.0286. The preparation method of the polyimide slurry described in this invention is described in detail below.
[0041] In this invention, 2,2'-bis(trifluoromethyl)benzidine, pyromellitic dianhydride and an organic solvent are mixed and subjected to a first polycondensation reaction to obtain a first polycondensation product system.
[0042] In this invention, 2,2'-bis(trifluoromethyl)benzidine is preferably mixed with a portion of an organic solvent to dissolve the 2,2'-bis(trifluoromethyl)benzidine, yielding a 2,2'-bis(trifluoromethyl)benzidine solution. In this invention, the mixing is preferably carried out under stirring conditions, with a stirring rate preferably of 200–300 rpm, more preferably 250 rpm; the stirring time is preferably 20–40 min, more preferably 30 min. In this invention, the mass ratio of the portion of the organic solvent to 2,2'-bis(trifluoromethyl)benzidine is preferably 1:4–5, more preferably 1:4.26.
[0043] In this invention, the organic solvent is preferably heated before mixing, and the heating temperature is preferably 27-35°C, more preferably 30°C; the heating time is preferably 10-20 min, more preferably 15 min. In this invention, the heating is preferably carried out under stirring conditions, and the stirring rate is preferably 200-300 rpm, more preferably 250 rpm.
[0044] After obtaining a 2,2'-bis(trifluoromethyl)benzidine solution, the present invention mixes the 2,2'-bis(trifluoromethyl)benzidine, pyromellitic dianhydride, and the remaining organic solvent to carry out a first polycondensation reaction, obtaining a first polycondensation product system. In the present invention, the mixing is preferably carried out under stirring conditions, and the stirring rate is preferably 100-200 rpm, more preferably 150 rpm. In the present invention, the mixing temperature is preferably 10-15°C, more preferably 10°C. In the present invention, the mass ratio of the remaining organic solvent to pyromellitic dianhydride is preferably 1:4-5, more preferably 1:4.26.
[0045] In this invention, the first polycondensation reaction is preferably carried out under stirring conditions; the stirring rate is preferably 150-250 rpm, more preferably 200 rpm. In this invention, the temperature of the first polycondensation reaction is preferably 20-30°C, more preferably 25°C; the time of the first polycondensation reaction is preferably 1.5-2.5 h, more preferably 2 h.
[0046] After the first polycondensation reaction, the present invention preferably does not require any post-processing, and directly mixes the obtained first polycondensation product system with hexafluorodianhydride to carry out a second polycondensation reaction to obtain a second polycondensation product system.
[0047] In this invention, an organic solvent is preferably added during the second polycondensation reaction. Specifically, the first polycondensation product system, hexafluorodianhydride, and the added organic solvent are mixed. In this invention, the mixing is preferably carried out under stirring conditions, with a stirring rate preferably of 100–200 rpm, more preferably 150 rpm. In this invention, the mixing temperature is preferably 10–15°C, more preferably 10°C. In this invention, the mass ratio of the added organic solvent to hexafluorodianhydride is preferably 1:4–5, more preferably 1:4.26.
[0048] In this invention, the temperature and stirring rate of the second polycondensation reaction and the first polycondensation reaction are preferably the same. In this invention, the time for the second polycondensation reaction is preferably 20–30 h, more preferably 20–25 h.
[0049] Following the second polycondensation reaction, the present invention preferably does not require any post-processing and directly heats the obtained second polycondensation product to carry out a third polycondensation reaction, obtaining a third polycondensation product system. In the present invention, the temperature of the third polycondensation reaction is preferably 60–70°C, more preferably 65°C; the time of the third polycondensation reaction is preferably 1–2 hours, more preferably 1.5 hours. In the present invention, heating during the third polycondensation reaction can depolymerize some molecular chains, thus reducing the molecular weight distribution.
[0050] Following the third polycondensation reaction, the present invention preferably requires no post-processing and directly mixes the obtained third polycondensation product system with trimellitic anhydride to carry out a fourth polycondensation reaction, thereby obtaining the polyimide slurry. The present invention uses trimellitic anhydride for the fourth polycondensation reaction. Trimetriatic anhydride, as a crosslinking end-capping agent, can partially crosslink the molecular chain segments, reducing the coefficient of thermal expansion of the polyimide film.
[0051] In this invention, the mixing is preferably carried out under stirring conditions, and the stirring rate is preferably 100-200 rpm, more preferably 150 rpm. In this invention, the temperature and stirring rate of the fourth polycondensation reaction are preferably the same as those of the first polycondensation reaction. In this invention, the time of the fourth polycondensation reaction is preferably 1.5-2.5 h, more preferably 2 h.
[0052] In this invention, the first, second, third, and fourth polycondensation reactions are preferably carried out under a protective gas atmosphere; the protective gas is preferably one of nitrogen, oxygen, and nitrogen, more preferably nitrogen; in this invention, the flow rate of the protective gas is preferably 2 to 7 mL / min, more preferably 5 mL / min.
[0053] The present invention also provides a polyimide film, which is prepared by coating a polyimide slurry onto a substrate and then drying and annealing it in sequence; wherein the polyimide slurry is the polyimide slurry described in the above technical solution or the polyimide slurry prepared by the preparation method described in the above technical solution.
[0054] In this invention, the thickness of the polyimide film is preferably 8 to 15 μm, more preferably 10 μm.
[0055] This invention involves coating a polyimide slurry onto a substrate to obtain a substrate coated with the polyimide slurry. In this invention, the process of degassing the polyimide slurry is preferably performed before coating. The degassing method is preferably vacuum degassing, and the degassing time is preferably 0.5–1 hour. The substrate is preferably a glass substrate or a quartz substrate, more preferably a glass substrate. The process of cleaning and drying the substrate is also preferably performed before coating. Deionized water is preferably used for cleaning. The drying process preferably includes drying with compressed air followed by vacuum drying; the vacuum drying temperature is preferably 50–80°C, more preferably 60°C; and the time is preferably 0.5–1 hour.
[0056] In this invention, the coating method is preferably spin coating; the spin coating speed is preferably 500-1000 rpm, more preferably 800 rpm; the time is preferably 80-100 s, more preferably 100 s.
[0057] In this invention, the coating process preferably further includes degassing the substrate coated with the polyimide slurry. Preferably, the degassing method described above is the same as the degassing method described in this invention.
[0058] After obtaining the substrate coated with polyimide slurry, the present invention sequentially dries and anneals the substrate coated with polyimide slurry. In the present invention, the drying temperature is preferably 100–120°C, more preferably 100°C; the drying time is preferably 1–1.5 h, more preferably 1 h. In the present invention, the annealing temperature is preferably 50–400°C, and the holding time is preferably 4–6 h. In a specific embodiment of the present invention, the annealing is preferably performed as follows: 100–120°C for 0.5–1 h, 200–220°C for 0.5–1 h, 260–280°C for 0.5–1 h, 380–400°C for 0.2–0.5 h, and 30–50°C for 1.5–2 h. In the present invention, the oxygen content during annealing is preferably below 10,000 rpm, more preferably 2,000 rpm.
[0059] In this invention, after annealing, it is preferable to peel off the polyimide film. In this invention, the peeling method is preferably to peel off the polyimide film by washing it with water; the washing temperature is preferably 70-80°C, more preferably 80°C. In this invention, after washing, it is preferable to dry the polyimide film; the drying temperature is preferably 100-120°C, and the drying time is preferably 1-2 hours.
[0060] The present invention also provides the application of the polyimide film described in the above technical solution in flexible display devices.
[0061] To further illustrate the present invention, the polyimide slurry and polyimide film provided by the present invention will be described in detail below with reference to the accompanying drawings and embodiments, but they should not be construed as limiting the scope of protection of the present invention.
[0062] Example 1
[0063] according to Figure 1 The flowchart shown illustrates the preparation of polyimide slurry, with the following specific steps:
[0064] Under a nitrogen atmosphere (nitrogen flow rate of 5 mL / min), 85.51 g of N-methylpyrrolidone was placed in a three-necked flask and stirred at 25 °C and 250 rpm for 10 min. Then, it was mixed with 0.045 mol (14.37 g) of 2,2'-bis(trifluoromethyl)benzidine and 10.69 g of N-methylpyrrolidone for another 30 min to obtain a 2,2'-bis(trifluoromethyl)benzidine solution. After cooling to 10 °C, 0.04 mol (8.72 g) of pyromellitic dianhydride, 5.34 g of N-methylpyrrolidone and the above 2,2'-bis(trifluoromethyl)benzidine solution were stirred at 150 rpm for 0.5 h. Then, the temperature was raised to 25 °C and stirred at 200 rpm for 2 h to obtain the first polycondensation product system.
[0065] The first polycondensation product system was cooled to 10°C, and 0.0044 mol (1.97 g) hexafluorodianhydride, 5.34 g N-methylpyrrolidone and the above first polycondensation product system were stirred and mixed at 150 rpm for 0.5 h. Then the temperature was raised to 25°C and stirred at 200 rpm for 24 h to obtain the second polycondensation product system.
[0066] The second polycondensation product system was heated at 65°C for 1 hour and then cooled to 25°C to obtain the third polycondensation product system.
[0067] 0.0013 mol (0.26 g) trimellitic anhydride and the above third condensation product system were mixed at 25°C and 150 rpm, and then stirred at 25°C and 100 rpm for 2 h to obtain polyimide slurry.
[0068] Comparative Example 1
[0069] Under a nitrogen atmosphere (nitrogen flow rate of 5 mL / min), 85.51 g of N-methylpyrrolidone was placed in a three-necked flask and stirred at 25 °C and 250 rpm for 10 min. Then, it was mixed with 0.045 mol (14.37 g) of 2,2'-bis(trifluoromethyl)benzidine and 10.69 g of N-methylpyrrolidone for another 30 min to obtain a 2,2'-bis(trifluoromethyl)benzidine solution. After cooling to 10 °C, 0.04 mol (8.72 g) of pyromellitic dianhydride, 0.0044 mol (1.97 g) of hexafluorodianhydride, 10.68 g of N-methylpyrrolidone and the above 2,2'-bis(trifluoromethyl)benzidine solution were stirred at 150 rpm for 0.5 h. Then, the temperature was raised to 25 °C and stirred at 200 rpm for 2 h to obtain the first polycondensation product system.
[0070] The first polycondensation product system was heated at 65°C for 1 hour and then cooled to 25°C to obtain the second polycondensation product system.
[0071] At 25°C and 150 rpm, 0.0013 mol (0.25 g) trimellitic anhydride and the above second polycondensation product system were mixed, and then stirred at 25°C and 100 rpm for 2 h to obtain polyimide slurry.
[0072] Comparative Example 2
[0073] Under a nitrogen atmosphere (nitrogen flow rate of 5 mL / min), 100.06 g of N-methylpyrrolidone was placed in a three-necked flask and stirred at 25 °C and 250 rpm for 10 min. Then, it was mixed with 0.0505 mol (16.17 g) of 2,2'-bis(trifluoromethyl)benzidine and 12.51 g of N-methylpyrrolidone for another 30 min to obtain a 2,2'-bis(trifluoromethyl)benzidine solution. After cooling to 10 °C, 0.04 mol (8.72 g) of pyromellitic dianhydride, 0.01 mol (4.44 g) of hexafluorodianhydride, 12.51 g of N-methylpyrrolidone and the above 2,2'-bis(trifluoromethyl)benzidine solution were stirred at 150 rpm for 0.5 h. Then, the temperature was raised to 25 °C and stirred at 200 rpm for 2 h to obtain the first polycondensation product system.
[0074] The first polycondensation product system was heated at 65°C for 1 hour and then cooled to 25°C to obtain the second polycondensation product system.
[0075] At 25°C and 150 rpm, 0.0015 mol (0.29 g) trimellitic anhydride and the above second polycondensation product system were mixed, and then stirred at 25°C and 100 rpm for 2 h to obtain polyimide slurry.
[0076] Comparative Example 3
[0077] Under a nitrogen atmosphere (nitrogen flow rate of 5 mL / min), 118.76 g of N-methylpyrrolidone was placed in a three-necked flask and stirred at 25 °C and 250 rpm for 10 min. Then, it was mixed with 0.0577 mol (18.48 g) of 2,2'-bis(trifluoromethyl)benzidine and 14.85 g of N-methylpyrrolidone for another 30 min to obtain a 2,2'-bis(trifluoromethyl)benzidine solution. After cooling to 10 °C, 0.04 mol (8.72 g) of pyromellitic dianhydride, 0.0171 mol (7.62 g) of hexafluorodianhydride, 14.85 g of N-methylpyrrolidone and the above 2,2'-bis(trifluoromethyl)benzidine solution were stirred at 150 rpm for 0.5 h. Then, the temperature was raised to 25 °C and stirred at 200 rpm for 2 h to obtain the first polycondensation product system.
[0078] The first polycondensation product system was heated at 65°C for 1 hour and then cooled to 25°C to obtain the second polycondensation product system.
[0079] 0.0017 mol (0.33 g) trimellitic anhydride and the above second polycondensation product system were mixed at 25°C and 150 rpm, and then stirred at 25°C and 100 rpm for 2 h to obtain polyimide slurry.
[0080] Comparative Example 4
[0081] Under a nitrogen atmosphere (nitrogen flow rate of 5 mL / min), 85.51 g of N-methylpyrrolidone was placed in a three-necked flask and stirred at 25 °C and 250 rpm for 10 min. Then, it was mixed with 0.045 mol (14.37 g) of 2,2'-bis(trifluoromethyl)benzidine and 10.69 g of N-methylpyrrolidone for another 30 min to obtain a 2,2'-bis(trifluoromethyl)benzidine solution. After cooling to 10 °C, 0.04 mol (8.72 g) of pyromellitic dianhydride, 5.34 g of N-methylpyrrolidone and the above 2,2'-bis(trifluoromethyl)benzidine solution were stirred at 150 rpm for 0.5 h. Then, the temperature was raised to 25 °C and stirred at 200 rpm for 2 h to obtain the first polycondensation product system.
[0082] The first polycondensation product system was cooled to 10°C, and 0.0044 mol (1.97 g) hexafluorodianhydride, 5.34 g N-methylpyrrolidone and the above first polycondensation product system were stirred and mixed at 150 rpm for 0.5 h. Then the temperature was raised to 25°C and stirred at 200 rpm for 24 h to obtain the second polycondensation product system.
[0083] The second polycondensation product system was heated at 65°C for 1 hour and then cooled to 25°C to obtain the third polycondensation product system.
[0084] 0.0009 mol (0.17 g) trimellitic anhydride and the above third polycondensation product system were mixed at 25°C and 150 rpm, and then stirred at 25°C and 100 rpm for 2 h to obtain polyimide slurry.
[0085] Comparative Example 5
[0086] Under a nitrogen atmosphere (nitrogen flow rate of 5 mL / min), 85.51 g of N-methylpyrrolidone was placed in a three-necked flask and stirred at 25 °C and 250 rpm for 10 min. Then, it was mixed with 0.045 mol (14.37 g) of 2,2'-bis(trifluoromethyl)benzidine and 10.69 g of N-methylpyrrolidone for another 30 min to obtain a 2,2'-bis(trifluoromethyl)benzidine solution. After cooling to 10 °C, 0.04 mol (8.72 g) of pyromellitic dianhydride, 5.34 g of N-methylpyrrolidone and the above 2,2'-bis(trifluoromethyl)benzidine solution were stirred at 150 rpm for 0.5 h. Then, the temperature was raised to 25 °C and stirred at 200 rpm for 2 h to obtain the first polycondensation product system.
[0087] The first polycondensation product system was cooled to 10°C, and 0.0044 mol (1.97 g) hexafluorodianhydride, 5.34 g N-methylpyrrolidone and the above first polycondensation product system were stirred and mixed at 150 rpm for 0.5 h. Then the temperature was raised to 25°C and stirred at 200 rpm for 24 h to obtain the second polycondensation product system.
[0088] The second polycondensation product system was heated at 65°C for 1 hour and then cooled to 25°C to obtain the third polycondensation product system.
[0089] 0.00135 mol (0.259 g) trimellitic anhydride and the above third condensation product system were mixed at 25°C and 150 rpm, and then stirred at 25°C and 100 rpm for 2 h to obtain polyimide slurry.
[0090] Application examples
[0091] according to Figure 2 The flowchart shown illustrates the preparation of polyimide films, with the specific steps as follows:
[0092] The polyimide slurry was placed in a vacuum oven and degassed under vacuum at 25°C for 0.5 h to obtain a pretreated polyimide slurry.
[0093] The glass substrate (8-inch) was cleaned with deionized water, dried with compressed air, and then placed in a vacuum drying oven and heated at 60°C for 0.5 hours to obtain a pretreated glass substrate.
[0094] 20 mL of the pretreated polyimide slurry was measured and spin-coated at 500 rpm for 100 s to obtain a uniform polyimide wet film on the glass substrate surface.
[0095] The polyimide wet film was placed in a vacuum oven and degassed under vacuum at 25°C for 0.5 hours. Then it was placed in a forced-air drying oven and heated at 100°C for 1 hour to remove the solvent, thus obtaining a polyimide dry film.
[0096] The polyimide dry film was annealed in an oxygen-free oven under nitrogen protection with an oxygen content below 10,000 ppm; held at 120°C for 1 hour, 220°C for 0.5 hours, 280°C for 0.5 hours, 400°C for 0.2 hours, and 50°C for 2 hours. After naturally cooling to room temperature, it was removed and placed in deionized water, heated to 80°C, and peeled off to obtain a polyimide film preform. The polyimide film preform was then dried in a forced-air oven at 100°C for 1 hour to obtain the polyimide film. The polyimide slurry used in this application example was obtained from Example 1 and Comparative Examples 1-5, and the final polyimide films were designated as Sample 1 and Samples 2-6, respectively.
[0097] Test case
[0098] The glass transition temperature (Tg), coefficient of thermal expansion (CTE), average transmittance, tensile strength, elongation and elastic modulus of samples 1 and 2-6 were tested, and the results are shown in Table 1.
[0099] The specific testing method is as follows:
[0100] The glass transition temperature was measured using a thermomechanical analyzer (TMA), model TATMAQ400EM, under the following conditions: nitrogen atmosphere, preload force 0.05N, and heating rate 10K / min.
[0101] The coefficient of thermal expansion (CTE) was measured using a thermomechanical analyzer (TMA), model TATMA Q400EM, under the following conditions: nitrogen atmosphere, preload force 0.05N, heating rate 10K / min, and the average coefficient of thermal expansion was measured in the range of 50 to 350℃.
[0102] Transmittance was measured using a UV spectrophotometer, model UV7600PRO, and the transmittance measured at a wavelength of 450nm was taken as the 450nm transmittance.
[0103] Tensile strength, elongation, and modulus of elasticity were tested using a tensile testing machine, model Labthink C610, at a speed of 500 mm / min.
[0104] Table 1. Performance test results of polyimide films
[0105]
[0106]
[0107] As shown in Table 1, the polyimide film prepared by this invention has a glass transition temperature of 407℃, a coefficient of thermal expansion of 5.15ppm / K, an average transmittance of 86%, a tensile strength of 316MPa, an elongation of 20.9%, and an elastic modulus of 6.7GPa. Its performance is better than that of the polyimide film in the comparative example and can meet the requirements of flexible display technology.
[0108] Although the above embodiments have provided a detailed description of the present invention, they are only some embodiments of the present invention, and not all embodiments. People can obtain other embodiments based on these embodiments without creative effort, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A method for preparing a polyamic acid slurry, characterized in that, The steps are as follows: Under a nitrogen atmosphere with a nitrogen flow rate of 5 mL / min, 85.51 g of N-methylpyrrolidone was placed in a three-necked flask and stirred at 25°C and 250 rpm for 10 min. Then, it was mixed with 14.37 g of 2,2'-bis(trifluoromethyl)benzidine and 10.69 g of N-methylpyrrolidone for another 30 min to obtain a 2,2'-bis(trifluoromethyl)benzidine solution. After cooling to 10°C, 8.72 g of pyromellitic dianhydride, 5.34 g of N-methylpyrrolidone, and the above 2,2'-bis(trifluoromethyl)benzidine solution were stirred at 150 rpm for 0.5 h. Then, the temperature was raised to 25°C and stirred at 200 rpm for 2 h to obtain the first polycondensation product system. The first polycondensation product system was cooled to 10°C, and 1.97g of hexafluorodianhydride, 5.34g of N-methylpyrrolidone and the first polycondensation product system were stirred and mixed at 150 rpm for 0.5 h. Then the temperature was raised to 25°C and stirred at 200 rpm for 24 h to obtain the second polycondensation product system. The second polycondensation product system was heated at 65°C for 1 hour and then cooled to 25°C to obtain the third polycondensation product system. 0.0013 mol trimellitic anhydride and the above third condensation product system were mixed at 25°C and 150 rpm, and then stirred at 25°C and 100 rpm for 2 h to obtain polyamic acid slurry.
2. A polyimide film characterized by comprising a polyimide film according to claim 1, wherein the polyimide film has a thickness of 5 to 50 μm. The polyamic acid slurry is prepared by coating a substrate with a polyamic acid slurry and then drying and annealing it. The polyamic acid slurry is the polyamic acid slurry prepared by the method described in claim 1.
3. The polyimide film according to claim 2, characterized by The drying temperature is 100~110℃ and the time is 1~1.5h; the annealing temperature is 50~400℃ and the holding time is 4~5h.
4. The polyimide film according to claim 2, wherein The coating method is spin coating; the spin coating speed is 500~1000 rpm, and the time is 80~100s.
5. The application of the polyimide film according to any one of claims 2 to 4 in flexible display devices.
Citation Information
Patent Citations
Method for preparing polyamic acid, and polyamic acid, polyimide resin and polyimide film manufactured thereby
CN111542562A
Polyimide film and method for manufacturing same
KR1020140049382A