A method for resource recovery of lithium-containing glass waste

By combining water-soluble fluoride salts and inorganic acids with cryolite precipitation, the problems of lithium loss and equipment corrosion in lithium-containing glass waste have been solved, achieving efficient and green recovery of valuable elements such as lithium and aluminum, and improving recovery rate and product purity.

CN117604271BActive Publication Date: 2026-11-17CENT SOUTH UNIV +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202311536002.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-17
Publication Date
2026-11-17
Estimated Expiration
2043-11-17

AI Technical Summary

Technical Problem

Existing technologies for processing lithium-containing glass waste suffer from low leaching rates, significant lithium loss, and severe equipment corrosion during the inorganic acid leaching process, posing environmental pollution risks and making it difficult to achieve efficient and green recovery of valuable elements such as lithium and aluminum.

Method used

Acid-deficient leaching was performed using water-soluble fluoride salts and inorganic acids, with the pH value controlled within the range of 0-4. Subsequently, the pH of the leaching solution was adjusted to 5-8 with alkali, and aluminum and fluorine were separated by cryolite precipitation to obtain lithium compound products.

Benefits of technology

It achieves efficient recovery of valuable elements such as lithium and aluminum, avoids HF gas volatilization and equipment corrosion, improves the overall lithium recovery rate and product purity, reduces processing costs, and is environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117604271B_ABST
    Figure CN117604271B_ABST
Patent Text Reader

Abstract

This invention relates to a method for the resource-based treatment of lithium-containing glass waste, comprising the following steps: pretreating the lithium-containing glass waste to be treated to obtain powder; mixing the powder with water-soluble fluoride salt and water to obtain a slurry; adding an inorganic acid to the slurry, and after the reaction is complete, separating the solid and liquid to obtain a leachate and a leachate residue; wherein, during the reaction, the pH value of the slurry is maintained at 0-4 by adding an inorganic acid; adjusting the pH value of the leachate to 5-8 with alkali and / or alkaline solution, and then separating the solid and liquid to obtain a purified liquid and cryolite product; subjecting the purified liquid to lithium precipitation treatment, and then separating the solid and liquid to obtain lithium compound products. This invention achieves comprehensive recycling of lithium-containing glass waste, not only extracting high-value lithium, but also recovering valuable components Al and Si from the glass, effectively improving the comprehensive treatment efficiency of waste glass, and producing byproducts such as silica powder and cryolite, which have wide applications, high sales value, and good market prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for the resource-based treatment of lithium-containing glass waste, and more particularly to a method for extracting metallic lithium from lithium-containing glass waste through under-acid leaching, which belongs to the field of solid waste resource-based treatment. Background Technology

[0002] Li₂O-Al₂O₃-SiO₂ (LAS) glass-ceramics, also known as glass ceramics, possess a series of excellent properties such as thermal shock resistance, high temperature resistance, corrosion resistance, and high strength. In particular, LAS glass is crystallizable, precipitating β-quartz solid solutions and β-spodumene solid solutions. This allows the linear expansion coefficient of LAS glass-ceramics to be adjusted over a wide range, achieving zero expansion or even negative expansion. Lithium aluminum silicate (LAS) glass-ceramics are manufactured by controlling the crystallization process. During its manufacturing, to lower the melting temperature and increase the melt viscosity, spodumene concentrate or Li₂CO₃ with a low iron content (less than 0.1%) is added to the glass melt.

[0003] Defective products and leftover scraps generated during the deep processing of LAS glass ceramics, such as cutting, forming, and polishing, are collectively referred to as glass waste. Simultaneously, glass-ceramic panels from waste 3C electronic products, waste photovoltaic panels, and scrapped automobiles also generate a large amount of glass waste after sorting and dismantling. This type of glass waste contains 0.1-5.5 wt.% Li2O, with main components being oxides such as Al2O3, Na2O, SiO2, B2O, K2O, and MgO. Compared to traditional lithium-containing mineral resources such as spodumene, lepidolite, petalite, and phosphogypsum, it has unique characteristics, and existing technologies for processing lithium-containing mineral resources cannot be simply applied to the resource recovery of lithium-containing glass waste. If lithium can be efficiently recovered from this type of lithium-containing glass waste and its resource utilization achieved, it can further expand the sources of lithium resources in my country and help alleviate the current lithium resource shortage.

[0004] At the same time, glass waste is also rich in elements such as Na, Al, and Si. If it is not used, it will also result in the waste of valuable resources.

[0005] The applicant discovered through phase analysis that the main components of lithium-containing glass waste are amorphous glassy substances, and no obvious diffraction peaks of lithium-containing phases were found. It is speculated that lithium-containing microcrystalline phases are interspersed between glass phases, with only a small amount "exposed" on the surface, which undoubtedly increases the difficulty of lithium extraction from lithium-containing glass waste.

[0006] Chinese invention patent application CN 115595445 A discloses a method for recovering lithium from lithium-containing glass powder. The method involves crushing lithium-containing glass powder waste to below 200 mesh; adding the powder to an acid washing tank with 30 wt.% hydrochloric acid solution at a solid-liquid volume ratio of 3:1, mixing and stirring, allowing it to stand, and then filtering to obtain a leachate; adjusting the pH of the leachate to purify it by precipitating aluminum hydroxide; and heating the purified solution to precipitate lithium, yielding lithium carbonate. This invention patent uses acid leaching to achieve the leaching of valuable lithium from glass powder. However, silicate-based glassy substances are difficult to react with acid, and a large amount of lithium-containing microcrystalline phase remains interspersed within the glass phase, which may lead to low leaching efficiency and a low leaching rate.

[0007] Chinese invention patent application CN 116445735 A discloses a method for extracting lithium metal from waste glass. The method involves crushing and grinding lithium-containing glass; then calcining it in a high-temperature furnace at 500-750℃ for 1-1.5 hours; followed by leaching with a mixed acid solution composed of 15-20% hydrofluoric acid and 70-72% perchloric acid at 65-85℃, resulting in an acidic leachate with a pH of 0.8-1.2; finally, causticization is performed to gradually extract products such as aluminum hydroxide and lithium carbonate. This invention patent uses calcination to pretreat the glass powder, followed by acid leaching with a mixed acid system of hydrofluoric acid and perchloric acid, achieving the leaching of 99.4% of the valuable lithium metal from the glass powder. However, the acid leaching temperature is high, and the mixed acid system severely corrodes the equipment, requiring high corrosion resistance from the reactor. At the same time, the hydrofluoric acid in the mixed acid system is highly volatile at the acid leaching temperature, seriously endangering the health of on-site operators. The large amount of fluoride ions introduced into the leachate will also corrode downstream process equipment, and improper handling can easily cause uncontrollable environmental pollution.

[0008] The aforementioned published invention patents all use inorganic acids as leaching agents to leach lithium from lithium-containing glass waste, achieving good leaching rates. However, in addition to SiO2, the main components of this type of lithium-containing glass also include 40%-60% Al2O3. The applicant's analysis shows that the Al2O3 in the lithium-containing glass is amorphous, non-crystalline active aluminum oxide, which will completely enter the liquid phase during acidic leaching. The aforementioned patents all use pH adjustment to remove the large amount of aluminum present in the liquid phase through aluminum hydroxide precipitation. This inevitably leads to a significant loss of lithium (intercalated in the aluminum hydroxide colloid), affecting the lithium recovery rate in the entire process and worsening the economics of the process. Moreover, the resulting aluminum hydroxide, due to the presence of other impurities, has low value for reuse or sale.

[0009] Therefore, there is an urgent need to develop a treatment process based on wet processing and using inorganic acid as a leaching agent. This process would achieve both quick and efficient green leaching of metallic lithium from glass waste and efficient separation of aluminum and lithium from the acidic leaching solution. This would reduce the loss of metallic lithium during the separation process, improve the overall recovery rate of metallic lithium, and realize the harmless and value-added recycling of waste glass. Summary of the Invention

[0010] In view of the shortcomings of the prior art, the purpose of this invention is to provide a resource-based treatment method for lithium-containing glass waste, so as to realize the resource recovery of valuable elements such as Li, Al, and Si in lithium-containing glass waste.

[0011] To solve the above-mentioned technical problems, the technical solution of the present invention is as follows: A method for the resource recovery of lithium-containing glass waste includes the following steps: S1. Pre-treat the lithium-containing glass waste to be processed to obtain powder; S2. Mix the powder with water-soluble fluoride salt and water evenly to obtain a slurry; S3. Add inorganic acid to the slurry. After the reaction is complete, separate the solid and liquid to obtain leachate and leach residue. During the reaction, inorganic acid is added to maintain the pH value of the slurry at 0-4, preferably 0.2-2.5, more preferably 0.5-2.0, and even more preferably 0.8-1.5; S4. Adjust the pH of the leachate to 5-8 (preferably 5.5-7.5, more preferably 5.8-7.2, and even more preferably 6.0-7.0) with alkali and / or alkali solution. After the reaction is complete, separate the solid and liquid to obtain purified liquid and cryolite product. S5. After the purified liquid is subjected to lithium precipitation treatment, solid-liquid separation is performed to obtain lithium compound products.

[0012] Furthermore, in S2, the water-soluble fluoride salt includes one or more of sodium fluoride, potassium fluoride, and ammonium fluoride; Preferably, the molar ratio of fluorine in the water-soluble fluoride salt to aluminum in the powder is 1.0-6.0:1, more preferably 2-5.5:1, and even more preferably 2.5-5:1.

[0013] Furthermore, in S2, the solid-liquid ratio of the powder to water is 1g:3-12ml, even more so 1g:4-10ml, preferably 1g:5-10ml, and even more preferably 1g:6-7ml.

[0014] Furthermore, in S3, the reaction time is 1-3 hours, even more so 1.2-2.5 hours, and preferably 1.5-2 hours; Preferably, the reaction temperature is 20-60℃, more preferably 25-55℃, and even more preferably 30-45℃; Preferably, the mixture is continuously stirred at a rate of 100-500 rpm during the reaction. More preferably, the stirring rate is 150-400 rpm, and more preferably 200-350 rpm.

[0015] Furthermore, in S3, the inorganic acid includes one or more of hydrochloric acid, sulfuric acid, and nitric acid; Preferably, the concentration of the inorganic acid is 30-98 wt%, more preferably 35-95 wt%, even more preferably 40-90 wt%, preferably 45-85 wt%, even more preferably 50-75 wt%, preferably 55-72 wt%, and even more preferably 60-70 wt%. Preferably, inorganic acid is added to the slurry in multiple batches, with an interval of 3-10 minutes between adjacent batches. Each batch adds 1.5-4 ml of inorganic acid per 100 ml of slurry (i.e., 1.5-4 ml of inorganic acid is added to each 100 ml of slurry per batch). During the leaching process, by adding inorganic acid in batches and in precise quantities, the added acid reacts rapidly with and is consumed by the "naked" oxides, thereby achieving effective control of the slurry pH.

[0016] Alternatively, an inorganic acid may be added dropwise to the slurry so that the pH of the slurry is maintained between 0 and 4 during the reaction.

[0017] Preferably, the inorganic acid is added in 3-10 batches with an interval of 3-10 minutes, more preferably 4-8 times with an interval of 4-8 minutes, and more preferably 5-6 times with an interval of 5-6 minutes. Preferably, after the inorganic acid is added, the reaction continues for 0.5-3 hours, more preferably for 1-2 hours.

[0018] Further, the leaching residue is washed to obtain a washing solution and silica powder; Preferably, the leaching residue is subjected to three-stage countercurrent washing to obtain washing liquid and silica powder; more preferably, the mass ratio of water used for the three-stage countercurrent washing to the mass of the leaching residue is 0.5-2.0:1, and even more preferably 1-1.5:1. Preferably, the washing liquid is returned to S2 for use in preparing the slurry.

[0019] Further, in S4, during the reaction process, when the pH value of the reaction system drops to 4-6 (this is considered the reaction endpoint), solid-liquid separation occurs; preferably, when the pH value of the reaction system drops to 4.5-5.8, solid-liquid separation occurs; more preferably, when the pH value of the reaction system drops to 4.8-5.5, solid-liquid separation occurs; more preferably, when the pH value of the reaction system drops to 5.0-5.5, solid-liquid separation occurs. Preferably, the base is sodium hydroxide and / or potassium hydroxide; Preferably, the alkaline solution is added dropwise to the leachate; more preferably, the dropping rate of the alkaline solution is 2-10 ml / min; even more preferably, the concentration of the alkaline solution is 10-60 wt%. Preferably, the reaction temperature is 60-90℃, more preferably 65-85℃; Preferably, the mixture is continuously stirred at a rate of 100-400 rpm during the reaction.

[0020] Further, in step S5, the purified liquid is causticized, concentrated to obtain a concentrated liquid, sodium carbonate is added, and after the reaction is complete, solid-liquid separation is performed to obtain lithium carbonate product (lithium compound product) and lithium precipitation mother liquor; preferably, the pH value of the purified liquid after causticization is 9.0-12.0; preferably, the Li2O content in the concentrated liquid is 30-50 g / L; preferably, the reaction is stirred at 90-95℃ for 2.0-3.0 h.

[0021] Further, in S1, the pretreatment includes one or more of crushing, screening, and grinding. Optionally, during pretreatment, other waste materials containing one or more of lithium, aluminum, and silicon may be added.

[0022] Further, in S1, the particle size of the powder is ≤0.3mm, even further, less than 0.20mm, preferably less than 0.15mm, and most preferably ≤0.1mm.

[0023] Optionally, in S1, the water source is one or more of the following: purified water, evaporated condensate, lithium precipitation mother liquor, and washing liquid.

[0024] Furthermore, in S1, the lithium-containing glass waste includes one or more of the following: waste 3C electronic product glass covers, photovoltaic glass panels, displays, and defective products and tailings from the deep processing of lithium-containing glass.

[0025] Preferably, the lithium-containing glass waste comprises 0.1-5.5 wt.% Li2O, 39.5-62.1 wt.% SiO2, and 37.8-64.0 wt.% Al2O3.

[0026] More preferably, the lithium-containing glass waste comprises Li2O 0.1-5.5 wt.%, SiO2 39.5-62.1 wt.%, Al2O3 37.8-64.0 wt.%, MgO 0-3.0 wt.%, N2O 0-2.0 wt.%, CaO 0.1-0.50 wt.%, K2O 0-0.5 wt.%, and B2O 2.5-4.0 wt.%.

[0027] Optionally, the cryolite product contains one or more of sodium cryolite, potassium cryolite, and sodium-potassium cryolite.

[0028] In this invention, powder is mixed with water and water-soluble fluoride salts, slurried, and then mixed with inorganic acid. The pH value is controlled for under-acid leaching. On the one hand, the acidic environment allows fluorine to corrode the chemically inert dense glassy phase SiO2 in the powder, destroying the dense surface layer. This allows dilute sulfuric acid to react with oxides such as Li2O and Al2O3, achieving effective leaching of valuable elements such as lithium and aluminum under under-acid and low-temperature conditions. On the other hand, by effectively controlling the pH of the slurry during the leaching process, the reaction process can prevent HF from reacting further with SiO2, thus avoiding corrosion of the reaction equipment and jeopardizing the safety of on-site personnel.

[0029] Subsequently, after solid-liquid separation, Li-rich materials can be obtained. + Na + and / or K + Al 3+ SO4 2- and F - The process involves leaching the leachate and leaching residue, primarily composed of unreacted SiO2 powder. The pH of the leachate is then gradually adjusted using alkali or an alkaline solution to remove Al and F impurities as cryolite precipitates, thus purifying the leachate. The particle size and morphology of cryolite are far superior to the aluminum hydroxide colloids produced during traditional acid-based slag removal processes, preventing adsorption loss of lithium metal in the liquid phase and effectively ensuring a high overall lithium metal recovery rate.

[0030] The process of this invention adopts an acid process, which has a short process flow, low energy consumption, and can realize the full utilization of elements such as lithium, silicon, sodium, and aluminum in lithium-containing waste glass. It is green, efficient, closed-loop treatment, does not generate secondary pollution, has low treatment cost, and has extremely high economic value.

[0031] Compared with the prior art, the beneficial effects of the present invention are as follows: (1) The entire process of the present invention realizes the comprehensive recycling of lithium-containing glass waste. It not only extracts high-value lithium, but also recovers valuable components Al and Si in the glass, effectively improving the comprehensive treatment efficiency of waste glass. The purity of the prepared lithium carbonate product can meet the requirements of the national standard GB / T 11075-2013 for the Li2CO3-0 grade. The by-products, silica powder and cryolite products, have a wide range of applications, high sales value, and good market prospects.

[0032] (2) The resource recovery method of the present invention, while ensuring the lithium metal leaching rate, effectively avoids further reaction between HF and SiO2 and the volatilization of HF gas by controlling the pH value of the system during the leaching process, and achieves the separation of SiO2 from Li2O and Al2O3 in a green and environmentally friendly manner.

[0033] (3) The resource recovery method of the present invention recovers and removes impurities Al and F in the leachate by cryolite, avoiding the enrichment of F element in the process flow, which would cause serious harm to equipment, personnel and environment. At the same time, it also effectively avoids the loss of a large amount of metallic lithium during the causticizing dealuminization process. Attached Figure Description

[0034] Figure 1 This is a flowchart of a method for the resource utilization of lithium-containing glass waste according to the present invention.

[0035] Figure 2 This is the XRD pattern of the lithium-containing waste glass used in Example 1.

[0036] Figure 3 This is the XRD pattern of cryolite obtained in Example 1. Detailed Implementation

[0037] The present invention will now be described in detail with reference to the accompanying drawings and embodiments. It should be noted that, unless otherwise specified, the embodiments and features described herein can be combined with each other. Unless otherwise specified, the relevant percentages refer to mass percentages.

[0038] Example 1 In this embodiment, the method for resource utilization of lithium-containing glass waste includes the following steps: S1. Take 100g of lithium-containing glass waste from a panel factory (Li₂O 4.93%, SiO₂ 57.56%, Al₂O₃ 31.47%, CaO 0.49%, MgO 2.65%, K₂O 0.36%, Na₂O 1.78%). See the phase analysis chart for details. Figure 2 ), crush, and obtain 100g of glass powder with a particle size ≤0.1mm; S2. Mix 100g of glass powder with 500mL of water (liquid-solid ratio of 5ml:1g), place in a glass beaker, stir, and slurry; add 77.75g of sodium fluoride to the glass slurry (the molar ratio of fluorine in the added sodium fluoride to aluminum in the glass waste is 3.0), stir and mix well to obtain 560mL of glass slurry; S3. Place 560 mL of glass slurry into the reactor; seal the reactor, turn on the stirrer, and heat to 30°C. Add 50% dilute sulfuric acid in 5 batches, with each batch containing 15 mL, at 5-minute intervals, maintaining the pH of the slurry in the reactor within the range of 0.8-1.2; during the addition of dilute sulfuric acid, turn on the cooling water switch inside the outer jacket of the reactor to maintain the slurry in the reactor at 30°C; after the last batch of acid is added, react for 1.0 h, and separate the solid and liquid to obtain leachate and leach residue. The leaching residue was subjected to a three-stage countercurrent washing process to obtain washing liquid and 55.3g of silica powder. The ratio of the mass of the water used for the three-stage countercurrent washing to the mass of the leaching residue is 3:1. S4. Place 470 mL of the leachate in a glass beaker, turn on the stirrer, heat to 90 °C, and add 30% sodium hydroxide solution at a dropping rate of 5 mL / min to gradually raise the pH of the system to 6.5. After the pH of the reaction system drops to 5.0-5.5, the solid and liquid are separated to obtain the purified solution and 127.4 g of cryolite. S5. After removing Al and F, the purified liquid is causticized with sodium hydroxide to a pH of 9.0, then evaporated and concentrated to a Li2O content of 40 g / L. Sodium carbonate is added to precipitate lithium, and the mixture is stirred at 90 °C for 2.5 h. After the reaction is complete, the solid and liquid are separated to obtain 10.73 g of lithium carbonate product and lithium precipitation mother liquor.

[0039] Figure 2 The XRD pattern of lithium-containing waste glass in S1 shows that, apart from the "non-z-crystalline bulge" unique to SiO2 in the 15-30° range, there are no diffraction peaks of other phases, indicating that the small amount of lithium-rich phase in the waste glass is almost completely covered by the glass phase. Figure 3 The XRD pattern of cryolite obtained from the acidic leachate in S3 after causticization and solid-liquid separation; Inductively coupled plasma atomic emission spectrometry (ICP-AES) was used to perform full elemental analysis on the washed lithium carbonate product. Three sets of samples were weighed in parallel, with 1.0 g of each sample. The samples were digested and diluted to volume with 1.40 mol / L hydrochloric acid before analysis. The average purity of the product reached 98.70%, and the total recovery rate of lithium was calculated to be 93.0%.

[0040] Comparative Example 1 Repeat Example 1, except that in S2, the amount of sodium fluoride added is 0.

[0041] The purity of the obtained lithium carbonate product was 86.10%. The overall lithium recovery rate was 23.7%.

[0042] Comparative Example 2 Repeat Example 1, except that in S2, the molar ratio of fluorine in the added sodium fluoride to aluminum in the glass waste is 0.5, and the mixture is stirred until homogeneous.

[0043] The purity of the obtained lithium carbonate product was 85.50%. The overall lithium recovery rate was 45.3%.

[0044] Example 2 Repeat Example 1, except that in S2, the molar ratio of fluorine in the added sodium fluoride to aluminum in the glass waste is 1.5, and the mixture is stirred until homogeneous. The purity of the obtained lithium carbonate product was 98.04%. The overall lithium recovery rate was 72.4%.

[0045] Example 3 Repeat Example 1, except that in S2, the molar ratio of fluorine in the added sodium fluoride to aluminum in the glass waste is 1.0, and the mixture is stirred and mixed. The purity of the obtained lithium carbonate product was 98.15%. The overall lithium recovery rate was 59.3%.

[0046] Example 4 Repeat Example 1, except that in S2, the molar ratio of fluorine in the added sodium fluoride to aluminum in the glass waste is 3.1, and the mixture is stirred until homogeneous. The purity of the obtained lithium carbonate product was 99.05%. The overall lithium recovery rate was 94.7%.

[0047] Example 5 Repeat Example 1, except that in S2, the molar ratio of fluorine in the added sodium fluoride to aluminum in the glass waste is 3.8, and the mixture is stirred and mixed. The purity of the obtained lithium carbonate product was 81.05%. The overall lithium recovery rate was 94.7%.

[0048] The comparison shows that the ratio of the molar amount of fluorine in the added sodium fluoride to the molar amount of aluminum in the lithium-containing glass waste is related to the purity of the lithium carbonate product and the overall recovery rate of lithium metal. This may be because when the sodium fluoride dosage is low, the aluminum in the leachate is not completely combined with fluorine, and some still precipitates as aluminum hydroxide colloid, causing adsorption loss of lithium metal in the liquid phase. When the sodium fluoride dosage is gradually increased, the aluminum in the leachate is completely converted into cryolite and removed, reducing adsorption loss of lithium and significantly improving the recovery rate. When the sodium fluoride dosage is excessive, a large amount of free fluorine still exists in the purified liquid, which further accumulates with evaporation and concentration, eventually entering the lithium carbonate product and affecting the purity of lithium carbonate.

[0049] Example 6 Example 4 was repeated, except that in S3, the concentration of sulfuric acid added was 98%, and the pH of the slurry in the leaching vessel was maintained in the range of 0.5-1.0 during the leaching process; The purity of the obtained lithium carbonate product was 80.04%. The overall lithium recovery rate was 49.2%.

[0050] Example 7 Example 4 was repeated, except that in S3, the concentration of sulfuric acid added was 75%, and the pH of the slurry in the leaching vessel was maintained in the range of 0.6-1.1 during the leaching process; The purity of the obtained lithium carbonate product was 85.13%. The overall lithium recovery rate was 67.0%.

[0051] Example 8 Example 4 was repeated, except that in S3, the concentration of sulfuric acid added was 60%, and the pH of the slurry in the leaching vessel was maintained in the range of 0.7-1.1 during the leaching process; The purity of the obtained lithium carbonate product was 85.30%. The overall lithium recovery rate was 83.5%.

[0052] Example 9 Example 4 was repeated, except that in S3, the concentration of sulfuric acid added was 55%, and the pH of the slurry in the leaching vessel was maintained in the range of 0.8-1.2 during the leaching process; The purity of the obtained lithium carbonate product was 85.30%. The overall lithium recovery rate was 90.7%.

[0053] Example 10 Example 4 was repeated, except that in S3, the concentration of sulfuric acid added was 45%, and the pH of the slurry in the leaching vessel was maintained in the range of 1.0-1.5 during the leaching process; The purity of the obtained lithium carbonate product was 93.10%. The overall lithium recovery rate was 88.10%.

[0054] Example 10 Example 4 was repeated, except that in S3, the concentration of sulfuric acid added was 35%, and the pH of the slurry in the leaching vessel was maintained in the range of 2.0-2.5 during the leaching process; The purity of the obtained lithium carbonate product was 93.10%. The overall lithium recovery rate was 36.2%.

[0055] The comparison shows that the concentration of sulfuric acid, the acidic leaching agent used in the acidic leaching process, has a significant impact on the recovery rate of lithium metal and the purity of lithium carbonate. This may be because when the sulfuric acid concentration is low, the metal oxides in the glass waste cannot react completely due to mass transfer limitations, resulting in a low lithium metal leaching rate. Conversely, when the sulfuric acid concentration is high, the diffusion rate of the acid solution limits the pH in some areas, leading to excessively low free F in those areas. - With H + The combination of these substances produces HF gas, which not only causes the loss of F and reduces the F / Al molar ratio, but also intensifies the reaction with SiO2, generating soluble fluorosilicates that eventually enter the product, reducing the purity of lithium carbonate products. It also affects the formation of cryolite, which may cause aluminum to precipitate in the form of aluminum hydroxide, reducing the recovery rate of Li.

[0056] As can be seen from the results of the above embodiments, the method provided by the present invention can realize the comprehensive utilization of lithium-containing waste glass and effectively recover valuable elements such as lithium, silicon, and aluminum.

[0057] The above embodiments should be understood as being used only to illustrate the present invention more clearly, and not to limit the scope of the present invention. After reading the present invention, any modifications of the present invention in various equivalent forms by those skilled in the art fall within the scope defined by the appended claims.

Claims

1. A method for the resource-based treatment of lithium-containing glass waste, characterized in that, Includes the following steps: S1. Pre-treat the lithium-containing glass waste to be processed to obtain powder; S2. Mix the powder with water-soluble fluoride salt and water evenly to obtain a slurry; The ratio of the molar amount of fluorine in the water-soluble fluoride salt to the molar amount of aluminum in the powder is 1.0-6.0:1; the solid-liquid ratio of the powder to water is 1g:3-12ml. S3. Add inorganic acid to the slurry. After the reaction is complete, separate the solid and liquid to obtain leachate and leach residue. During the reaction, inorganic acid is added to maintain the pH value of the slurry at 0-4; the concentration of the inorganic acid is 30-98wt%; the inorganic acid is added to the slurry in multiple batches, with an interval of 3-10 minutes between adjacent batches, and 1.5-4 ml / 100 ml of inorganic acid is added to each batch of slurry. S4. Adjust the pH of the leachate to 5-8 with alkali and / or alkali solution. After the reaction is complete, separate the solid and liquid to obtain the purified liquid and cryolite product. S5. After the purified liquid is subjected to lithium precipitation treatment, solid-liquid separation is performed to obtain lithium compound products.

2. The resource recovery method according to claim 1, characterized in that, In S2, the water-soluble fluoride salt includes one or more of sodium fluoride, potassium fluoride, and ammonium fluoride.

3. The resource recovery method according to claim 1, characterized in that, In S2, the molar ratio of fluorine in the water-soluble fluoride salt to aluminum in the powder is 2-5.5:

1.

4. The resource recovery method according to claim 1, characterized in that, In S2, the molar ratio of fluorine in the water-soluble fluoride salt to aluminum in the powder is 2.5-5:

1.

5. The resource recovery method according to claim 1, characterized in that, In S2, the solid-liquid ratio of powder to water is 1g:5-10ml.

6. The resource recovery method according to claim 1, characterized in that, In S2, the solid-liquid ratio of powder to water is 1g:6-8ml.

7. The resource recovery method according to claim 1, characterized in that, In S3, the reaction time is 1-3 hours.

8. The resource recovery method according to claim 1, characterized in that, In S3, the reaction time is 1.5-2.5 hours.

9. The resource recovery method according to claim 1, characterized in that, In S3, the reaction temperature is 20-60℃.

10. The resource recovery method according to claim 1, characterized in that, In S3, the reaction temperature is 25-55℃.

11. The resource recovery method according to claim 1, characterized in that, In S3, the mixture is continuously stirred at a rate of 100-500 rpm during the reaction.

12. The resource recovery method according to claim 1, characterized in that, In S3, the inorganic acid includes one or more of hydrochloric acid, sulfuric acid, and nitric acid.

13. The resource recovery method according to claim 1, characterized in that, In S3, the concentration of the inorganic acid is 35-95 wt%.

14. The resource recovery method according to claim 1, characterized in that, In S3, the concentration of the inorganic acid is 40-90 wt%.

15. The resource recovery method according to claim 1, characterized in that, In S3, after the inorganic acid has been added, the reaction continues for 0.5-3 hours.

16. The resource recovery method according to claim 1, characterized in that, In S3, after the inorganic acid has been added, the reaction continues for 1-2 hours.

17. The resource recovery method according to claim 1, characterized in that, The leaching residue is washed to obtain a washing solution and silica powder.

18. The resource recovery method according to claim 17, characterized in that, The leaching residue was subjected to three-stage countercurrent washing to obtain washing liquid and silica powder.

19. The resource recovery method according to claim 18, characterized in that, The ratio of the mass of water used in the three-stage countercurrent washing to the mass of the leaching residue is 0.5-2.0:

1.

20. The resource recovery method according to claim 17, characterized in that, The washing liquid is returned to S2 for use in preparing the slurry.

21. The resource recovery method according to claim 1, characterized in that, In S4, during the reaction process, when the pH value of the reaction system drops to 5-6, solid-liquid separation occurs.

22. The resource recovery method according to claim 21, characterized in that, When the pH of the reaction system drops to 5.0-5.5, solid-liquid separation occurs.

23. The resource recovery method according to claim 1, characterized in that, In S4, the base is sodium hydroxide and / or potassium hydroxide.

24. The resource recovery method according to claim 1, characterized in that, In step S4, the alkaline solution is added dropwise to the leachate.

25. The resource recovery method according to claim 24, characterized in that, The alkaline solution is added at a rate of 2-10 ml / min.

26. The resource recovery method according to claim 24, characterized in that, The concentration of the alkaline solution is 10-60 wt%.

27. The resource recovery method according to claim 1, characterized in that, In S4, the reaction time is 0.5-1.5 h.

28. The resource recovery method according to claim 1, characterized in that, In S4, the reaction temperature is 60-90℃.

29. The resource recovery method according to claim 1, characterized in that, In S4, the mixture is continuously stirred at a rate of 100-400 rpm during the reaction.

30. The resource recovery method according to any one of claims 1-29, characterized in that, In S5, the purified liquid is causticized and concentrated to obtain a concentrated liquid. Sodium carbonate is then added, and after the reaction is complete, solid-liquid separation is performed to obtain lithium carbonate product and lithium precipitation mother liquor.

31. The resource recovery method according to claim 30, characterized in that, The pH value of the purified solution after causticization is 9.0-12.

0.

32. The resource recovery method according to claim 30, characterized in that, The concentration of Li2O in the concentrate is 30-50 g / L.

33. The resource recovery method according to claim 30, characterized in that, Stir the reaction at 90-95℃ for 2.0-3.0 hours.

34. The resource recovery method according to any one of claims 1-29, characterized in that, In S1, the particle size of the powder is ≤0.3mm.

35. The resource recovery method according to any one of claims 1-29, characterized in that, In S1, the particle size of the powder is ≤0.1mm.

36. The resource recovery method according to any one of claims 1-29, characterized in that, In S1, the lithium-containing glass waste includes one or more of the following: waste 3C electronic product glass covers, photovoltaic glass panels, displays, and defective products and tailings from the deep processing of lithium-containing glass.

37. The resource recovery method according to any one of claims 1-29, characterized in that, In S1, the lithium-containing glass waste includes 0.1-5.5 wt.% Li2O, 39.5-62.1 wt.% SiO2, and 37.8-64.0 wt.% Al2O3.

Citation Information

Patent Citations

  • Method for recovering lithium in lithium-containing glass powder

    CN115595445A

  • Method for extracting metal lithium from waste glass

    CN116445735A

  • Improved method for extracting lithium through lepidolite fluorination circulation

    CN106676286A