Seed crystal holder and preparation method thereof, crystal growth device, crystal growth method
By opening grooves on the seed crystal holder and filling them with different thermal conductive materials, the temperature field of the silicon carbide crystal is modulated, which solves the problem of high dislocation density in silicon carbide single crystal materials and achieves reduction of screw dislocation density and improvement of growth temperature. Uniformity effect, suitable for large-scale production.
Patent Information
- Application Number
- CN202311547649.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-15
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-11-15
AI Technical Summary
During the formation process of existing silicon carbide single crystal materials, the dislocation density of silicon carbide crystals is high, especially the high screw dislocation density, which leads to an increase in device leakage current, and the existing methods for reducing dislocation density are complex and unsuitable for scale. chemical production.
Seed crystal holders with different thermal conductivity properties are used, and grooves are opened on the surface of the seed crystal holder and filled with different thermal conductive materials to modulate the temperature field of the seed crystal, promote the nucleation and lateral growth of silicon carbide crystals in the low temperature area, and reduce the spiral shape. Dislocation density.
It effectively reduces the screw dislocation density of silicon carbide single crystal materials, improves the uniformity of crystal growth temperature, simplifies the process, and is suitable for large-scale production and popularization.
Smart Images

Figure CN117587501B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the field of semiconductor chip technology, and in particular to a seed crystal tray and a preparation method thereof, a crystal growth device, and a crystal growth method. Background Art
[0002] Silicon carbide single crystal material has a wide bandgap, high thermal conductivity, high breakdown electric field and high electron saturation migration rate. It is one of the most widely used wide bandgap semiconductor materials and is also a material with relatively mature crystal growth technology and device manufacturing level. Therefore, it is widely used in high-temperature, high-frequency, radiation-resistant and high-power devices.
[0003] At present, the formation process of silicon carbide single crystal material mainly adopts high-purity silicon carbide powder, and obtains silicon carbide crystal by high-temperature sublimation at a temperature of more than 2000 degrees through the physical vapor transport process (PVT). In the silicon carbide single crystal material prepared by the above process, the dislocation density of silicon carbide crystal is still at a relatively high level, so it is very necessary to reduce the dislocation density, especially the density of threading screw dislocation (TSD), because the threading screw dislocation belongs to the threading dislocation, which can be inherited to the growing crystal through the seed crystal during the crystal growth process, which will lead to an increase in the leakage current of the device prepared by the crystal. Summary of the invention
[0004] Embodiments of the present disclosure provide a seed crystal holder and a preparation method thereof, a crystal growth device, and a crystal growth method, which are intended to reduce the dislocation density in silicon carbide single crystal materials.
[0005] To achieve the above objectives, the embodiments of the present disclosure adopt the following technical solutions:
[0006] On the one hand, a seed crystal holder is provided. The seed crystal holder includes a seed crystal holder body and a plurality of filling parts. A first surface of the seed crystal holder body is provided with a plurality of grooves, the plurality of grooves are arranged at intervals, and the first surface is used to place seed crystals. The plurality of filling parts are arranged in the plurality of grooves correspondingly. The material of the filling part includes a first material, the material of the seed crystal holder body includes a second material, and the thermal conductivity of the first material is different from the thermal conductivity of the second material.
[0007] In the seed crystal holder provided by the above-mentioned embodiment of the present disclosure, the thermal conductivity of the first material is different from the thermal conductivity of the second material, so that the thermal conductivity of the filling part is different from the thermal conductivity of the seed crystal holder body; in this way, by modulating the shape and distribution of the multiple filling parts and the thermal conductivity of the first material, the temperature field of the surface of the seed crystal holder on which the seed crystal is arranged can be modulated, so that the temperature field of the seed crystal attached to the seed crystal holder can be modulated; in this way, after heat conduction, the regional temperature distribution (for example, radial temperature distribution) of the growth surface of the silicon carbide crystal (for example, the C surface of the seed crystal) can be changed, so that a plurality of low-temperature regions are formed on the growth surface of the seed crystal (that is, the growth surface of the silicon carbide crystal), so that the crystal preferentially nucleates in the plurality of low-temperature regions at the same time, and after nucleation, the crystal growth in the 0001 direction of the non-preferential growth region (for example, the region located between the two low-temperature regions) is blocked by lateral growth perpendicular to the 0001 plane (that is, the plane parallel to and opposite to the C plane), so that the crystal growth mode is changed, and the TSD density of the growing crystal is reduced. At the same time, the above arrangement can improve the temperature uniformity of the seed crystal holder and reduce the sublimation of the seed crystal material from the back. Moreover, the above arrangement will not affect the structure and internal stress of the seed crystal, the process is simple, the feasibility is high, and it is convenient to prefabricate, which is conducive to large-scale production and promotion and application.
[0008] In some embodiments, the thermal conductivity of the first material is smaller than the thermal conductivity of the second material, and the minimum size of the bottom surface of the groove is in the range of 10 to 100 μm.
[0009] In some embodiments, the thermal conductivity of the first material is greater than the thermal conductivity of the second material, and the minimum distance between two adjacent grooves ranges from 10 to 100 μm.
[0010] In some embodiments, the size of the groove in the second direction ranges from 10 to 500 μm, and the second direction is the thickness direction of the seed holder body.
[0011] In some embodiments, the plurality of grooves are evenly distributed on the seed tray body along a third direction; the third direction is a direction from the geometric center of the seed tray body to the boundary of the seed tray body.
[0012] In some embodiments, the plurality of grooves are distributed on the seed crystal holder body according to a predetermined rule, wherein the predetermined rule includes: along a third direction, the distribution density of the plurality of grooves on the seed crystal holder body gradually decreases; and the third direction is the direction from the geometric center of the seed crystal holder body to the boundary of the seed crystal holder body.
[0013] In some embodiments, the plurality of grooves are divided into a plurality of groove groups, and the groove group includes at least one groove. In the case where the groove group includes one groove, the groove is located at the geometric center of the seed crystal holder body. In the case where the groove group includes a plurality of grooves, the plurality of grooves included in the groove group surround the geometric center of the seed crystal holder body. Along the third direction, there is a first interval between each two adjacent groove groups. The plurality of first intervals are equal; or, along the third direction, the plurality of first intervals gradually increase; the third direction is the direction from the geometric center of the seed crystal holder body to the boundary of the seed crystal holder body.
[0014] In some embodiments, a ratio of a maximum value in the first interval to a minimum value in the first interval is less than or equal to 3.
[0015] In some embodiments, a surface of the filling portion away from the bottom surface of the groove is flush with the first surface; and a surface of the seed crystal holder on which the seed crystal is disposed has a flatness less than or equal to 150 μm.
[0016] In some embodiments, the first material includes any one or more of tantalum, tantalum carbide and silicon carbide; and / or the second material is graphite.
[0017] In some embodiments, the material forming the filling part further includes modified epoxy resin.
[0018] In some embodiments, in the material forming the filling portion, the mass ratio of the first material to the modified epoxy resin is in the range of 3:1 to 5:1.
[0019] On the other hand, a method for preparing a seed crystal holder is provided. The preparation method comprises: providing an initial seed crystal holder body. Forming a plurality of grooves on the first initial surface of the initial seed crystal holder body; the plurality of grooves are arranged at intervals; the first initial surface of the initial seed crystal holder body forms the first surface of the seed crystal holder body, and the first surface is used to set the seed crystal. Filling the plurality of grooves forms a plurality of filling parts correspondingly. The material of the filling parts comprises a first material, the material of the initial seed crystal holder body comprises a second material, and the thermal conductivity of the first material is different from the thermal conductivity of the second material.
[0020] In some embodiments, the groove is a cylindrical groove; forming a plurality of grooves on the first initial surface of the initial seed crystal holder body includes: using a laser process to groove a set area of the first initial surface to form a plurality of grooves.
[0021] In some embodiments, the groove is a prism-shaped groove; forming a plurality of grooves on the first initial surface of the initial seed crystal holder body includes: using an etching process to groove a set area of the first initial surface to form a plurality of grooves.
[0022] In another aspect, a crystal growth device is provided, comprising the above-mentioned seed crystal holder, a crucible body and a crucible cover disposed on the crucible body, wherein the seed crystal holder is connected to the inner surface of the crucible cover.
[0023] In another aspect, a crystal growth method is provided, which is implemented based on the above-mentioned crystal growth device.
[0024] In some embodiments, in the crystal growth method, the crystal growth process includes: in the first growth stage, nucleation growth to form a crystal nucleus; the growth temperature of the first growth stage is 2150°C, and the insulation time is 8 to 12 hours. In the second growth stage, the crystal growth is continued to form a crystal growth body; the growth temperature of the second growth stage is 2280 to 2380°C, and the pressure of the growth environment is 400 to 800Pa.
[0025] It can be understood that the beneficial effects that can be achieved by the preparation method of the seed crystal tray, the crystal growth device, and the crystal growth method provided in the above embodiments of the present disclosure can refer to the beneficial effects of the seed crystal tray described above, and will not be repeated here. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the technical solutions in the present disclosure, the following briefly introduces the drawings required to be used in some embodiments of the present disclosure. Obviously, the drawings described below are only drawings of some embodiments of the present disclosure. For ordinary technicians in this field, other drawings can also be obtained based on these drawings. In addition, the drawings described below can be regarded as schematic diagrams, and are not limitations on the actual size of the product involved in the embodiments of the present disclosure, the actual process of the method, the actual timing of the signal, etc.
[0027] Figure 1 is a schematic structural diagram of a crystal growth device according to some embodiments;
[0028] Figure 2 is a schematic structural diagram of a seed crystal holder according to some embodiments;
[0029] Figure 3 is a schematic structural diagram of a seed crystal holder according to some other embodiments;
[0030] Figure 4 is a schematic structural diagram of a seed crystal according to some further embodiments;
[0031] Figure 5 is a schematic structural diagram of a seed crystal according to some further embodiments;
[0032] Figure 6 is a schematic structural diagram of a seed crystal holder according to some other embodiments;
[0033] Figure 7is a schematic structural diagram of a seed crystal holder according to some other embodiments;
[0034] Figure 8 is a schematic structural diagram of a seed crystal holder according to some other embodiments;
[0035] Fig. 9 is a schematic flow chart of a method for preparing a seed crystal tray according to some embodiments;
[0036] Fig.10 is a schematic diagram of step S2 in a method for preparing a seed crystal tray according to some embodiments;
[0037] Fig.11 is a schematic structural diagram of a crystal growth device according to some further embodiments;
[0038] Fig.12 is a schematic flow chart of a crystal growth method according to some embodiments;
[0039] Fig.13 is a schematic diagram of a structure for forming a crystal growth body in a crystal growth method according to some embodiments;
[0040] Fig.14 is a metallographic microscope photograph of a crystal growth body according to some embodiments. DETAILED DESCRIPTION
[0041] The following will be combined with the accompanying drawings to clearly and completely describe the technical solutions in some embodiments of the present disclosure. Obviously, the described embodiments are only part of the embodiments of the present disclosure, rather than all the embodiments. Based on the embodiments provided by the present disclosure, all other embodiments obtained by ordinary technicians in this field belong to the scope of protection of the present disclosure.
[0042] In the description of the present disclosure, it should be understood that the terms "center", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc., indicating orientations or positional relationships, are based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present disclosure and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present disclosure.
[0043] Unless the context requires otherwise, throughout the specification and claims, the term "including" is to be interpreted as an open, inclusive meaning, that is, "including, but not limited to". In the description of the specification, the terms "one embodiment", "some embodiments", "exemplary embodiments", "exemplarily" or "some examples" and the like are intended to indicate that specific features, structures, materials or characteristics associated with the embodiment or example are included in at least one embodiment or example of the present disclosure. The schematic representation of the above terms does not necessarily refer to the same embodiment or example. In addition, the specific features, structures, materials or characteristics may be included in any one or more embodiments or examples in any appropriate manner.
[0044] In the following, the terms "first" and "second" are used for descriptive purposes only and are not to be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of the embodiments of the present disclosure, unless otherwise specified, "plurality" means two or more.
[0045] “At least one of A, B and C” has the same meaning as “at least one of A, B or C”, and both include the following combinations of A, B and C: only A, only B, only C, a combination of A and B, a combination of A and C, a combination of B and C, and a combination of A, B and C. “A and / or B” includes the following three combinations: only A, only B, and a combination of A and B.
[0046] Additionally, the use of “based on” is meant to be open and inclusive, as a process, step, calculation, or other action “based on” one or more stated conditions or values may, in practice, be based on additional conditions or values beyond those stated.
[0047] As used herein, "about," "substantially," or "approximately" includes the stated value and an average value that is within an acceptable range of variation from the particular value as determined by one of ordinary skill in the art taking into account the measurements in question and the errors associated with the measurement of the particular quantity (i.e., the limitations of the measurement system).
[0048] Exemplary embodiments are described herein with reference to cross-sectional views and / or plan views that are idealized exemplary drawings. In the drawings, the thickness of layers and regions are exaggerated for clarity. Therefore, variations in shape relative to the drawings due to, for example, manufacturing techniques and / or tolerances are conceivable. Therefore, the exemplary embodiments should not be interpreted as being limited to the shapes of the regions shown herein, but include shape deviations due to, for example, manufacturing. For example, an etched region shown as a rectangle will typically have curved features. Therefore, the regions shown in the drawings are schematic in nature, and their shapes are not intended to illustrate the actual shape of regions of the device, and are not intended to limit the scope of the exemplary embodiments.
[0049] As used herein, the term "substrate" refers to a material on which subsequent material layers may be added. The substrate itself may be patterned. The material added to the substrate may be patterned or may remain unpatterned. In addition, the substrate may include a variety of semiconductor materials such as silicon, germanium, gallium arsenide, indium phosphide, etc. Alternatively, the substrate may be made of non-conductive materials such as glass, plastic, or sapphire wafers.
[0050] The technical terms in the embodiments of the present application are described as follows:
[0051] The hexagonal crystal system refers to the crystal affiliation in which there are six-fold or six-fold anti-axis characteristic symmetry elements in the direction of the c-crystal axis, the only high-order axis. The hexagonal crystal system is also called the "hexagonal galaxy" and belongs to the intermediate crystal family. In the hexagonal crystal system, the four crystal axes a1, a2, a3 and c are usually used to calibrate the crystal plane index and crystal direction index to reflect the crystal direction and crystal plane of the hexagonal crystal system atoms. Among them, the crystal direction refers to the direction of the array of points in the space lattice (the direction of the straight line connecting any node column in the lattice). In the hexagonal crystal system, the crystal direction is used to indicate certain directions in the crystal, involving the position of atoms in the crystal, the direction of atomic columns, and marking the direction of a group of parallel and consistent straight lines. The crystal plane refers to a plane passing through any lattice point in the space lattice (a plane formed by nodes in the lattice). In the hexagonal crystal system, the crystal plane is used to indicate the plane formed by atoms in the crystal.
[0052] It should be noted that the labels "A to B" appearing in the drawings mean that structure / region A belongs to structure / region B, that is, the structure referred to by the labels is both structure A and structure B. For example, Fig.11 The "51-50" in the figure means that the structure indicated by the reference number is an induction heating coil, and the induction heating coil 51 belongs to the heating assembly 50. The reference numbers "A / B" appearing in the drawings mean that the structure / area A and the structure / size B can be referred to by the same structure / size, for example, Figure 7 "L1 / L1 min ” refers to the smallest L1 between the first interval L1 and the first interval L1 minThis size can be used to refer to both.
[0053] As mentioned in the background, silicon carbide single crystal materials are widely used in high-temperature, high-frequency, radiation-resistant, and high-power devices. With the expansion of the market scale and the need to reduce costs, the preparation of large-size and low-defect-density silicon carbide crystals is currently in urgent need. Among them, the defect density of silicon carbide crystals includes dislocation defect density and micropipe defect density (Micropipe density, MPD); dislocation defect density includes threading screw dislocation (TSD) density, ductile dislocation (TED) density, and basal plane dislocation (BPD) density.
[0054] In the related art, when a silicon carbide single crystal is formed by a physical vapor transport method, Figure 1 As shown, medium frequency electromagnetic induction heating is adopted; the crystal growth device 100 used includes: a crucible 40, a seed crystal holder 10 and an induction heating coil 51. Among them, the crucible 40 includes a crucible body 20 and a crucible cover 30; the seed crystal holder 10 is connected to the inner surface of the crucible cover 30; the seed crystal 60 is bonded to the seed crystal holder 10; and the induction heating coil 51 is wound on the outer peripheral wall of the crucible 40. The heating principle is that after the induction heating coil 51 coaxial with the crucible 40 is energized, eddy currents are generated on the surface of the crucible 40 due to the skin effect, thereby generating Joule heat, providing heat to the crystal growth device 100, so that the raw material (for example, silicon carbide powder K) is sublimated at high temperature, and the sublimated raw material is crystallized on the surface of the seed crystal 60 to form a silicon carbide single crystal.
[0055] In the above technology, when the induction heating coil 51 provides heat, the temperature required for crystal growth is provided by heating all around, and the heat is transferred from the crucible wall from the outside to the inside, which will form an axial temperature gradient in the inner cavity of the crucible 40, as well as a radial temperature gradient distributed radially along the seed crystal 60, resulting in uneven temperature in the crucible 40, and the temperature at the edge of the seed crystal 60 is higher than the temperature at the center of the seed crystal 60. In this case, crystal growth generally nucleates preferentially in the central area of the seed crystal 60, and the defects inherited from the seed crystal 60 generally extend to the growing crystal, so that the dislocation defect density in the grown crystal is higher, and the dislocation defect density is higher than the micropipe defect density. In some examples, the micropipe defect density on a 6-foot silicon carbide single crystal has reached less than 1e.a / cm 2 , and even close to zero micropipe defects; the micropipe defect density on 8-inch silicon carbide single crystal is also close to the above level; while the dislocation defect density (including TSD density, BPD density and TED density) is greater than 5000e.a / cm 2Therefore, as mentioned in the background, it is necessary to reduce the dislocation density, especially the density of threading screw dislocation (TSD), to avoid leakage current in the device prepared by growing the crystal. In addition, since the edge temperature of the seed crystal 60 is higher than the temperature at the center of the seed crystal 60, it is easy to form uniformly distributed high temperature points, resulting in local sublimation of the material of the seed crystal 60, making the thickness of the seed crystal 60 locally thinner, and even causing the seed crystal 60 to melt.
[0056] At present, the growth plane of silicon carbide crystal is mainly 000-1 plane (also called carbon plane, C plane). In some implementations, in order to reduce the dislocation density of silicon carbide single crystal, attempts are made to grow the crystal on different growth planes, such as 11-20 plane, 1-100 plane or 0001 plane (also called Si plane), etc. Although some crystals with lower TSD density are obtained, undesirable effects such as complex process and higher stacking fault (SF) are produced.
[0057] In some other implementations, such as Figure 4 As shown, by making a groove on the back side 60b of the seed crystal 60 (i.e., the surface opposite to the growth surface 60a), and filling the groove with a material having a thermal conductivity different from that of silicon carbide, or directly coating the back side 60b of the seed crystal 60 with a thin film made of a material having a thermal conductivity different from that of silicon carbide, the axial temperature gradient on the surface of the seed crystal 60 during the crystal growth process is changed; in this way, there are two materials with different thermal conductivities on the back side 60b of the seed crystal 60, which makes the heat dissipation uneven, and at the same time makes the temperature field on the surface of the seed crystal 60 unevenly distributed. Therefore, the periodic distribution of the two materials with different thermal conductivities located on the back side of the seed crystal 60 can be used to modulate the temperature field distribution on the surface of the seed crystal 60 during the growth of silicon carbide (SiC) by the physical vapor transport method, forcing the preferential nucleation in the lower temperature area corresponding to the predefined pattern, selectively growing preferentially according to the predefined pattern, and then growing laterally, so as to achieve the purpose of reducing the threading dislocation density. However, in this implementation, since it is necessary to groove the back of the seed crystal 60 or to coat a thin film, there is a problem that the structure of the seed crystal 60 and the processing process are relatively complicated.
[0058] In other implementations, such as Figure 5As shown, the growth surface 60a of the seed crystal 60 is patterned by coating photoresist and plasma etching to obtain a patterned substrate for growing crystals, and the substrate is cleaned and then transferred for crystal growth. By setting in this way, the radial temperature distribution of the growth surface 60a of the seed crystal can be modulated, so that when the crystal grows, it starts to grow preferentially at the groove U, and in the groove U (i.e., the part between the conical protrusions J), the defect growth direction is converted from parallel growth (i.e., longitudinal growth) to lateral growth, so as to achieve the purpose of reducing the crystal defect density. However, in this implementation, the surface of the seed crystal 60 also needs to be etched, and particle bombardment reaction and chemical reaction will occur during the etching process, which will have a certain impact on the structure and surface energy of the seed crystal 60. In addition, the cleaning method is relatively special, which greatly increases the manufacturing cost.
[0059] Based on this, Figure 2 As shown, some embodiments of the present disclosure provide a seed crystal holder. The seed crystal holder 10 includes a seed crystal holder body 11 and a plurality of filling parts 12. A first surface 11a of the seed crystal holder body 11 is provided with a plurality of grooves 13, and the plurality of grooves 13 are arranged at intervals. The first surface 11a is used to arrange the seed crystal 60. The plurality of filling parts 12 are correspondingly arranged in the plurality of grooves 13. The material of the filling part 12 includes a first material, the material of the seed crystal holder body 11 includes a second material, and the thermal conductivity of the first material is different from the thermal conductivity of the second material.
[0060] The first surface 11a is used to set the seed crystal 60, which means that the seed crystal 60 is located on the first surface 11a, and the surface of the seed crystal 60 close to the first surface 11a (for example, the Si surface) is attached to the first surface 11a, thereby realizing the connection between the seed crystal 60 and the seed crystal holder body 11. Here, there is no limitation on the connection method between the seed crystal 60 and the first surface 11a. For example, the seed crystal 60 can be bonded to the first surface 11a by an adhesive. It should be noted that when the first surface 11a of the seed crystal holder body 11 is provided with a plurality of grooves 13, the surface shared by the seed crystal holder body 11 and the grooves 13 does not belong to the first surface 11a of the seed crystal holder body 11.
[0061] The plurality of filling parts 12 are correspondingly arranged in the plurality of grooves 13. Figure 2 As shown, the number of filling parts 12 can be equal to the number of grooves 13. In this case, multiple filling parts 12 are arranged one-to-one in multiple grooves 13; or, the number of filling parts 12 can be less than the number of grooves 13. In this case, filling parts 12 are arranged one-to-one in a part of the grooves 13, and filling parts 12 are not arranged in another part of the grooves 13.
[0062] Here, there is no limitation on the type of the second material, as long as it can withstand the high temperature environment when the silicon carbide single crystal is formed by the physical vapor transport method. For example, the second material may be graphite.
[0063] Here, there is no limitation on the type of the first material, as long as it is different from the second material and can withstand the high temperature environment when forming silicon carbide single crystals by physical vapor transport.
[0064] Understandably, if Figure 2 As shown, when the thermal conductivity of the first material is different from the thermal conductivity of the second material, the thermal conductivity of the filling portion 12 is different from that of the seed crystal holder body 11; at the same time, since the first surface 11a of the seed crystal holder body 11 and the surface 12a of the filling portion 12 away from the bottom surface 13a of the groove 13 jointly form the surface 10a of the seed crystal holder 10 where the seed crystal 60 is arranged; in this way, by modulating the shapes and distribution of the plurality of filling portions 12 and the thermal conductivity of the first material, the temperature field of the surface 10a of the seed crystal holder 10 where the seed crystal 60 is arranged can be modulated, and the temperature field includes not only the temperature field of the surface 12a of the filling portion 12 away from the bottom surface 13a of the groove 13, but also the temperature field of the first surface 11a of the seed crystal holder body 11, so that the temperature field of the seed crystal 60 attached to the seed crystal holder 10 can be modulated; in this way, after heat conduction, the growth surface of the silicon carbide crystal (for example, the growth surface of the seed crystal) can be changed. The regional temperature distribution (for example, radial temperature distribution) of the C surface 60a of the seed crystal 60 is compared with the situation in the related art where the edge temperature of the seed crystal 60 is higher than the temperature at the center of the seed crystal 60, so that multiple low-temperature regions Q are formed on the growth surface 60a of the seed crystal 60 (i.e., the growth surface of the silicon carbide crystal), so that the crystal preferentially nucleates in the multiple low-temperature regions Q at the same time, and after nucleation, according to the step flow theory of silicon carbide crystal growth, the step surfaces of multiple nucleation centers will diffuse outward at the same time, and finally connect into one piece. In this process, the TSD dislocations in the seed crystal 60 will be transformed into BPD dislocations or disappear due to the lateral growth of the crystal; that is, the crystal growth in the 0001 direction of the non-preferential growth area (for example, the area P located between the two low-temperature regions Q) can be blocked by lateral growth perpendicular to the 0001 surface (i.e., perpendicular to the C surface 60a), so that the crystal growth pattern can be changed, and the TSD density of the growing crystal can be reduced. Here, the crystal growth in the 0001 direction refers to the growth along the Figure 2 Crystal growth in the second direction Y.
[0065] At the same time, through the above arrangement, compared with the situation in which uniformly distributed high-temperature points are formed on the seed crystal 60 in the related art, the temperature uniformity of the seed crystal holder 10 can be improved, the number of high-temperature points is reduced, and the temperature of the high-temperature points is low, which can reduce the sublimation of the material of the seed crystal 60 from the back. Moreover, through the above arrangement, compared with the situation in which the structure and / or processing method of the seed crystal 60 are changed in some implementations, the seed crystal holder body 11 made of the second material (such as graphite) is used for grooving and filling, which will not affect the structure and internal stress of the seed crystal 60, the process is simple, the feasibility is high, and it is convenient to prefabricate, which is conducive to large-scale production and popularization and application.
[0066] It should be noted that the relative magnitude relationship between the thermal conductivity of the first material and the thermal conductivity of the second material is not limited here.
[0067] In some examples, such as Figure 2 As shown, the thermal conductivity of the first material is greater than that of the second material. At this time, the thermal conductivity of the first material is better than that of the second material. A plurality of low-temperature regions Q on the growth surface 60a of the seed crystal 60 correspond to the filling portion 12 up and down along the second direction Y. At this time, the first material may be silicon carbide. The second direction Y is the thickness direction of the seed crystal holder body 11.
[0068] In other examples, such as Figure 3 As shown, the thermal conductivity of the first material is smaller than that of the second material. At this time, the thermal conductivity of the second material is better than that of the first material. The plurality of low-temperature regions Q on the growth surface 60a of the seed crystal 60 correspond vertically to a portion of the first surface 11a of the seed crystal holder body 11 along the second direction Y, that is, they do not correspond vertically to the filling portion 12 along the second direction Y. At this time, the first material may be tantalum or tantalum carbide.
[0069] In some embodiments, the thermal conductivity of the first material is smaller than the thermal conductivity of the second material, and the minimum size of the bottom surface 13 a of the groove 13 is in the range of 10 to 100 μm.
[0070] Here, the size of the bottom surface 13a of the groove 13 refers to the size of a line formed from one boundary point of the bottom surface 13a of the groove 13 through the geometric center to another boundary point. The minimum size of the bottom surface 13a of the groove 13 refers to the smallest of the multiple sizes of the bottom surface 13a of the groove 13.
[0071] As mentioned above, if Figure 3 As shown, when the thermal conductivity of the first material is less than that of the second material, the plurality of low-temperature regions Q on the growth surface 60a of the seed crystal 60 do not correspond to the filling portion 12 up and down along the second direction Y, so that the filling portion 12 and a portion of the region between the low-temperature regions Q (for example, Figure 3At the same time, since the filling portion 12 is filled in the groove 13, the size of the groove 13 corresponds to the size of the filling portion 12. In this way, when the minimum size of the bottom surface 13a of the groove 13 is in the range of 10 to 100 μm, the distance between two adjacent low-temperature regions Q is small. In this way, after the crystal nucleates in multiple low-temperature regions Q, the effect of blocking the 0001 direction of the non-preferential growth region by lateral growth is relatively good, which can reduce the TSD density of the growing crystal.
[0072] Preferably, the minimum size of the bottom surface 13a of the groove 13 is in the range of 25 to 80 μm.
[0073] For example, the minimum size of the bottom surface 13 a of the groove 13 may be 10 μm, 25 μm, 30 μm, 50 μm, 70 μm, 80 μm, 85 μm or 100 μm, etc.
[0074] In some embodiments, Figure 2 and Figure 3 As shown, the thermal conductivity of the first material is greater than the thermal conductivity of the second material, and the minimum distance L2 between two adjacent grooves 13 is in the range of 10 to 100 μm.
[0075] Here, the spacing between two adjacent grooves 13 refers to the size of a line formed from a boundary point of the first groove 13 to a boundary point of the second groove 13 on a reference plane. The reference plane is parallel to the first surface 11a. The minimum spacing L2 between two adjacent grooves 13 refers to the minimum of multiple spacings between two adjacent grooves 13.
[0076] As mentioned above, if Figure 2 As shown, when the thermal conductivity of the first material is greater than that of the second material, multiple low-temperature regions Q on the growth surface 60a of the seed crystal 60 correspond to the filling portion 12 up and down along the second direction Y, so that the area between two adjacent low-temperature regions Q corresponds to the area between the filling portions 12. At the same time, since the filling portion 12 is filled in the groove 13, the area between the grooves 13 corresponds to the area between the filling portions 12. In this way, when the minimum spacing L2 between two adjacent grooves 13 has a value range of 10 to 100 μm, the spacing between two adjacent low-temperature regions Q is small. In this way, after the crystal nucleates in multiple low-temperature regions Q, the effect of blocking the 0001 direction of the non-preferential growth region by lateral growth is relatively good, and the TSD density of the growing crystal can be reduced.
[0077] Preferably, the minimum distance L2 between two adjacent grooves 13 is in the range of 25 to 80 μm.
[0078] For example, the minimum distance L2 between two adjacent grooves 13 may be 10 μm, 20 μm, 25 μm, 52 μm, 75 μm, 80 μm, 90 μm or 100 μm.
[0079] In some embodiments, Figure 2 and Figure 3 As shown, the dimension H of the groove 13 in the second direction Y is in the range of 10 to 500 μm, and the second direction is the thickness direction of the seed crystal holder body 11 .
[0080] It can be understood that when the dimension H of the groove 13 in the second direction Y is in the range of 10 to 500 μm, the depth of the groove 13 is relatively large, so that the height of the filling portion 12 filled in the groove 13 is relatively high, and the filling amount of the first material located in the filling portion 12 can be relatively high. In this way, the first material has a greater influence on the temperature field of the surface 10a of the seed crystal holder 10 where the seed crystal 60 is set. When the temperature field of the surface 10a of the seed crystal holder 10 where the seed crystal 60 is set is modulated by multiple filling portions 12, the modulation effect can be better.
[0081] Preferably, a dimension H of the groove 13 in the second direction Y is in the range of 100 to 300 μm.
[0082] For example, a dimension H of the groove 13 in the second direction Y may be 10 μm, 50 μm, 100 μm, 150 μm, 200 μm, 250 μm, 300 μm, 400 μm or 500 μm, etc.
[0083] In some embodiments, Figure 2 and Figure 3 As shown, the groove 13 is a columnar groove or a prism-shaped groove. The dimension D1 of the opening 13b of the groove 13 in the first direction X is greater than or equal to the dimension D2 of the bottom surface 13a of the groove 13 in the first direction X; the first direction X is parallel to the first surface 11a.
[0084] Here, the first direction X may be any direction parallel to the first surface 11 a , as long as the dimension D1 of the opening 13 b of the groove 13 and the dimension D2 of the bottom surface 13 a of the groove 13 are satisfied, and the requirements of the same first direction X are referred to.
[0085] In some examples, such as Figure 2 As shown, the groove 13 is a cylindrical groove. The dimension D1 of the opening 13b of the groove 13 in the first direction X is equal to the dimension D2 of the bottom surface 13a of the groove 13 in the first direction X. At this time, the shape of the opening 13b of the groove 13 is consistent with the shape of the bottom surface 13a of the groove 13. In this case, the shape of the opening 13b of the groove 13 (that is, the shape of the bottom surface 13a of the groove 13) is not limited here.
[0086] Exemplarily, the shape of the opening 13 b of the groove 13 may be circular, square, rectangular, triangular, hexagonal, or the like.
[0087] Exemplarily, when the opening 13b of the groove 13 is circular, the diameter of the circle is in the range of 5 to 500 μm, preferably, the diameter of the circle is in the range of 30 to 50 μm; for example, the diameter of the circle can be 5 μm, 15 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, 100 μm, 200 μm, 300 μm, 400 μm or 500 μm, etc. It should be noted that, when the thermal conductivity of the first material is less than that of the second material, since the diameter of the circle is the minimum size of the bottom surface 13a of the groove 13, its preferred value range is 10 to 100 μm.
[0088] Exemplarily, when the shape of the opening 13b of the groove 13 is a square, the side length of the square is in the range of 10 to 300 μm, for example, the side length of the square may be 10 μm, 50 μm, 100 μm, 150 μm, 200 μm, 250 μm or 300 μm, etc. It should be noted that, when the thermal conductivity of the first material is less than the thermal conductivity of the second material, since the side length of the square is consistent with the minimum size of the bottom surface 13a of the groove 13, at this time, the preferred value range of the side length of the square is 10 to 100 μm.
[0089] For example, when the opening 13b of the groove 13 is in the shape of a rectangle, the length of the longer side of the rectangle is in the range of 100-400 μm, and the length of the shorter side of the rectangle is in the range of 10-300 μm. For example, the length of the longer side of the rectangle can be 100 μm, 150 μm, 200 μm, 250 μm, 300 μm, 350 μm or 400 μm, etc.; the length of the shorter side of the rectangle can be 10 μm, 50 μm, 80 μm, 100 μm, 160 μm, 200 μm, 240 μm or 300 μm, etc. It should be noted that, when the thermal conductivity of the first material is less than the thermal conductivity of the second material, since the length of the shorter side of the rectangle is consistent with the minimum size of the bottom surface 13a of the groove 13, at this time, the preferred length of the shorter side of the rectangle is in the range of 10-100 μm.
[0090] In other examples, such as Figure 3As shown, the groove 13 is a prism-shaped groove. Moreover, the opening 13b of the groove 13 and the bottom surface 13a of the groove 13 are arranged in parallel and coaxially. The dimension D1 of the opening 13b of the groove 13 in the first direction X is greater than the dimension D2 of the bottom surface 13a of the groove 13 in the first direction X, that is, the large end of the groove 13 is located at the opening, and the small end is located at the bottom of the groove. At this time, the shape of the opening 13b of the groove 13 and the shape of the bottom surface 13a of the groove 13 can be the same or different, and there is no limitation here.
[0091] Exemplarily, when the shape of the opening 13b of the groove 13 is the same as the shape of the bottom surface 13a of the groove 13, the groove 13 may be a truncated cone or a polygonal cone, etc.; wherein the polygonal cone may be a triangular cone, a square cone or a hexagonal cone, etc.
[0092] For example, when the groove 13 is a truncated cone, the diameter of the opening 13b of the groove 13 is in the range of 20 to 500 μm, and the diameter of the bottom surface 13a of the groove 13 is in the range of 10 to 200 μm. Preferably, the diameter of the opening 13b of the groove 13 is in the range of 50 to 100 μm, and the diameter of the bottom surface 13a of the groove 13 is in the range of 40 to 60 μm. The diameter of the opening 13b can be 20 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, 210 μm, 300 μm, 430 μm or 500 μm, etc. The diameter of the bottom surface 13a of the groove 13 can be 10 μm, 20 μm, 40 μm, 50 μm, 55 μm, 60 μm, 100 μm, 140 μm, 180 μm or 200 μm, etc. It should be noted that, when the thermal conductivity of the first material is less than the thermal conductivity of the second material, since the diameter of the bottom surface 13a of the groove 13 is the minimum size of the bottom surface 13a of the groove 13, its preferred value range is 10 to 100 μm.
[0093] Exemplarily, when the groove 13 is a polygonal table, the side length of the opening 13b of the groove 13 is in the range of 5 to 100 μm; the side length of the bottom surface 13a of the groove 13 is in the range of 3 to 50 μm; preferably, the side length of the opening 13b of the groove 13 is in the range of 5 to 20 μm; the side length of the bottom surface 13a of the groove 13 is in the range of 3 to 10 μm; for example, the side length of the opening 13b of the groove 13 can be 5 μm, 10 μm, 20 μm, 30 μm, 50 μm, 70 μm, 85 μm or 100 μm, etc.; the side length of the bottom surface 13a of the groove 13 can be 3 μm, 5 μm, 10 μm, 20 μm, 30 μm, 41 μm or 50 μm, etc.
[0094] Exemplarily, when the groove 13 is a prism-shaped groove, the dimension H of the groove 13 in the second direction Y ranges from 100 to 300 μm. For example, the dimension of the groove 13 in the second direction Y may be 100 μm, 150 μm, 200 μm, 260 μm or 300 μm.
[0095] It can be understood that when the groove 13 is a cylindrical groove or a prism-shaped groove, firstly, the process feasibility of forming the groove 13 on the first surface 11a of the seed crystal holder body 11 can be improved; secondly, the shape of the groove 13 can be made relatively regular, and the distribution area of the first material can be made relatively regular. In this way, when the temperature field of the surface 10a of the seed crystal holder 10 on which the seed crystal 60 is set is modulated by multiple filling parts 12, the modulation controllability can be improved.
[0096] In some embodiments, Figure 6 and Figure 8 As shown, a plurality of grooves 13 are evenly distributed along a third direction Z on the seed crystal holder body 11 ; the third direction Z is a direction from the geometric center M of the seed crystal holder body 11 to the boundary N of the seed crystal holder body 11 .
[0097] When a plurality of grooves 13 are evenly distributed along the third direction Z on the seed crystal holder body 11, as a possible implementation method, Figure 6 As shown, the plurality of grooves 13 are divided into a plurality of groove groups 13G, and the groove group 13G includes at least one groove 13. Along the third direction Z, there is a first interval L1 between each two adjacent groove groups 13G. The plurality of first intervals L1 are equal. The third direction Z is the direction from the geometric center M of the seed crystal holder body 11 to the boundary N of the seed crystal holder body 11.
[0098] It can be understood that when multiple grooves 13 are evenly distributed along the third direction Z on the seed crystal holder body 11, the temperature uniformity of the surface 10a of the seed crystal holder 10 on which the seed crystal 60 is set is improved, which can improve the temperature uniformity of the seed crystal holder 10 and reduce the sublimation of the material of the seed crystal 60 from the back.
[0099] In some other embodiments, the plurality of grooves 13 are unevenly distributed on the seed holder body 11 .
[0100] In some embodiments, Figure 7 As shown, multiple grooves 13 are distributed on the seed crystal holder body 11 according to a predetermined rule, and the predetermined rule includes: along the third direction Z, the distribution density of the multiple grooves 13 on the seed crystal holder body 11 gradually decreases; the third direction Z is the direction from the geometric center M of the seed crystal holder body 11 to the boundary N of the seed crystal holder body 11.
[0101] As a possible implementation, Figure 7As shown, the plurality of grooves 13 are divided into a plurality of groove groups 13G, each groove group 13G including at least one groove 13. Along the third direction Z, there is a first interval L1 between each two adjacent groove groups 13G. Along the third direction Z, the plurality of first intervals L1 gradually increase.
[0102] It can be understood that when distributed according to the above predetermined rule, the plurality of grooves 13 are unevenly distributed on the seed crystal holder body 11 , and the plurality of grooves 13 are densely distributed inside and sparsely distributed outside, so that the structural strength of the seed crystal holder 10 is higher.
[0103] In some embodiments, Figure 6 to Figure 8 As shown, the plurality of grooves 13 are divided into a plurality of groove groups 13G, and the groove group 13G includes at least one groove 13. When the groove group 13G includes one groove 13, the groove 13 is located at the geometric center M of the seed crystal holder body 11. When the groove group 13G includes a plurality of grooves 13, the plurality of grooves 13 included in the groove group 13G surround the geometric center M of the seed crystal holder body 11. Along the third direction Z, there is a first interval L1 between each two adjacent groove groups 13G. The plurality of first intervals L1 are equal; or, along the third direction Z, the plurality of first intervals L1 gradually increase; the third direction Z is the direction from the geometric center M of the seed crystal holder body 11 to the boundary N of the seed crystal holder body 11.
[0104] Here, if Figure 6 and Figure 7 As shown, the groove 13 is located at the geometric center M of the seed crystal holder body 11, which means that the geometric center of the groove 13 coincides with the geometric center M of the seed crystal holder body 11. In the case where the groove group 13G includes a plurality of grooves 13, such as Figure 6 to Figure 8 As shown, the multiple grooves 13 included in the groove group 13G surround the geometric center M of the seed crystal holder body 11, and the multiple grooves 13 are arranged around the geometric center M of the seed crystal holder body 11. As a possible implementation method, the geometric center of the arrangement pattern of the multiple grooves 13 included in the groove group 13G coincides with the geometric center M of the seed crystal holder body 11.
[0105] Here, along the third direction Z, the multiple first intervals L1 gradually increase, which means that along the third direction Z, among any two adjacent first intervals L1, the first interval L1 close to the geometric center M of the seed crystal holder body 11 is larger than the first interval L1 far from the geometric center M of the seed crystal holder body 11.
[0106] It can be understood that when the first intervals L1 are equal, the distribution uniformity of the grooves 13 is high, so that the temperature uniformity of the surface 10a of the seed crystal holder 10 where the seed crystal 60 is arranged is improved, the temperature uniformity of the seed crystal holder 10 can be improved, and the sublimation of the material of the seed crystal 60 from the back can be reduced. When the first intervals L1 gradually increase along the third direction Z, the distribution of the grooves 13 is dense inside and sparse outside, so that the structural strength of the seed crystal holder 10 is high.
[0107] In some embodiments, Figure 7 As shown, the maximum L1 in the first interval L1 max , and the smallest L1 in the first interval L1 mi The ratio between n is less than or equal to 3.
[0108] When a plurality of first intervals L1 are equal, the largest one L1 among the first intervals L1 max , and the smallest L1 in the first interval L1 min The ratio between them is equal to 1. When the plurality of first intervals L1 gradually increase along the third direction Z, the largest one L1 among the first intervals L1 max , and the smallest L1 in the first interval L1 min The ratio between is greater than 1; and, if Figure 7 As shown, along the third direction Z, when the plurality of first intervals L1 gradually increase, the largest one L1 among the first intervals L1 max , is the first interval L1 farthest from the geometric center M of the seed crystal holder 10 among the plurality of first intervals L1. The smallest L1 among the first intervals L1 min , is the first interval L1 closest to the geometric center M of the seed crystal holder 10 among the multiple first intervals L1.
[0109] It can be understood that when the crystal growth device 100 provides heat through the induction heating coil 51, the edge temperature of the seed crystal 60 is higher than the center temperature of the seed crystal 60, and accordingly, the edge temperature of the seed crystal holder 10 is higher than the center temperature of the seed crystal holder 10. In this case, when the maximum L1 in the first interval L1 is max , and the smallest L1 in the first interval L1 min When the ratio is greater than 3, the groove group 13G near the boundary of the seed crystal holder 10 is sparsely distributed. In this way, the groove 13 has little effect on the temperature field at the boundary of the seed crystal holder 10, and it is easy for a high temperature point to still exist at the boundary of the seed crystal holder 10. max , and the smallest L1 in the first interval L1 minWhen the ratio is less than or equal to 3, the distribution of the grooves 13 at the boundary of the seed crystal holder 10 can be optimized, thereby improving the modulation effect of the grooves 13 on the temperature field at the boundary of the seed crystal holder 10 .
[0110] For example, the largest L1 in the first interval L1 max , and the smallest L1 in the first interval L1 min The ratio between can be 1.0, 1.5, 2.0, 2.5 or 3.0.
[0111] In some embodiments, Figure 2 and Figure 3 As shown, a surface 12 a of the filling portion 12 away from the bottom surface 13 a of the groove 13 is flush with the first surface 11 a ; and a surface 10 a of the seed crystal holder 10 on which the seed crystal 60 is disposed has a flatness less than or equal to 150 μm.
[0112] In the relevant technology, flatness refers to the deviation of the macroscopic concave-convex height of the substrate from the ideal plane, which can be measured by plane interferometry, table measurement, liquid plane method or beam plane method.
[0113] Here, the flatness of the surface 10 a of the seed holder 10 on which the seed crystal 60 is disposed refers to the flatness of the surface formed by the first surface 11 a of the seed holder body 11 and the surface 12 a of the filling portion 12 away from the bottom surface 13 a of the groove 13 .
[0114] It can be understood that when the flatness of the surface 10a of the seed crystal holder 10 on which the seed crystal 60 is arranged is less than or equal to 150μm, the flatness of the surface 10a of the seed crystal holder 10 on which the seed crystal 60 is arranged is relatively high. In this way, firstly, the connection performance between the seed crystal holder 10 and the seed crystal 60 can be improved; secondly, the seed crystal holder 10 can be made to fit the seed crystal 60 more closely, and when the temperature field of the surface 10a of the seed crystal holder 10 on which the seed crystal 60 is arranged is modulated by multiple filling parts 12, the modulation effect can be better.
[0115] For example, the flatness of the surface 10 a of the seed crystal holder 10 on which the seed crystal 60 is disposed may be 10 μm, 30 μm, 50 μm, 70 μm, 100 μm, 120 μm, 150 μm, etc.
[0116] In some embodiments, the first material includes any one or more of tantalum, tantalum carbide and silicon carbide; and / or the second material is graphite.
[0117] It can be understood that tantalum, tantalum carbide and silicon carbide are all high-temperature resistant materials that are different from the second material (for example, graphite), and can maintain the shape and state of the filling portion 12 in a high-temperature environment (for example, an environment with a temperature higher than 2000°C) when a silicon carbide single crystal is formed by a physical vapor transport method. In this way, the filling portion 12 can play the function of modulating the temperature field of the surface 10a of the seed crystal holder 10 on which the seed crystal 60 is set when a silicon carbide single crystal is formed by a physical vapor transport method.
[0118] In some embodiments, when forming the filling portion 12, the first material is in a powder state, such as silicon carbide powder. In this case, in addition to the first material, auxiliary materials can be added to the material forming the filling portion 12 to increase the coating uniformity of the material forming the filling portion 12, so that the first material is more evenly distributed.
[0119] In some embodiments, the material forming the filling portion 12 further includes modified epoxy resin.
[0120] It can be understood that when the first material is in a powder state when forming the filling portion 12, when the material forming the filling portion 12 also includes a modified epoxy resin, the powder particles of the first material can be evenly distributed in the modified epoxy resin. In this way, the coating uniformity of the material forming the filling portion 12 can be increased, making the first material more evenly distributed.
[0121] For example, the modified epoxy resin may include epoxy resin, phenolic resin, furfuryl alcohol resin, ethylenediamine, thickener, and surfactant; wherein the thickener may be carboxymethyl cellulose. Here, there is no limitation on the type of surfactant and the mass ratio of epoxy resin, phenolic resin, furfuryl alcohol resin, ethylenediamine, thickener, and surfactant, as long as the requirements for achieving the above functions are met.
[0122] In some embodiments, in the material forming the filling portion, the mass ratio of the first material to the modified epoxy resin is in the range of 3:1 to 5:1.
[0123] It can be understood that when the mass ratio of the first material and the modified epoxy resin in the material forming the filling portion is in the range of 3:1 to 5:1, the mass ratio of the first material and the modified epoxy resin is set appropriately. In this way, the coating uniformity of the material forming the filling portion 12 can be increased, and the solid content of the first material in the formed filling portion 12 can be at a higher level.
[0124] For example, in the material forming the filling portion, the mass ratio of the first material to the modified epoxy resin may be 3:1, 3.5:1, 4:1, 4.2:1, 4.8:1, or 5:1.
[0125] Some embodiments of the present disclosure also provide a method for preparing a seed crystal tray, such as Fig. 9 As shown, the preparation method includes S1 to S3:
[0126] S1: providing an initial seed pad body 14 .
[0127] Exemplarily, the material of the initial seed pad body 14 is graphite.
[0128] Exemplarily, the diameter of the initial seed crystal holder body 14 is slightly larger than the diameter of the seed crystal 60 .
[0129] S2: Figure 2 , Figure 3 and Fig.10 As shown, a plurality of grooves 13 are formed on the first initial surface of the initial seed crystal holder body 14 ; the plurality of grooves 13 are arranged at intervals; the first initial surface of the initial seed crystal holder body 14 forms the first surface 11 a of the seed crystal holder body 11 , and the first surface 11 a is used to place the seed crystal 60 .
[0130] S3: Fill multiple grooves 13 to form multiple filling parts 12. The filling parts 12 are made of a first material, and the initial seed crystal holder body 14 is made of a second material. The thermal conductivity of the first material is different from that of the second material.
[0131] Exemplarily, when the material of the filling portion 12 further includes modified epoxy resin, filling a plurality of grooves 13 and correspondingly forming a plurality of filling portions 12 include S3.1 to S3.3:
[0132] S3.1: Fill the groove 13 with powder of the first material (such as silicon carbide) mixed with modified epoxy resin (hereinafter referred to as filler), and flatten it after removing excess powder.
[0133] Exemplarily, the flattening operation may be first flattening with a blade and then flattening with a pressurizing device, the pressurizing pressure being 30 to 50 kg, for example, 30 kg, 35 kg, 40 kg, 45 kg or 50 kg, etc.; the pressurizing time may be 3 hours.
[0134] S3.2: Place the initial seed crystal holder body 14 with the filling material into an oven at a preset temperature and keep the temperature for 4 hours.
[0135] Exemplarily, the preset temperature is 300°C.
[0136] Exemplarily, S3.2 may be replaced by S3.2', and S3.2' specifically comprises: annealing at 500-800° C. for 2-3 h.
[0137] In some examples, the modified epoxy resin may undergo a carbonization reaction under a preset temperature, and the products of the carbonization reaction may remain in the filling portion 12 .
[0138] S3.3: Take out the initial seed crystal holder body 14, and detect the flatness of the surface of the initial seed crystal holder body 14 exposed to the first material. If the flatness is less than the flatness threshold, the initial seed crystal holder body 14 forms the seed crystal holder body 11, and the material filled in the groove 13 forms the filling part 12, thereby completing the preparation of the seed crystal holder 10. If the flatness is greater than or equal to the flatness threshold, use a grinding wheel with a preset mesh number to process the surface of the initial seed crystal holder body 14 exposed to the first material, remove a certain thickness, until the flatness meets the requirements, thereby completing the preparation of the seed crystal holder 10.
[0139] Exemplarily, the planarity threshold is 150 μm.
[0140] Exemplarily, the preset mesh grinding wheel is an 800-mesh grinding wheel.
[0141] Exemplarily, when a grinding wheel with a preset mesh is used to process the surface of the initial seed holder body 14 where the first material is exposed, the removed thickness may be 5-10 μm, for example, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm or 10 μm.
[0142] In some embodiments, the grooves 13 are cylindrical grooves; S2 forming a plurality of grooves 13 on the first initial surface of the initial seed crystal holder body 14 includes: using a laser process to make grooves in a set area of the first initial surface to form a plurality of grooves 13 .
[0143] Exemplarily, the laser process may be a green light picosecond laser process or an ultraviolet nanosecond laser process.
[0144] Exemplarily, the cross-sectional pattern of the formed groove 13 parallel to the first surface 11a is a set pattern, which can be a circle, a square, a rectangle, a triangle, a hexagon or the like.
[0145] In some embodiments, after using a laser process to groove a set area of the first initial surface to form a plurality of grooves 13, before S3, it also includes: transferring the initial seed crystal holder body 14 with the grooves 13 to a cleaning basket for cleaning, and drying the initial seed crystal holder body 14 after cleaning for use.
[0146] Exemplarily, the above cleaning process can be completed in three steps.
[0147] Exemplarily, the cleaning agent used in the first cleaning step is SC1 solution, and its formula may be: 27% ammonia water, 30% hydrogen peroxide and water mixed in a volume ratio of 1:1:5; the first cleaning time may be 5 minutes.
[0148] Exemplarily, the cleaning agent used in the second step of cleaning is SC2 solution, and its formula may be: 37% by mass hydrochloric acid solution, 30% by mass hydrogen peroxide and water mixed in a volume ratio of 1:1:6; the cleaning time of the second step may be 5 minutes.
[0149] Exemplarily, the third cleaning step can be completed using a QDR tank, and the time for the third cleaning step can be 3 minutes.
[0150] In some embodiments, Fig.10 As shown, the groove 13 is a prism-shaped groove; S2 forms a plurality of grooves 13 on the first initial surface of the initial seed crystal holder body 14, including: using an etching process to groove a set area of the first initial surface 14a to form a plurality of grooves 13.
[0151] Exemplarily, the etching process may be a dry etching process or a wet etching process. The dry etching process may be, for example, an inductively coupled plasma (ICP)-reactive ion etching (RIE) dry etching process.
[0152] For example, when the etching process is an ICP-RIE dry etching process, Fig.10 As shown, S2 may include S2.1 to S2.6:
[0153] S2.1: Coating a photoresist material layer W on the first initial surface 14 a of the initial seed pad body 14 .
[0154] Exemplarily, the material of the photoresist material layer W may be photoresist, or an inorganic non-metallic material; for example, an acrylate material.
[0155] Exemplarily, when the photoresist material layer W is made of acrylate material, coating a layer of photoresist material on the first initial surface 14a of the initial seed holder body 14 further includes: drying naturally for 10 minutes at room temperature to preliminarily dry the acrylate material.
[0156] S2.2: forming a plurality of pits 16 on the photoresist material layer W by using the imprinting mold 15 .
[0157] Exemplarily, the imprinting mold 15 is a micro-nano imprinting mold.
[0158] Exemplarily, the position of the pit 16 corresponds to the position of the groove 13 .
[0159] S2.3: Curing the photoresist material layer W.
[0160] For example, when the photoresist material layer W is made of an acrylate material, the method for curing the photoresist material layer W may be: irradiating the photoresist material under ultraviolet light for 2 to 3 minutes to cause the acrylate material to undergo a curing reaction and generate an acrylate crosslinking agent.
[0161] S2.4: Using RIE equipment, remove the residual photoresist material at the bottom of the pit 16 .
[0162] For example, using RIE equipment, the residual photoresist material at the bottom of the pit 16 can be removed by chemical reaction.
[0163] S2.5: Using ICP equipment, etching the initial seed crystal holder body 14 with the photoresist material to form a plurality of grooves 13 .
[0164] It can be understood that, since the etching speeds of the photoresist material and the initial seed tray body 14 are different, grooves 13 of different shapes can be formed by selecting different etching ratios.
[0165] Exemplarily, in S2.5, the etching gas may be chlorine (Cl2), hydrogen chloride (HCl) or oxygen (O2), etc.
[0166] Illustratively, in S2.5, the flow rate of the etching gas may be 40 to 80 sccm, for example, 40 sccm, 50 sccm, 60 sccm, 70 sccm or 80 sccm.
[0167] For example, in S2.5, the temperature in the dry etching chamber may be 40-120° C., for example, 40° C., 60° C., 80° C., 102° C. or 120° C. The above chamber temperature is measured using a color-changing temperature band.
[0168] Illustratively, in S2.5, the pressure in the dry etching chamber may be 200-800 Pa, for example, 200 Pa, 300 Pa, 400 Pa, 500 Pa, 620 Pa, 700 Pa or 800 Pa.
[0169] S2.6: removing the remaining photoresist material on the first initial surface 14a to form the first surface 11a.
[0170] In some embodiments, after a plurality of grooves 13 are formed by grooving a set area of the first initial surface 14a of the initial seed crystal holder body 14 using an etching process, before S3, the process further includes: transferring the initial seed crystal holder body 14 with the grooves 13 to a cleaning basket for cleaning, and drying the initial seed crystal holder body 14 after cleaning for use.
[0171] Exemplarily, the above cleaning process can be completed in four steps.
[0172] For example, the cleaning agent used in the first step of cleaning is an SPM solution, and its formula can be: a sulfuric acid solution with a mass fraction of 98.3%, a hydrogen peroxide solution with a mass fraction of 35%, and water mixed in a volume ratio of 3:1:1 to 5:1:1; the first step of cleaning time can be 5 minutes. Among them, in the SPM solution, the volume ratio of the sulfuric acid solution with a mass fraction of 98.3%, the hydrogen peroxide solution with a mass fraction of 35%, and water can be 3:1:1.
[0173] Exemplarily, the cleaning agent used in the second step of cleaning is SC1 solution, and its formula may be: 27% ammonia water by mass, 30% hydrogen peroxide by mass and water mixed in a volume ratio of 1:1:5; the cleaning time of the second step may be 5 minutes.
[0174] Exemplarily, the cleaning agent used in the third step of cleaning is SC2 solution, and its formula may be: 37% by mass hydrochloric acid solution, 30% by mass hydrogen peroxide and water mixed in a volume ratio of 1:1:6; the cleaning time of the third step may be 5 minutes.
[0175] Exemplarily, the fourth cleaning step can be completed using a QDR tank, and the fourth cleaning step can take 3 minutes.
[0176] It can be understood that the beneficial effects that can be achieved by the method for preparing the seed crystal tray provided in the above embodiment of the present disclosure can refer to the beneficial effects of the seed crystal tray described above, and will not be repeated here.
[0177] Some embodiments of the present disclosure also provide a crystal growth device 100. Fig.11 As shown, the crystal growth device includes a seed crystal holder 10 ; a crucible body 20 and a crucible cover 30 covering the crucible body 20 ; the seed crystal holder 10 is connected to the inner surface of the crucible cover 30 .
[0178] Here, the seed crystal holder 10 is connected to the inner surface of the crucible cover 30, which means that the seed crystal holder 10 is connected to the inner surface of the crucible cover 30, and there is no relative movement between the seed crystal holder 10 and the inner surface of the crucible cover 30. The inner surface of the crucible cover 30 refers to the surface of the crucible cover 30 relative to the inner cavity of the crucible body 20. It should be noted that the connection method between the seed crystal holder 10 and the inner surface of the crucible cover 30 is not limited here.
[0179] Exemplarily, the seed crystal holder 10 may be connected to the inner surface of the crucible cover 30 by first integrating the seed crystal holder 10 into the inner surface of the crucible cover 30 and then reinforcing it by an annealing process; wherein the temperature of the annealing process may be set to 500°C.
[0180] It can be understood that the crucible body 20 and the crucible cover 30 can constitute a crucible 40 for containing raw materials (such as silicon carbide powder K).
[0181] Exemplarily, the material of the crucible body 20 may be graphite.
[0182] By way of example, the material of the seed pad 10 may be graphite.
[0183] In addition, the crystal growth device 100 may further include a heating component 50 , and the heating component 50 is used to heat the raw material (such as silicon carbide powder K) in the crucible 40 to sublime the raw material at a high temperature.
[0184] In some examples, the heating assembly 50 includes an induction heating coil 51 wound around the outer peripheral wall of the crucible 40 and coaxially arranged with the crucible 40. In this way, the raw material can be heated by medium frequency electromagnetic induction heating. Specifically, after the induction heating coil 51 is energized, eddy currents are generated on the surface of the crucible 40 due to the skin effect, thereby generating Joule heat and providing heat to the crystal growth device 100.
[0185] It can be understood that the beneficial effects that can be achieved by the crystal growth device provided by the above-mentioned embodiments of the present disclosure can refer to the beneficial effects of the seed crystal holder mentioned above, which will not be repeated here.
[0186] Some embodiments of the present disclosure also provide a crystal growth method, wherein the crystal growth is achieved based on the crystal growth apparatus provided by some embodiments of the present disclosure.
[0187] It can be understood that the beneficial effects that can be achieved by the crystal growth method provided by the above embodiments of the present disclosure can refer to the beneficial effects of the seed crystal holder mentioned above, which will not be repeated here.
[0188] In some embodiments, in the crystal growth method, such as Fig.12 As shown, the crystal growth process includes a first growth stage R1 and a second growth stage R2.
[0189] In the first growth stage R1, nucleation growth occurs to form a crystal nucleus T; the growth temperature of the first growth stage R1 is 2150° C., and the insulation time is 8 to 12 hours.
[0190] Illustratively, the insulation time of the first growth stage can be 8.0 h, 8.5 h, 9.0 h, 9.4 h, 10.0 h, 10.5 h, 11.0 h, 11.5 h or 12.0 h.
[0191] In some examples, the first growth stage R1 is performed in an argon environment, and the pressure of the growth environment is 2000-4000 Pa. For example, the pressure of the growth environment can be 2000 Pa, 2500 Pa, 3000 Pa, 3600 Pa or 4000 Pa.
[0192] For example, the above growth environment can be achieved by: before the first growth stage R1, the single crystal furnace is vacuumized to 10 -5 pa; and then slowly fill with argon until the pressure reaches the set pressure (for example, 2000-4000Pa); and then heat the crystal growth device 100 by the heating component 50 until the temperature in the chamber of the crucible 40 reaches 2150°C.
[0193] It can be understood that when the growth temperature of the first growth stage R1 is 2150° C., the growth temperature is relatively low, which can prevent the polymorphic growth of the crystal, thereby improving the crystal purity of the grown crystal.
[0194] In the second growth stage R2, as Fig.13 As shown, the crystal growth continues to form a crystal growth body E; the growth temperature of the second growth stage R2 is 2280-2380° C., and the pressure of the growth environment is 400-800 Pa.
[0195] Illustratively, the growth temperature of the second growth stage R2 may be 2280° C., 2320° C., 2340° C., 2360° C., or 2380° C., etc.
[0196] Illustratively, the pressure of the growth environment in the second growth stage R2 may be 400 Pa, 510 Pa, 600 Pa, 700 Pa or 800 Pa, etc.
[0197] It can be understood that in the second growth stage R2, the initial growth surface has been formed and is relatively stable. Moreover, in the growth process of the crystal (for example, silicon carbide crystal), the growth rate is proportional to the growth temperature within a certain range of conditions, and the growth rate is inversely proportional to the pressure of the growth environment. Therefore, when the growth temperature of the second growth stage R2 is 2280-2380°C and the pressure of the growth environment is 400-800Pa, the growth temperature is higher and the pressure of the growth environment is lower, which can make the growth rate of the crystal faster and help reduce the dislocation density.
[0198] In order to objectively evaluate the technical effects of the embodiments of the present disclosure, the technical solutions provided by the present disclosure will be described in detail and exemplarily through the following experimental examples and comparative examples.
[0199] The following examples and comparative examples use different methods to prepare seed crystal holders, use a crystal growth device including the seed crystal holders prepared in the examples and comparative examples to grow crystals, and measure and compare the dislocation defect density of the grown crystals.
[0200] In the following comparative examples and embodiments, the test conditions for the screw dislocation (TSD) density, the ductile dislocation (TED) density and the basis vector dislocation (BPD) density are the same.
[0201] Example 1
[0202] Step 1: Prepare the seed crystal tray.
[0203] The method for preparing a seed crystal tray comprises steps V1 to V3:
[0204] V1: Take a piece of initial seed crystal support body 14 made of graphite, and use laser technology to open cylindrical grooves 13 on the first initial surface 14a of the initial seed crystal support body. The diameter of the groove 13 is 40 μm and the depth is 300 μm. Moreover, the minimum spacing between two adjacent grooves 13 is 60 μm. The arrangement of the grooves 13 on the initial seed crystal support body 14 is as follows: Figure 6 shown.
[0205] V2: The initial seed crystal holder body 14 with the groove 13 is transferred to the cleaning basket for cleaning, and the initial seed crystal holder body 14 is dried after cleaning for standby use. The cleaning process can be completed in three steps: The cleaning agent used in the first step of cleaning is SC1 solution, and its formula is: 27% ammonia water, 30% hydrogen peroxide and water are mixed in a volume ratio of 1:1:5; the cleaning time can be 5 minutes. The cleaning agent used in the second step of cleaning is SC2 solution, and its formula is: 37% hydrochloric acid solution, 30% hydrogen peroxide and water are mixed in a volume ratio of 1:1:6; the cleaning time can be 5 minutes. The third step of cleaning is completed with a QDR tank, and the cleaning time can be 3 minutes.
[0206] V3: Fill the groove 13 with silicon carbide powder mixed with modified epoxy resin (hereinafter referred to as filler), remove the excess filler, flatten it, and then put it in an oven at 300°C for 4 hours. After taking it out, process the surface of the initial seed crystal holder body 14 exposed to the first material until the flatness reaches less than 150μm.
[0207] Step 2: Connect the seed crystal holder, seed crystal, and crucible cover.
[0208] The connection methods of the seed crystal holder, seed crystal, and crucible cover include V4~V5:
[0209] V4: Use adhesive to bond the seed crystal prepared in advance to the seed crystal holder prepared in the first step, so that the non-crystalline growth surface of the seed crystal, i.e., the Si surface, is bonded to the surface of the seed crystal holder provided with the filling portion.
[0210] V5: The seed crystal holder with the seed crystal bonded to it is integrated with the crucible cover, and then reinforced by annealing at 500℃.
[0211] Step 3: Preparation of crystal growth equipment.
[0212] First, put the crucible cover with the seed crystal holder bonded to the crucible body and seal the crucible. Install the crucible in the single crystal furnace. Then, evacuate the single crystal furnace until the vacuum degree reaches 10 -5 Then slowly fill the argon gas until the pressure of the single crystal furnace reaches 2000-4000 Pa. Then heat the crucible until the temperature inside the crucible rises to 2150℃.
[0213] Step 4: Crystal growth.
[0214] The first growth stage: under the condition that the temperature in the crucible cavity is 2150℃, keep warm for 12h, carry out nucleation growth, form crystal nucleus T, and obtain the semi-finished product of crystal growth, such as Figure 2 shown.
[0215] Second growth stage: reduce the pressure of the single crystal furnace to 800pa, heat the crucible until the temperature in the crucible cavity rises to 2280℃, and continue the crystal growth for 168h to form a crystal growth body E. Then cool down to obtain a crystal growth body, such as Fig.13 shown.
[0216] Step 5: Characterization of dislocation density of the crystal growth body.
[0217] The crystal growth body was taken out, and after multi-wire cutting, grinding and thinning, and CMP polishing into a 6-foot substrate sheet, it was immersed in a potassium hydroxide (KOH) melt at a temperature of 540°C and subjected to strong corrosion for 10 minutes. The dislocation density was then characterized using a metallographic microscope; among them, the screw dislocation (TSD) density was 86e.a / cm 2 , ductile dislocation (TED) density is 2859e.a / cm 2 , basis vector dislocation (BPD) density is 1251e.a / cm 2 .
[0218] Example 2
[0219] Step 1: Prepare the seed crystal tray.
[0220] The method for preparing a seed crystal holder comprises steps V1' to V3':
[0221] V1: Take an initial seed crystal holder body 14 made of a piece of graphite, and use an etching process to open a square trapezoidal groove 13 on the first initial surface 14a of the initial seed crystal holder body. Referring to the above steps S2.1 to S2.6, an ICP-RIE dry etching process is used; wherein, the material of the photoresist material layer W is an acrylate material, and after coating the photoresist material layer W, it is naturally dried at room temperature for 10 minutes; the imprinting mold 15 is a micro-nano imprinting mold; and the method of curing the photoresist material layer W is irradiating under ultraviolet light for 2 to 3 minutes. The side length of the bottom surface 13a of the groove 13 is 5μm, the side length of the opening 13b of the groove 13 is 15μm, and the depth is 300μm. The arrangement of the groove 13 on the initial seed crystal holder body 14 is as follows Figure 8 shown.
[0222] V2: The initial seed crystal holder body 14 with the groove 13 is transferred to the cleaning basket for cleaning, and the initial seed crystal holder body 14 is dried after cleaning for standby use. The cleaning process can be completed in four steps: The cleaning agent used in the first step of cleaning is SPM solution, and its formula is: sulfuric acid solution with a mass fraction of 98.3%, hydrogen peroxide with a mass fraction of 35% and water mixed in a volume ratio of 3:1:1; the cleaning time can be 5 minutes. The cleaning agent used in the second step of cleaning is SC1 solution, and its formula is: ammonia water with a mass fraction of 27%, hydrogen peroxide with a mass fraction of 30% and water mixed in a volume ratio of 1:1:5; the cleaning time can be 5 minutes. The cleaning agent used in the third step of cleaning is SC2 solution, and its formula is: hydrochloric acid solution with a mass fraction of 37%, hydrogen peroxide with a mass fraction of 30% and water mixed in a volume ratio of 1:1:6; the cleaning time can be 5 minutes. The fourth step of cleaning is completed with a QDR tank, and the cleaning time can be 3 minutes.
[0223] V3: Fill the groove 13 with silicon carbide powder mixed with modified epoxy resin (hereinafter referred to as filler), remove the excess filler, flatten it, and then put it in an oven at 300°C for 4 hours. After taking it out, process the surface of the initial seed crystal holder body 14 exposed to the first material until the flatness reaches less than 150μm.
[0224] Referring to the methods of the second to fifth steps above, the connection of the seed crystal holder, the seed crystal, and the crucible cover, the preparation of the crystal growth device, the crystal growth, and the dislocation density characterization of the crystal growth body are completed. In the fourth step, the semi-finished crystal growth product obtained in the first growth stage, such as Figure 3 In the fifth step, the measured dislocation density result is that the screw dislocation (TSD) density is 79e.a / cm 2 , ductile dislocation (TED) density is 2231e.a / cm 2 , basis vector dislocation (BPD) density is 1315e.a / cm 2In the fifth step, metallographic microscope photos were also obtained, such as Fig.14 shown.
[0225] Comparative Example
[0226] Step 1: Prepare the seed crystal tray.
[0227] Take a piece of initial seed crystal holder body 14 made of graphite and use it directly as a seed crystal holder.
[0228] Referring to the methods of the second to fifth steps above, the connection of the seed crystal holder, seed crystal, and crucible cover, the preparation of the crystal growth device, crystal growth, and the dislocation density characterization of the crystal growth body are completed. In the fifth step, the dislocation density result measured is that the screw dislocation (TSD) density is 425e.a / cm 2 , ductile dislocation (TED) density is 4288e.a / cm 2 , basis vector dislocation (BPD) density is 3218e.a / cm 2 .
[0229] In order to more clearly describe the comparison results of the embodiment and the comparative example, the following Table 1 is used to more clearly show the dislocation density results obtained by measuring the embodiment and the comparative example.
[0230] Table 1
[0231]
[0232]
[0233] Compared with the comparative example, please refer to Table 1. The TSD density, BPD density and TED density of Example 1 and Example 2 are relatively low. This is because the seed crystal holders of Examples 1 and 2 include a filling part, and the thermal conductivity of the material of the filling part (the first material) is different from the thermal conductivity of the material of the seed crystal holder body (the second material), so that the temperature field of the surface of the seed crystal holder on which the seed crystal is arranged can be modulated, and then the temperature field of the seed crystal in contact with the seed crystal holder can be modulated; in this way, after heat conduction, the regional temperature distribution (for example, the radial temperature distribution) of the growth surface of the silicon carbide crystal (for example, the C surface of the seed crystal) can be changed, so that a plurality of low-temperature regions are formed on the growth surface of the seed crystal (that is, the growth surface of the silicon carbide crystal), so that the crystal preferentially nucleates in the plurality of low-temperature regions at the same time, and after nucleation, the crystal growth in the 0001 direction of the non-preferential growth region (for example, the region located between the two low-temperature regions) is blocked by lateral growth perpendicular to the 0001 plane (that is, the plane parallel to and opposite to the C plane), so that the crystal growth mode is changed, and the TSD density of the growing crystal is reduced. When the TSD density decreases, the conversion of TSD to BPD and TSD to TED is relatively small, which causes the BPD density and TED density to decrease.
[0234] It can be seen from the above embodiments and comparative examples that the present disclosure can reduce the dislocation density in the silicon carbide single crystal material by opening a plurality of grooves on the first surface of the seed crystal holder body and arranging a filling part in the groove so that the thermal conductivity of the material of the filling part (first material) is different from the thermal conductivity of the material of the seed crystal holder body (second material).
[0235] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A seed crystal holder, characterized in that: include: A seed crystal holder body, wherein a first surface of the seed crystal holder body is provided with a plurality of grooves, the plurality of grooves are arranged at intervals, and the first surface is used for arranging the seed crystal; The plurality of grooves are distributed on the seed crystal holder body according to a predetermined rule, and the predetermined rule includes: along a third direction, the distribution density of the plurality of grooves on the seed crystal holder body gradually decreases; the third direction is a direction from the geometric center of the seed crystal holder body to the boundary of the seed crystal holder body; A plurality of filling parts, correspondingly disposed in the plurality of grooves; The material of the filling part includes a first material, the material of the seed crystal holder body includes a second material, and the thermal conductivity of the first material is different from the thermal conductivity of the second material.
2. The seed crystal holder according to claim 1, characterized in that: The thermal conductivity of the first material is smaller than the thermal conductivity of the second material, and the minimum size of the bottom surface of the groove is in the range of 10 to 100 μm.
3. The seed crystal holder according to claim 1, characterized in that: The thermal conductivity of the first material is greater than the thermal conductivity of the second material, and the minimum distance between two adjacent grooves is in the range of 10 to 100 μm.
4. The seed crystal holder according to claim 1, characterized in that: The size of the groove in the second direction ranges from 10 to 500 μm, and the second direction is the thickness direction of the seed crystal holder body.
5. The seed crystal holder according to any one of claims 1 to 4, characterized in that: The plurality of grooves are divided into a plurality of groove groups, wherein the groove group includes at least one groove; In the case where the groove set includes one groove, the groove is located at the geometric center of the seed holder body; In the case where the groove group includes a plurality of grooves, the plurality of grooves included in the groove group surround the geometric center of the seed tray body; Along the third direction, there is a first interval between every two adjacent groove groups; Along the third direction, the plurality of first intervals gradually increase; The third direction is a direction from the geometric center of the seed crystal holder body to the boundary of the seed crystal holder body.
6. The seed crystal holder according to claim 5, characterized in that: A ratio of the largest value in the first interval to the smallest value in the first interval is less than or equal to 3.
7. The seed crystal holder according to any one of claims 1 to 4, characterized in that: A surface of the filling portion away from the bottom surface of the groove is flush with the first surface; The flatness of the surface of the seed crystal holder on which the seed crystal is disposed is less than or equal to 150 μm.
8. The seed crystal holder according to any one of claims 1 to 4, characterized in that: The first material includes any one or more combinations of tantalum, tantalum carbide and silicon carbide; and / or the second material is graphite.
9. The seed crystal holder according to any one of claims 1 to 4, characterized in that: The material forming the filling portion further includes modified epoxy resin.
10. The seed crystal holder according to claim 9, characterized in that: In the material forming the filling portion, the mass ratio of the first material to the modified epoxy resin is in the range of 3:1 to 5:
1.
11. A method for preparing a seed crystal tray, characterized in that: include: Providing an initial seed crystal holder body; forming a plurality of grooves on a first initial surface of the initial seed crystal holder body; The plurality of grooves are arranged at intervals; The first initial surface of the initial seed crystal holder body forms the first surface of the seed crystal holder body, and the first surface is used for setting the seed crystal; The plurality of grooves are distributed on the seed crystal holder body according to a predetermined rule, and the predetermined rule includes: along a third direction, the distribution density of the plurality of grooves on the seed crystal holder body gradually decreases; the third direction is a direction from the geometric center of the seed crystal holder body to the boundary of the seed crystal holder body; Filling the plurality of grooves to correspondingly form a plurality of filling portions; The material of the filling portion includes a first material, the material of the initial seed crystal holder body includes a second material, and the thermal conductivity of the first material is different from the thermal conductivity of the second material.
12. The method for preparing a seed crystal tray according to claim 11, characterized in that: The groove is a cylindrical groove; The forming of a plurality of grooves on the first initial surface of the initial seed crystal holder body includes: using a laser process to groove a set area of the first initial surface to form a plurality of grooves.
13. The method for preparing a seed crystal tray according to claim 11, characterized in that: The groove is a prism-shaped groove; Forming a plurality of grooves on the first initial surface of the initial seed crystal holder body includes: using an etching process to groove a set area of the first initial surface to form a plurality of grooves.
14. A crystal growth device, characterized in that: comprising the seed crystal holder as claimed in any one of claims 1 to 10; The invention also comprises a crucible body and a crucible cover arranged on the crucible body, wherein the seed crystal holder is connected to the inner surface of the crucible cover.
15. A crystal growth method, characterized in that: The crystal growth method is implemented based on the crystal growth device as claimed in claim 14.
16. The crystal growth method according to claim 15, characterized in that: In the crystal growth method, the crystal growth process includes: In the first growth stage, nucleation growth is performed to form a crystal nucleus; the growth temperature of the first growth stage is 2150° C., and the insulation time is 8 to 12 hours; In the second growth stage, the crystal growth is continued to form a crystal growth body; the growth temperature of the second growth stage is 2280-2380° C., and the pressure of the growth environment is 400-800 Pa.