Pre-foamed materials, their preparation methods and applications

By designing modified polymers and combining crystalline thermoplastic resins with unsaturated monomers, a pre-foamed material with low three-dimensional structural regularity was prepared. This solved the problems of delamination and high water absorption in syndiotactic polystyrene during supercritical foaming, and achieved the dielectric performance and lightweight requirements of high-frequency PCB boards.

CN117624482BActive Publication Date: 2026-11-17HUAWEI TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202210956656.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-10
Publication Date
2026-11-17
Estimated Expiration
2042-08-10

AI Technical Summary

Technical Problem

Existing syndiotactic polystyrene materials are prone to delamination during supercritical foaming, with mostly open-cell cells and high water absorption, making it difficult to meet the dielectric properties and lightweight requirements of high-frequency PCBs.

Method used

By using modified polymers, a pre-foamed material with low three-dimensional structural regularity is prepared by combining crystalline thermoplastic resins with unsaturated monomers. The modified polymers have a wide melting range, high melt strength, are not prone to delamination during foaming, and most of the cells are closed cells with low water absorption.

Benefits of technology

It achieves foamed molding material with low dielectric constant, low dielectric loss and low water absorption, suitable for dielectric layer material of high frequency and high speed PCB board, and has good mechanical strength and heat resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117624482B_ABST
    Figure CN117624482B_ABST
Patent Text Reader

Abstract

This application provides a pre-foamed material and its preparation method, a foamed molded body and its foaming device, a modified polymer, and their related applications. The pre-foamed material includes a modified polymer having a first structural unit derived from an unsaturated monomer, and the ends of the polymer's molecular chains are capped with crystalline thermoplastic resin. The modified polymer in this pre-foamed material has a novel structure, low stereoregularity, wide melting range, and long relaxation time, making it suitable for producing foamed molded bodies using supercritical foaming. Furthermore, the foamed molded body is less prone to delamination, has a high closed-cell rate, low water absorption, and good mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of pre-foamed materials technology, specifically to a pre-foamed material, its preparation method, and its application. Background Technology

[0002] Printed circuit boards (PCBs) are widely used in base station antenna systems and devices such as mobile phones and computers. As communication technology develops towards high frequency and high speed, higher requirements are placed on PCBs. PCB dielectric layer materials with low dielectric constant, low dielectric loss, and lightweight are one of the main development directions of the PCB market.

[0003] Syndiotactic polystyrene (sPS) is considered a potential dielectric layer material for high-frequency PCBs due to its high melting point, low density, low water absorption, and excellent high-frequency dielectric properties. However, sPS is a crystalline material with a narrow melting range, making it difficult to obtain a lightweight dielectric layer through supercritical foaming. Directly supercritical foaming of sPS foam is prone to delamination, and the cells are mostly open-cell with high water absorption, failing to meet the requirements of PCBs. Therefore, it is necessary to provide a foam with low water absorption and good dielectric properties. Summary of the Invention

[0004] In view of this, embodiments of this application provide a foamed molded body with low dielectric constant and dielectric loss and low water absorption, as well as its preparation raw materials and applications.

[0005] Specifically, in a first aspect of this application, a pre-foamed material is provided, the pre-foamed material comprising a modified polymer having a first structural unit derived from an unsaturated monomer, and the ends of the molecular chains of the modified polymer being capped with a crystalline thermoplastic resin.

[0006] The modified polymer in the aforementioned pre-foamed material is a novel polymer derived from the structural units of unsaturated monomers and crystalline thermoplastic resins. This modified polymer has a low degree of regularity in its three-dimensional structure, resulting in a wider melting range. Consequently, the foaming temperature does not need to be controlled within a particularly narrow window when using this pre-foamed material for foaming. The distribution of this modified polymer in the surface and inner layers of the pre-foamed material is not significantly different, thus the foamed molded body obtained using this pre-foamed material is less prone to delamination. Furthermore, compared to pure crystalline thermoplastic resins, the presence of this modified polymer increases the melt strength of the pre-foamed material, ensuring that most of the cells in the resulting foamed molded body are closed-cell, resulting in a low water absorption rate.

[0007] In this embodiment, the crystalline thermoplastic resin includes one or more of syndiotactic polystyrene, polytetrafluoroethylene, polyvinylidene fluoride, perfluoroalkoxy vinyl ether polymers, polyphenylene sulfide, polyether ether ketone, and liquid crystal polymers. These crystalline thermoplastic resins typically have good heat resistance and low dielectric properties, making them more suitable as foaming materials for PCB manufacturing.

[0008] In this embodiment, the unsaturated monomer includes one or more of styrene, maleic anhydride, pentaerythritol triacrylate, methacrylate, glycidyl methacrylate, and ethyl acrylate. Structural units derived from these monomers help improve the melt strength of the modified polymer, thereby effectively alleviating the problems of delamination and open-cell structures in the foamed pre-foamed material, while having minimal impact on the dielectric properties of the modified polymer.

[0009] In this embodiment of the application, the modified polymer has the structural formula shown in formula (Ⅰ):

[0010]

[0011] In formula (Ⅰ), M1 represents the first structural unit derived from an unsaturated monomer, m represents the degree of polymerization of M1, and P1 is independently selected from crystalline thermoplastic resins.

[0012] In this embodiment, the pre-foamed material is obtained by reacting the following raw materials in parts by weight: 100 parts of crystalline thermoplastic resin matrix, 0.1-5 parts of unsaturated monomer, and 0.1-5 parts of initiator. Using smaller amounts of initiator and unsaturated monomer helps ensure a higher yield of the modified polymer, while minimizing the amount of polymerized byproducts—unsaturated monomers.

[0013] In this embodiment, the initiator includes one or more of dicumyl peroxide, di(tert-butylperoxyisopropyl)benzene, 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, 2-(tert-butylperoxyisopropyl)benzene, butanone peroxide, benzoyl peroxide, and dodecyl peroxide. The initiator can cause free radicals to be generated on the molecular chain of the crystalline thermoplastic resin as reaction sites, initiating the polymerization reaction of unsaturated monomers, thereby obtaining a modified polymer having the above-mentioned structure.

[0014] In this embodiment, the pre-foamed material further contains an antioxidant. The antioxidant is present in an amount of 0.09 wt% to 1 wt% of the modified polymer. The addition of an appropriate amount of antioxidant can improve the stability of the pre-foamed material during manufacturing and use.

[0015] In this embodiment, the pre-foamed material, measured by differential scanning calorimetry at a heating rate of 10°C for 1 minute, has a melting range of over 15°C and a melting point of over 270°C. This helps reduce the difficulty of precisely controlling the foaming temperature during the foaming process, ensuring good heat resistance of the resulting foamed molded body.

[0016] The second aspect of this application provides a foamed molded article, which is obtained by foaming the pre-foamed material described in the first aspect of this application.

[0017] In this embodiment, most of the cells in the foamed molded body are closed-cell. Closed-cell cells help ensure that the foamed molded body has excellent water resistance.

[0018] In this embodiment, the water absorption rate of the foamed molded body after being placed in water for 24 hours at a temperature of 23°C and a relative humidity of 50% is less than 1%. A lower water absorption rate is beneficial for extending the service life of the foamed molded body.

[0019] In this embodiment of the application, the average cell size of the foamed molded body is in the range of 5-100 μm.

[0020] In this embodiment of the application, the density of the foamed molded body is 1g / cm³. 3 The following applies. Low-density foamed moldings help ensure the lightweight of devices using them.

[0021] In this embodiment, the dielectric constant of the foamed material measured using the resonant cavity method under electromagnetic waves at a frequency of 10 GHz is below 2.0, and the dielectric loss is below 0.0015. This foamed material exhibits excellent dielectric properties and is suitable for manufacturing high-frequency, high-speed PCBs.

[0022] The third aspect of this application provides a method for preparing a pre-foamed material, comprising the following steps:

[0023] First, a crystalline thermoplastic resin is melt-blended with an initiator, and then an unsaturated monomer is added and melt-blended to obtain a pre-foamed material containing a modified polymer. In this process, under the action of the initiator, the crystalline thermoplastic resin can end-cap the polymer obtained by the polymerization reaction of the unsaturated monomer to obtain a modified polymer.

[0024] The specific feeding sequence described above ensures a high yield of the modified polymer and a wide melting range of the pre-foamed material.

[0025] In this embodiment of the application, based on 100 parts by weight of the crystalline thermoplastic resin, the initiator is 0.1-5 parts by weight, and the unsaturated monomer is 0.1-5 parts by weight. The amount of initiator and unsaturated monomer added is lower than that of the crystalline thermoplastic resin, which helps to ensure a higher yield of modified polymer and fewer byproducts in the pre-foamed material.

[0026] A fourth aspect of this application provides a foaming apparatus for preparing foamed molded articles, comprising:

[0027] A foaming container for holding a product to be foamed, wherein the product to be foamed is the pre-foamed material described in the first aspect of the present application or a molded product of the pre-foamed material;

[0028] A temperature control system is used to heat the foaming container to reach a preset temperature;

[0029] A high-pressure delivery system is used to deliver supercritical foaming agent into the foaming container so that the pressure in the foaming container reaches a preset pressure.

[0030] A pressure relief system is used to release the pressure inside the foaming container after the supercritical foaming agent has saturated the product to be foamed, so that the product to be foamed will foam and form the foamed molded body.

[0031] By using the above-mentioned foaming device to foam the product containing the aforementioned modified polymer, a foamed molded body with uniform cell size, high closed-cell ratio, and low stratification can be obtained.

[0032] A fifth aspect of this application provides a foaming raw material, comprising component A and component B, wherein component A comprises a crystalline thermoplastic resin and an initiator, and component B comprises an unsaturated monomer; wherein, when components A and B are melt-blended, under the action of the initiator, the crystalline thermoplastic resin can end-cap the polymer obtained by polymerizing the unsaturated monomer.

[0033] In this process, components A and B are placed separately. When using the foaming raw material to prepare the above-mentioned pre-foamed material, component A can be converted into a molten state first, and then component B can be added. After a melt blending reaction, a pre-foamed material containing the above-mentioned modified polymer can be obtained.

[0034] The sixth aspect of this application provides the application of the pre-foamed material described in the first aspect of this application and the foaming raw material described in the fifth aspect of this application in the preparation of foamed molded articles. This foamed molded article can also be referred to as a foamed material.

[0035] The seventh aspect of this application provides the application of the pre-foamed material described in the first aspect of this application, the foamed molded body described in the second aspect of this application, and the foaming raw material described in the fifth aspect of this application in the preparation of printed circuit boards, cushioning materials, shock-absorbing materials, heat-insulating materials, and sound-absorbing materials. Among these, the foaming method can be used in the preparation of printed circuit boards, cushioning materials, shock-absorbing materials, heat-insulating materials, and sound-absorbing materials. That is, printed circuit boards, cushioning materials, shock-absorbing materials, heat-insulating materials, and sound-absorbing materials may include foamed molded bodies.

[0036] An eighth aspect of this application provides a laminate comprising a dielectric layer sheet and a metal foil located on the surface of the dielectric layer sheet, wherein the dielectric layer sheet comprises the foamed material described in the second aspect of this application. The dielectric layer sheet in this laminate has low dielectric properties, low water absorption, and low density, making it suitable for manufacturing lightweight, high-frequency, high-speed printed circuit boards.

[0037] A ninth aspect of this application provides a printed circuit board, the printed circuit board including at least one laminate as described in an eighth aspect of this application.

[0038] A tenth aspect of this application provides an electronic component, which includes the printed circuit board described in a ninth aspect of this application.

[0039] According to the eleventh aspect of this application, an electronic device is provided, which includes the electronic components of the tenth aspect of this application or the printed circuit board described in the ninth aspect of this application. Using the electronic components or printed circuit boards of this application can improve the performance of the electronic device.

[0040] This application also provides a modified polymer having the structural formula shown in formula (I):

[0041]

[0042] In formula (Ⅰ), M1 represents the first structural unit derived from an unsaturated monomer, m represents the degree of polymerization of M1, and P1 is independently selected from crystalline thermoplastic resins. This modified polymer has low stereoregularity, a wide melting range, and high melt strength.

[0043] This application also provides the application of the above-mentioned modified polymer in the preparation of foam materials, molding materials, adhesives, and resin compositions. Attached Figure Description

[0044] Figure 1 This is a schematic diagram of the structure of the laminate in the PCB board provided in the embodiments of this application.

[0045] Figure 2 This is a schematic diagram of a foaming apparatus used to prepare a foamed molded article, as provided in an embodiment of this application.

[0046] Figure 3 This is a scanning electron microscope image of the foamed molded article obtained in Example 1 of this application.

[0047] Figure 4 This is a scanning electron microscope image of the foamed molded article obtained in Example 2 of this application.

[0048] Figure 5 This is a scanning electron microscope image of the foamed molded body obtained in Comparative Example 1. Detailed Implementation

[0049] The embodiments of this application are described below with reference to the accompanying drawings.

[0050] PCB boards are typically manufactured by hot-pressing multiple laminates, such as... Figure 1 As shown, the laminate 10 generally includes a dielectric layer sheet 11 and a metal foil 12 located on at least one surface of the dielectric layer sheet 11. The laminate 10 is generally a copper-clad laminate (CCL), which may include the dielectric layer sheet 11 and copper foils formed on opposite sides of the dielectric layer sheet 11. Signal transmission in the PCB board takes place on the metal foil 12. The dielectric layer sheet 11 between the metal foils 12 acts as an isolation layer. The lower the dielectric constant of the dielectric layer sheet 11, the smaller its impact on signal delay; the lower the dielectric loss of the dielectric layer sheet 11, the smaller its impact on signal attenuation. Therefore, as the signal transmission frequency and rate of communication technology increase, the requirements for low signal delay and low attenuation also increase. The fabrication of dielectric layer materials with low dielectric constant and low dielectric loss is a future development trend for PCB circuit boards. Furthermore, considering the ease of assembly and transportation of PCB boards, the requirement for lightweight PCB boards is also increasing. Therefore, there is a need to provide lightweight dielectric layer materials with good dielectric properties.

[0051] To match high-frequency and high-speed communication technologies, this application provides a pre-foamed material suitable for preparing the aforementioned dielectric layer sheet 11 in a PCB board by a foaming method, thereby giving the foamed molded body—dielectric layer sheet 11 good dielectric properties, as well as light density and low water absorption.

[0052] Specifically, this application provides a pre-foamed material comprising a modified polymer, wherein the modified polymer has a first structural unit derived from an unsaturated monomer, and the ends of the molecular chains of the modified polymer are capped with a crystalline thermoplastic resin.

[0053] Crystalline thermoplastic resins generally have a melting point and a relatively orderly molecular arrangement. The more orderly the molecular arrangement, the narrower the melting range of the crystalline thermoplastic resin, and the higher the precision required to control the foaming temperature when using it for foaming. Furthermore, when using unmodified crystalline thermoplastic resins to manufacture pre-foamed materials, such as during injection molding, the high regularity of the crystalline thermoplastic resin's three-dimensional structure makes it easy for the surface polymers to align along the mold. This results in an inconsistency between the surface and inner layers of the pre-foamed material (specifically, the foaming particles), with the surface structure generally being denser. This leads to less supercritical gas dissolving in the surface layer and more in the inner layer during supercritical foaming. While rapid pressure release generates cells, the resulting foamed molded body is also prone to delamination. Additionally, the low melt strength of crystalline thermoplastic resins cannot support cell growth, resulting in mostly open-cell foams and a low water absorption rate in the foamed molded body.

[0054] The modified polymer provided in this application is a novel polymer composed of structural units of unsaturated monomers and crystalline thermoplastic resins. Compared with pure crystalline thermoplastic resins, the regularity of the three-dimensional structure of the modified polymer is destroyed or reduced. Therefore, the melting range of the modified polymer is widened and the relaxation time is longer. When using pre-foamed materials containing the modified polymer for foaming, the foaming temperature does not need to be strictly controlled because of its widened melting range. Furthermore, the longer relaxation time of the pre-foamed material can improve the stable growth time of the cells during the foaming process, which is beneficial to improving the uniformity of the cells. Furthermore, due to the low regularity of the three-dimensional structure of the aforementioned modified polymers, the molecular arrangement of the polymers in the surface and inner layers of the pre-foamed material is not significantly different. This ensures that when using the pre-foamed material for supercritical foaming, the amount of supercritical gas dissolved in the surface and inner layers of the pre-foamed material is basically the same, thus making the resulting pre-foamed material less prone to stratification. In addition, compared to simple crystalline thermoplastic resins, the aforementioned modified polymers have a higher melt strength, and the melt strength of the pre-foamed material is also correspondingly higher. During the foaming process, this can support the formation of cells, ensuring that most of the cells in the resulting pre-foamed material are closed cells, reducing its water absorption rate and improving its mechanical strength.

[0055] In this application, the term "relaxation time" refers to the time required for an object to return to its normal state after being deformed by an external force and the force is removed. The relaxation time can be calculated using Maxwell's constitutive equation model. The aforementioned pre-foamed material can specifically be foaming particles or pre-foamed particles, and its shape is not particularly limited; it can be cylindrical, spherical, ellipsoidal, strip-shaped, rod-shaped, block-shaped, sheet-shaped, etc. In this application, the molecular chain ends of the aforementioned modified polymer are capped with crystalline thermoplastic resin. Here, "crystalline thermoplastic resin" specifically refers to the crystalline thermoplastic resin portion connected to the first structural unit, that is, the parent crystalline thermoplastic resin.

[0056] In this embodiment of the application, the modified polymer has the structural formula shown in formula (Ⅰ):

[0057]

[0058] In formula (Ⅰ), M1 represents the first structural unit derived from an unsaturated monomer, m represents the degree of polymerization of M1, and P1 is independently selected from crystalline thermoplastic resins.

[0059] The modified polymer described above may contain one first structural unit or multiple first structural units with different structures. Furthermore, the two end-capping groups P1 located at the ends of the molecular chains of the modified polymer may be the same or different crystalline thermoplastic resins. In the embodiments of this application, the two P1 groups in formula (I) above are preferably the same.

[0060] In this application, the crystalline thermoplastic resin includes one or more of syndiotactic polystyrene (sPS), polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), perfluoroalkoxy vinyl ether polymers, polyphenylene sulfide (PPS), polyether ether ketone, and liquid crystal polymers, but is not limited thereto. In some embodiments, the crystalline thermoplastic resin includes one or more of sPS, PTFE, polyphenylene sulfide, and liquid crystal polymers. These four types of resins have good heat resistance and low dielectric properties, making them more suitable for manufacturing PCB boards. Specifically, polyphenylene sulfide has a melting point of around 280°C and a dielectric loss factor Df of around 0.002; PTFE has a dielectric loss factor Df of around 0.005-0.0008. The dielectric loss of the liquid crystal polymer is between 0.0006 and 0.002. Exemplary liquid crystal polymers can be type I and type II, with corresponding heat distortion temperatures of above 300°C and 240-280°C, respectively.

[0061] In this application, the unsaturated monomers possess unsaturated bonds such as carbon-carbon double bonds and carbon-carbon triple bonds in their molecular structure, thereby exhibiting certain polymerization reactivity during the preparation of the aforementioned pre-foamed materials. In the embodiments of this application, the unsaturated monomers possess carbon-carbon double bonds in their molecular structure. The unsaturated monomers may include one or more of styrene, maleic anhydride, pentaerythritol triacrylate, methacrylate, glycidyl methacrylate, and ethyl acrylate, but are not limited to these. Structural units derived from these monomers help improve the melt strength of the modified polymer, thereby effectively alleviating the problems of delamination and predominantly open-cell structures in the foamed molded articles obtained from the aforementioned pre-foamed materials, while having minimal impact on the dielectric properties of the modified polymer.

[0062] In this embodiment of the application, the modified polymer is obtained by reacting the following raw materials in parts by weight: 100 parts of crystalline thermoplastic resin matrix, 0.1-5 parts of unsaturated monomer, and 0.1-5 parts of initiator.

[0063] At a certain temperature, an initiator can cause free radicals to be generated on the molecular chains of crystalline thermoplastic resins, serving as reaction sites to initiate the polymerization reaction of unsaturated monomers, thereby obtaining a modified polymer with the aforementioned structure. From another perspective, the introduction of the initiator and unsaturated monomers causes micro-crosslinking of the crystalline thermoplastic resin, disrupting its stereoregularity. Therefore, the modified polymer has a wider melting range, increased molecular entanglement, increased viscosity, and a longer relaxation time. Understandably, when preparing this modified polymer, the initiator should be mixed with the crystalline thermoplastic resin matrix first, followed by the addition of the unsaturated monomers. This prevents the highly reactive unsaturated monomers from undergoing polymerization under the initiator's action before being capped by the crystalline thermoplastic resin when the crystalline thermoplastic resin matrix, unsaturated monomers, and initiator are added simultaneously. Furthermore, the amount of unsaturated monomers added is small; their presence will not significantly affect the low dielectric properties of the modified polymer capped by the crystalline thermoplastic resin, nor will it cause excessive micro-crosslinking that would affect molding and processing performance. A smaller amount of initiator also helps reduce the probability of unsaturated monomers undergoing self-polymerization.

[0064] Taking crystalline thermoplastic resin, specifically sPS, as an example, the reaction formula for preparing the above-mentioned modified polymer can be as follows:

[0065]

[0066] In this application, the initiator can be an organic peroxide compound initiator, which can thermally decompose to generate free radicals on the molecular chain of the crystalline thermoplastic resin as reaction sites. The initiator may include, but is not limited to, one or more of the following: dicumyl peroxide (DCP), bis(tert-butylperoxyisopropyl)benzene, 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, 2-(tert-butylperoxyisopropyl)benzene, butanone peroxide, benzoyl peroxide, and dodecyl peroxide.

[0067] In this embodiment, the pre-foamed material further contains an antioxidant. The presence of the antioxidant enhances the antioxidant properties of the modified polymer during the granulation process of the pre-foamed material, preventing it from aging and degrading due to heat and oxygen, thus losing its usability. Specifically, the antioxidant may include one or more of antioxidant 1010 (chemical name: pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]), antioxidant 168 (chemical name: tris[2,4-di-tert-butylphenyl]phosphite), and antioxidant 1790, but is not limited to these. In this embodiment, the mass of the antioxidant in the pre-foamed material can be 0.09wt%-1wt% of the mass of the modified polymer, for example, 0.1wt%, 0.3wt%, 0.5wt%, 0.6wt%, or 0.9wt%.

[0068] In this embodiment, the modified polymer or the pre-foamed material, measured by Differential Scanning Calorimetry (DSC) at a heating rate of 10°C for 1 minute, has a melting range of over 15°C and a melting point of over 270°C. This wide melting range reduces the difficulty of precisely controlling the foaming temperature during the foaming process. The high melting point of the modified polymer or the pre-foamed material results in pre-foamed materials with good heat resistance, making them suitable for use in PCBs requiring high high-temperature resistance. In some embodiments, the melting range of the modified polymer or the pre-foamed material is over 20°C, or even over 25°C.

[0069] This application also provides a method for preparing the above-mentioned pre-foamed material, including the following steps:

[0070] First, a crystalline thermoplastic resin is melt-blended with an initiator, and then an unsaturated monomer is added and melt-blended to obtain a pre-foamed material containing a modified polymer. In this process, under the action of the initiator, the crystalline thermoplastic resin can end-cap the polymer obtained by the polymerization reaction of the unsaturated monomer to obtain the modified polymer.

[0071] In the above preparation method, the initiator is first melt-blended with a crystalline thermoplastic resin matrix, and then the unsaturated monomer is added. This facilitates the generation of free radicals on the molecular chains of the crystalline thermoplastic resin as reaction sites to initiate the polymerization reaction of the unsaturated monomer, thereby obtaining a modified polymer with the aforementioned structural and physicochemical properties. This avoids the situation where the crystalline thermoplastic resin matrix, unsaturated monomer, and initiator are added simultaneously, causing the highly reactive unsaturated monomer to polymerize under the action of the initiator without being capped by the crystalline thermoplastic resin. Therefore, this specific order of addition ensures a high yield of the modified polymer and a wide melting range for the pre-foamed material.

[0072] In some embodiments of this application, after adding the initiator and performing melt blending for approximately 20-60 seconds, the unsaturated monomer is added and further melt blending is performed. The total melt blending time can be 3-30 minutes, for example 5-20 minutes, and more specifically 5-10 minutes. The melt blending temperature can be 270-300°C, for example 275, 280, 285, 290, or 295°C.

[0073] In this embodiment, based on 100 parts by weight of the crystalline thermoplastic resin, the initiator comprises 0.1-5 parts by weight, and the unsaturated monomer comprises 0.1-5 parts by weight. The amounts of initiator and unsaturated monomer added are lower than those added to the crystalline thermoplastic resin. This helps to ensure a higher yield of the modified polymer in the resulting product and fewer byproducts (such as polymers containing unsaturated monomers). Specifically, the lower amount of unsaturated monomer does not significantly affect the low dielectric properties and molding / processing properties of the modified polymer (e.g., it does not turn the modified polymer into a thermosetting resin, making injection molding impossible), while simultaneously improving the melt strength of the modified polymer and reducing the probability of delamination and open-cell formation during foaming of the pre-foamed material.

[0074] In this embodiment, based on 100 parts by weight of crystalline thermoplastic resin, the initiator can be 0.2 parts, 0.4 parts, 0.5 parts, 0.6 parts, 0.8 parts, 1 part, 1.5 parts, 2 parts, 3 parts, or 4 parts by weight, etc.; in some embodiments, the initiator is 0.2-2 parts by weight. Based on 100 parts by weight of crystalline thermoplastic resin, the unsaturated monomer can be 0.2 parts, 0.4 parts, 0.5 parts, 0.6 parts, 0.8 parts, 1 part, 1.5 parts, 2 parts, 3 parts, 4 parts, or 4.5 parts by weight, etc.; in some embodiments, the unsaturated monomer is 0.2-4 parts by weight, and more specifically, 0.2-2 parts.

[0075] In some embodiments of this application, an antioxidant is also used in the preparation of the pre-foamed material. This antioxidant may be added entirely with the crystalline thermoplastic resin and the initiator; or entirely with the unsaturated monomer; or a portion may be added with the crystalline thermoplastic resin and the initiator, and another portion with the unsaturated monomer. Specifically, based on 100 parts by weight of the crystalline thermoplastic resin, the initiator is 0.1-1 parts by weight, for example, 0.2 parts, 0.5 parts, 0.6 parts, 0.8 parts, or 0.9 parts, etc. The role of the antioxidant is as described above in this application and will not be repeated here.

[0076] Furthermore, in other embodiments of this application, other additives may be added during the preparation of the pre-foamed material, and these other additives will not adversely affect the foaming performance and the cell structure after foaming of the pre-foamed material. These other additives include, but are not limited to, at least one of: slip agents, antistatic agents, anti-sticking agents, plasticizers, and flame retardants.

[0077] In this application, the aforementioned melt blending can be carried out in a mixing equipment, which can provide shearing, mixing, heating, and optionally granulation and material conveying equipment. Exemplarily, the mixing equipment can be a melt extruder, a Hacker internal mixer, or a two-roll mill, but is not limited to these. Accordingly, the melt blending method can be extrusion melt blending, Hacker internal mixer melt blending, or two-roll melt blending, etc. Among these, extrusion melt blending and Hacker internal mixer melt blending are closed-loop melt blending, while two-roll melt blending is open-loop melt blending.

[0078] Specifically, when using a melt extruder as the mixing equipment, the aforementioned crystalline thermoplastic resin, initiator, and unsaturated monomer can be heated and melted in the extruder. The screw of the extruder rotates at a certain speed, continuously extruding, mixing, and reacting the molten mixture. The reacted material can be extruded from the die of the extruder into strips, and then cut into granules by rotating blades to obtain the aforementioned granular pre-foamed material. When using a Hacker internal mixer as the mixing equipment, the aforementioned crystalline thermoplastic resin, initiator, and unsaturated monomer can be heated and melted in the internal mixer. The rotor movement in the internal mixer performs shearing, kneading, and reaction. The reacted material is then granulated using auxiliary equipment such as shears to obtain the aforementioned pre-foamed material. When a two-roll mill is used as the mixing equipment, the above-mentioned crystalline thermoplastic resin, initiator, and unsaturated monomer can be heated and melted in the two-roll mill. The two rolls of the two-roll mill rotate in opposite directions at a certain speed, which drives the molten mixture to be continuously squeezed, mixed, and reacted. The reacted material is a sheet sample, which can be prepared into granules with the help of auxiliary equipment such as scissors to obtain the above-mentioned pre-foamed material.

[0079] As described above, due to the low regularity of the three-dimensional structure of the modified polymer, when the material containing the modified polymer is granulated into a pre-foamed material, the modified polymer on the surface of the granulation cavity is not easily oriented along the mold. Therefore, there is no significant difference in the arrangement of the modified polymer in the surface and inner layers of the obtained pre-foamed material, which is beneficial for obtaining a foamed molded body that is not easy to delaminate after foaming.

[0080] In this application, the shape of the pre-foamed material is not particularly limited, and it can be relatively small in size, such as cylindrical, spherical, ellipsoidal, strip, rod, block, or sheet. In some embodiments of this application, the pre-foamed material is in fragment form. Before foaming, the pre-foamed material can be formed into a product to be foamed with a certain shape, for example, by hot pressing to transform it into a sheet-like product to be foamed, and then the sheet-like product can be directly foamed.

[0081] The preparation method of the pre-foamed material provided in this application is simple to operate. The modified polymer contained in the pre-foamed material has a novel structure and low regularity of three-dimensional structure. It has a wide melting range and high melt strength, which is conducive to the smooth foaming of the pre-foamed material to obtain a foamed molded body that is not easy to delaminate, and improves its closed-cell rate, mechanical strength, etc.

[0082] Accordingly, this application also provides a foaming raw material that can be used to prepare the above-mentioned pre-foamed material. The foaming raw material includes component A and component B, wherein component A includes a crystalline thermoplastic resin and an initiator, and component B includes an unsaturated monomer. When components A and B are melt-blended, under the action of the initiator, the crystalline thermoplastic resin can end-cap the polymer obtained by polymerizing the unsaturated monomer.

[0083] In this process, components A and B are placed separately. When preparing the pre-foamed material using this foaming raw material, component A can be first converted into a molten state, and then component B can be added. After a melt blending reaction, a pre-foamed material containing the modified polymer is obtained. In this application, the molding method for converting the above-mentioned foaming raw material into a pre-foamed material is not limited, and it can be one or more of the following: extrusion molding, injection molding, compression molding, blow molding, die casting, vacuum forming, etc.

[0084] As described above in this application, based on 100 parts by weight of the crystalline thermoplastic resin, the initiator comprises 0.1-5 parts by weight, and the unsaturated monomer comprises 0.1-5 parts by weight. In some embodiments of this application, component A and component B further contain antioxidants or other additives. Specifically, based on 100 parts by weight of the crystalline thermoplastic resin, the antioxidant comprises 0.1-1 parts by weight.

[0085] This application also provides a foamed molded article, which is obtained by foaming the pre-foamed material as described above in the embodiments of this application, or by preparing it from the foaming raw materials described above in the embodiments of this application. Accordingly, the foamed molded article contains the above-mentioned modified polymer.

[0086] In this application, the foamed molded body can be obtained directly by foaming the above-mentioned pre-foamed material, or the pre-foamed material can be processed into a product to be foamed that corresponds to the shape of the foamed molded body, and then the product to be foamed can be obtained.

[0087] In some embodiments of this application, the foaming process is specifically a supercritical foaming process. Exemplarily, the preparation process of the foamed molded article includes:

[0088] S1, the pre-foamed material is molded into a product to be foamed;

[0089] S2, the product to be foamed is subjected to supercritical foaming treatment to obtain a foamed molded body.

[0090] In step S1, the pre-foamed material is molded into a product to be foamed under heating to melt and integrate the pre-foamed material, for example, by hot pressing to transform it into a product with a certain shape. The shape of the product to be foamed corresponds to the shape of the desired foamed molded body, and their thicknesses may differ; understandably, the thickness of the foamed molded body is greater than that of the product to be foamed.

[0091] The supercritical foaming process in step S2 may specifically include the following steps:

[0092] S21, Place the product to be foamed in a foaming container that can withstand high pressure and high temperature, and heat the foaming container to a preset temperature;

[0093] S22, introduce supercritical foaming agent into the foaming container to make the pressure inside the foaming container reach a preset pressure, so as to impregnate the product to be foamed;

[0094] S23, release the pressure inside the foaming container to allow the product to be foamed to form a foamed molded body.

[0095] In this embodiment, the supercritical blowing agent includes carbon dioxide (CO2, critical temperature 31.1℃, critical pressure 7.38MPa), nitrogen (N2, critical temperature -147℃, critical pressure 3.39MPa), or combinations thereof. In some embodiments, a co-blowing agent is also introduced into the foaming container in step S22. The co-blowing agent can be one or more of ethanol, propanol, isopropanol, acetone, and ethyl acetate. The presence of the co-blowing agent increases the absorption of the supercritical blowing agent by the product to be foamed. It is understood that the supercritical blowing agent and the co-blowing agent should be inert to the product to be foamed.

[0096] In step S21, the preset temperature can be set according to the melting point of the supercritical foaming agent and the modified polymer. The preset temperature should be higher than the critical temperature of the supercritical foaming agent to ensure that the foaming agent is in a supercritical state. Correspondingly, in step S22, when the supercritical foaming agent is introduced into the foaming container, the preset pressure reached in the foaming container should be maintained higher than the critical pressure of the supercritical foaming agent to ensure that the foaming agent is in a supercritical state, facilitating diffusion into the product to be foamed and achieving a high solubility therein. The impregnation process is to allow the product to be foamed to absorb a certain amount of supercritical foaming agent. In some embodiments, when the supercritical foaming agent is CO2, the preset temperature can be in the range of 270-300℃, such as 270, 275, 280, 285, 290℃, etc.; the preset pressure of the foaming container in step S22 can be in the range of 8-20MPa, such as 9, 10, 12, 15, 18, or 20MPa, etc.

[0097] In step S23, after the product to be foamed is saturated with the supercritical foaming agent (or after the supercritical foaming agent reaches dissolution equilibrium), the pressure inside the foaming container can be released all at once or in stages. This process can also be called "pressure relief," that is, reducing the pressure inside the foaming container, for example, to atmospheric pressure. During the pressure relief process, a large number of cell nuclei are generated in the product to be foamed. The continuous growth of the cell nuclei results in a foamed molded body with cells. In some embodiments, the pressure inside the foaming container is reduced to atmospheric pressure at a rate of 0.8-10 MPa / s. Optionally, the pressure relief time can be 2-10 seconds.

[0098] The above-described supercritical foaming process can be carried out in a foaming apparatus. See [link / reference] Figure 2 The foaming device 200 may include:

[0099] Foaming container 21, used to hold product 201 to be foamed;

[0100] Temperature control system 22 is used to heat foam container 21 to reach preset temperature;

[0101] High-pressure delivery system 23 is used to deliver supercritical foaming agent into foam container 21 so that the pressure in foam container 21 reaches the preset pressure;

[0102] The pressure relief system 24 is used to release the pressure inside the foaming container 21 after the supercritical foaming agent has saturated the product to be foamed 201, so that the product to be foamed 201 foams and forms a foamed molded body.

[0103] In this embodiment, the temperature control system 22 includes a heating component 221 and a temperature sensor 222. The heating component 221 provides a heat source to the foaming container 21 to bring the temperature inside the foaming container 21 to a preset value. The temperature sensor 222 monitors the temperature inside the foaming container 21. The foaming container 21 may specifically be a foaming mold.

[0104] In this embodiment, the high-pressure delivery system 23 includes a fluid source 231 (usually a gas source, such as CO2, N2, etc.), a pump 232, an air inlet pipe 233, and an air inlet valve 234. The pump 232 is piped between the fluid source 231 and the foaming container 21. The cavity of the foaming container 21 is connected to the pump 232 via the air inlet pipe 233, which is equipped with the air inlet valve 234. The air inlet valve 234 can regulate the flow rate of the supercritical foaming agent delivered to the foaming container 21, the pressure of the foaming container 21, etc. Furthermore, a pressure sensor 202 is also provided on the foaming container 21 to facilitate monitoring of the pressure inside the foaming container 21. In this application, the number of air inlet pipes 233, air inlet valves 234, and fluid sources 231 can be one or more, depending on the type of supercritical foaming agent and whether a co-foaming agent is used.

[0105] In this embodiment, the pressure relief system 24 includes a pressure relief channel 241 communicating with the foaming container 21. A pressure relief valve 242 is provided on the pressure relief channel 241 to release the pressure inside the foaming container 21 when needed. Understandably, the foaming container 21 is provided with an air inlet I1 and an air outlet O1. An air inlet pipe 233 communicates with the foaming container 21 through the air inlet I1, and the pressure relief channel 241 communicates with the foaming container 21 through the air outlet O1. Of course, in other embodiments of this application, the pressure relief valve may also be directly provided on the foaming container 21.

[0106] In some embodiments of this application, the foaming apparatus 200 further includes a hydraulic system 25 for providing pressure to close the foaming container 21 containing the article 201 to be foamed, thereby bringing the foaming container 21 into a closed state to facilitate heating, fluid delivery, etc. Understandably, the hydraulic system 25 is in communication with the cavity of the foaming container 21.

[0107] By using the above-mentioned foaming device to foam the product containing the aforementioned modified polymer, a foamed molded body with uniform cell size, high closed-cell ratio, and low stratification can be obtained.

[0108] In this application, the shape of the foamed molded body is not limited; for example, it can be sheet-like, block-like, rod-like, tubular, column-like, or other shapes. In some embodiments of this application, when the foamed molded body is used in a PCB board, such as specifically as... Figure 1 The medium layer sheet 11 in the foamed body can be in sheet form, or the foamed body can be referred to as a "foamed sheet".

[0109] In this application, the foamed molded body has a porous structure. Most of the cells in the foamed molded body are closed-cell. In embodiments of this application, the closed-cell ratio (also referred to as "closed-cell rate") of the foamed molded body is above 50%, for example, above 55%, above 60%, or even above 80%. A higher closed-cell ratio helps ensure that the foamed molded body has excellent water resistance. Specifically, the closed-cell ratio can be 50%, 52%, 55%, 58%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 99%, or 100%, etc. In some embodiments, the closed-cell ratio of the foamed molded body can be 50%-80%, and more specifically, 50%-60%. The closed-cell ratio of the foamed molded body can be measured according to the GB1T 10799-2008 standard.

[0110] In this embodiment, the water absorption rate of the foamed molded body after being placed in water for 24 hours at a temperature of 23°C and a relative humidity of 50% is less than 1%. A lower water absorption rate is beneficial for extending the service life of the foamed molded body, especially in humid environments. In some embodiments, the aforementioned water absorption rate of the foamed molded body is less than 0.8%, and in some cases, it can be less than 0.7%, or even less than 0.6%.

[0111] The water absorption rate was tested according to GB / T 8810-2005. First, a sample with dimensions of 10mm × 10mm was prepared, dried at 100℃ for 2 hours, and its weight was measured. Then, the sample was placed in water and kept in an environment with a temperature of 23℃±2℃ and a relative humidity of 50%±5% for 24 hours. Afterward, the sample was removed, the surface moisture was wiped dry with filter paper, and it was weighed immediately. The water absorption rate was reflected by the weight change of the sample before and after being placed in water.

[0112] In this embodiment, the average cell size of the foamed body is in the range of 5-100 μm. This average cell size can refer to the average of the maximum width of the open cross-section of each cell. The relatively small average cell size of the foamed body allows for better conduction of the upper and lower metal foil circuitry in the laminate 10 when used as the dielectric layer sheet 11 of the laminate 10 in a PCB board, thanks to the metal film (such as copper film) deposited within the cells, thus shortening the circuit path. In some embodiments of this application, the average cell diameter of the foamed body is 10 μm-60 μm.

[0113] In this embodiment of the application, the density of the foamed molded body is 1g / cm³. 3 The apparent density of porous foam can be tested according to GB1T6343-2009 standard. Lower density foam moldings are beneficial for achieving lightweight devices using them. In particular, when this foam molding is used in PCB boards, it facilitates the transportation and installation of the PCB. In some embodiments, the density of the foam molding is 0.1-0.8 g / cm³. 3 In other embodiments, the density of the foamed molded body is 0.2-0.6 g / cm³. 3 Even as low as 0.2-0.4 g / cm³ 3 .

[0114] In this embodiment, the dielectric constant Dk of the foamed material under electromagnetic waves at a frequency of 10 GHz is measured to be below 2.0, and the dielectric loss Df is below 0.0015, based on the resonant cavity method. This indicates that the foamed material has excellent dielectric properties. Using it to fabricate PCBs results in less impact on signal delay and attenuation, enabling the PCBs to meet the requirements of high-frequency and high-speed communication. The dielectric constant Dk and dielectric loss Df can be measured using the splice postdielectric resonator (SPDR) method at a test frequency of 10 GHz.

[0115] This application also provides the application of the aforementioned pre-foamed material, the aforementioned foamed molded body, and the aforementioned foaming raw material in the preparation of lightweight materials such as printed circuit boards (specifically used as low-dielectric materials for printed circuit boards), cushioning materials, shock-absorbing materials, heat-insulating materials, and sound-absorbing materials. Among these, printed circuit boards, cushioning materials, heat-insulating materials, and sound-absorbing materials can be obtained through a foaming method. It should be noted that the applications of the pre-foamed material, foamed molded body, and foaming raw material mentioned in this application are not limited to the manufacture of printed circuit boards, cushioning materials, and shock-absorbing materials; they can also be used in other application scenarios as needed.

[0116] Specifically, when the aforementioned pre-foamed materials, foamed molded bodies, and foaming raw materials are used to manufacture printed circuit boards, they can be used as dielectric materials in the laminates of printed circuit boards. Furthermore, when used to manufacture cushioning materials, they can be used as cushioning structures between adjacent components or layers in electronic assemblies.

[0117] Accordingly, embodiments of this application provide a laminate comprising the foamed molded body described above in embodiments of this application. Printed circuit boards can be manufactured using this laminate.

[0118] The structure of the laminate is as described above in this application. Figure 1 The laminate 10 includes a dielectric layer sheet 11 and a metal foil 12 located on the surface of the dielectric layer sheet 11. The dielectric layer sheet 11 can be the foamed molded body described in the embodiments of this application. In some cases, the laminate can also be referred to as a "metal-clad laminate". The dielectric layer sheet in this laminate has low dielectric properties, low water absorption, and low density, making it suitable for manufacturing lightweight, high-frequency, and high-speed printed circuit boards.

[0119] Metal foil 12 can be placed on one side or opposite sides of the dielectric layer sheet 11. The metal foil 12 can be copper foil, aluminum foil, nickel foil, silver foil, or its alloy foil, etc. Copper foil is the most common, and the laminate 10 with copper foil can be called a "copper-clad laminate". The laminate 10 can be obtained by the following method: taking the above-mentioned foamed molded body as the dielectric layer sheet 11, placing metal foil 12 on one side or opposite sides of it, and then hot-pressing them together to obtain the laminate 10.

[0120] This application also provides a printed circuit board, which includes at least one of the laminates described in this application embodiment.

[0121] The printed circuit board may include one of the aforementioned laminates, or a stacked structure comprising at least two laminates. Multiple laminates may be stacked by hot pressing.

[0122] Furthermore, the metal foil 12 of the aforementioned laminate 10 also has circuitry. Specifically, a photosensitive film is laminated onto the surface of the metal foil 12 of the laminate 10, and the photosensitive film is exposed and developed under a circuit mask to obtain a patterned photosensitive layer. This layer is then used as a mask to etch copper foil, and the photosensitive film is removed to obtain a laminate with circuitry patterns. Multiple laminates 10 with circuitry patterns can then be hot-pressed together to obtain a stacked board. By drilling holes in the stacked board and chemically depositing copper on the hole walls, signal conduction between different laminates can be achieved. Finally, a solder mask layer can be applied to the outer circuitry pattern of the stacked board, and surface treatment can be performed to obtain a complete printed circuit board.

[0123] This application also provides an electronic component, which includes the printed circuit board described above in this application embodiment.

[0124] In addition to the aforementioned printed circuit board, the electronic component may also include various electronic components attached to the printed circuit board (such as various chips, transistors, LED devices, resistive, capacitive and inductive components (such as resistors, capacitors, and inductors)), as well as the plastic encapsulation structure covering them.

[0125] This application also provides an electronic device, which includes the electronic components described in the embodiments of this application or the printed circuit board described in the embodiments of this application.

[0126] The electronic components or printed circuit boards used in the embodiments of this application can improve the performance of electronic devices. These electronic devices can be mobile phones, tablets, laptops, desktop computers, wearable devices (such as smartwatches and smart bracelets), portable devices, base station antennas, automotive radars, and other products.

[0127] This application also provides a modified polymer having the structural formula shown in formula (Ⅰ):

[0128]

[0129] In formula (Ⅰ), M1 represents the first structural unit derived from the unsaturated monomer, m represents the degree of polymerization of M1, and P1 is independently selected from crystalline thermoplastic resins. The descriptions of the unsaturated monomers and crystalline thermoplastic resins are as described above in this application.

[0130] In this embodiment, the modified polymer, measured by differential scanning calorimetry at a heating rate of 10°C for 1 minute, has a melting range of over 15°C and a melting point of over 270°C. This modified polymer is suitable as a raw material for preparing pre-foamed materials, resulting in foamed molded bodies with high closed-cell ratios and minimal delamination.

[0131] This application also provides the application of the modified polymer described above in the preparation of foamed materials, molding compounds, adhesives, and resin compositions. The modified polymer can be used as a raw material for preparing the aforementioned foaming materials, pre-foamed materials, products to be foamed, and foamed molded bodies. Furthermore, the modified polymer can also be used as molding compounds and adhesives, which can be manufactured through injection molding, injection molding, compression molding, casting, or coating.

[0132] In this application, "at least one" means one or more, and "more than one" means two or more. "At least one of the following" or similar expressions refer to any combination of these items, including any combination of single or multiple items. For example, "at least one of a, b or c", or "at least one of a, b and c", can both mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, and c can be single or multiple.

[0133] In this application, "and 1 or" describes the relationship between related objects, indicating that three relationships can exist. For example, A and 1 or B can represent: A existing alone, A and B existing simultaneously, or B existing alone, where A and B can be singular or plural. The character "1" generally indicates that the preceding and following related objects have an "or" relationship.

[0134] Furthermore, when this application refers to a parameter range as "below c" or "above d", it includes the number itself. For example, when a parameter is below c, it means that the value includes the number c and any value smaller than c. Similarly, when a parameter is in the range of e to f, it also includes the number itself, meaning it includes the endpoint value e, the endpoint value f, and any value between e and f.

[0135] The embodiments of this application will be further described below with reference to several specific examples. However, the embodiments of this application are not limited to the specific examples described below.

[0136] Example 1

[0137] Preparation of pre-foamed materials (specifically, foaming particles):

[0138] 100 parts by weight of syndiotactic polystyrene (sPS) resin particles, 0.5 parts by weight of initiator—dicumyl peroxide (DCP), 0.25 parts by weight of antioxidant 1010, and 0.25 parts by weight of antioxidant 168 were stirred evenly and then added to a Hacker internal mixer for melt blending. The Hacker internal mixer was operated at 50 rpm, and the melt blending temperature was 285°C. After 30 seconds, 0.5 parts by weight of styrene containing double bonds was added to the Hacker internal mixer, and melt blending continued for a total melt blending time of 5 minutes. The resulting sample was then removed from the Hacker internal mixer and cut into 3mm × 3mm fragments. These fragments are the desired foaming particles. The foaming particles contain the modified polymer P1, which is obtained by end-capping the polymer obtained by the polymerization reaction of styrene monomers under the action of an initiator.

[0139] The reaction formulas involved in the above melt blending process are as follows:

[0140]

[0141] The melting point of the foaming particles containing the modified polymer P1 was measured to be 273°C, the melting range to be 25°C, and the relaxation time to be approximately 33 seconds.

[0142] Preparation of foamed molded parts:

[0143] (1) The foaming particles described in Example 1 were placed into a mold of a 50 mm diameter disc and pressed on a flat vulcanizing machine at a pressing temperature of 285 °C, a pressure of 10 MPa, and a pressing time of 5 min. After pressing, the disc was removed from the mold to obtain a 50 mm diameter disc containing the modified polymer P1, which was used as the product to be foamed.

[0144] (2) Place the above-mentioned product to be foamed in a high pressure vessel and heat the high pressure vessel to the required foaming temperature of 280°C; then introduce CO2 into the vessel to purge the air in the vessel, repeat the purging three times, and then introduce CO2 into the vessel until the pressure in the vessel reaches 14MPa. At 280°C, let the product to be foamed be impregnated with CO2 for 40 minutes to achieve absorption saturation; then quickly depressurize through the high pressure ball valve set on the pipe connected to the high pressure vessel, and depressurize the vessel to atmospheric pressure within 6 seconds to make the product to be foamed. Finally, take out the obtained foamed molded body from the high pressure vessel, which is in sheet form.

[0145] Figure 3 This is a scanning electron microscope (SEM) image of the foamed molded article obtained in Example 1 of this application. Figure 3 It can be seen that the foamed molded body has relatively uniform cell size, and most of them are closed cells. Based on this, the average cell size can be calculated to be 30μm.

[0146] In this application, the density of the foamed molded body obtained in Example 1 was measured to be 0.38 g / cm³, according to the method described above. 3 The closed-cell rate is 50.4%, the water absorption rate is 0.54%, and the flexural strength is 3.5 MPa. The dielectric constant Dk of the foamed molded body is 1.7 and the dielectric loss Df is 0.0006 under electromagnetic waves at a frequency of 10 GHz.

[0147] Example 2

[0148] The difference between Example 2 and Example 1 is that, in preparing the foaming particles, 0.5 parts by weight of pentaerythritol triacrylate (PETA) was used to replace the styrene monomer used in Example 1. Thus, the foaming particles of Example 2 contain the modified polymer P2, which is obtained by end-capping the polymer obtained by polymerizing PETA monomer with sPS resin under the action of initiator DCP.

[0149] In Example 2, the synthesis reaction formula of the modified polymer P2 involved in the preparation of foaming particles is as follows:

[0150]

[0151] The melting point of the foaming particles containing the above-mentioned modified polymer P2 was measured to be 272°C, the melting range was 20°C, and the relaxation time was approximately 32 seconds.

[0152] According to the method described in Example 1, the foaming particles obtained in Example 2 were prepared into a foamed molded body.

[0153] in, Figure 4 This is a SEM image of the foamed molded article obtained in Example 2 of this application. From... Figure 4 It can be seen that the foamed molded body has relatively uniform cell size, and most of them are closed cells. Based on this, the average cell size can be calculated to be 40μm.

[0154] Furthermore, the density of the foamed molded body obtained in Example 2 was measured to be 0.36 g / cm³. 3 The closed-cell rate is 56.3%, the water absorption rate of the foamed molded body is 0.59%, and the flexural strength is 3.3 MPa. The dielectric constant Dk of the foamed molded body under electromagnetic waves at a frequency of 10 GHz is 1.5, and the dielectric loss Df is 0.0005.

[0155] Example 3

[0156] The difference between Example 3 and Example 1 is that, in preparing the foaming particles, 0.5 parts by weight of maleic anhydride (MA) was used to replace the styrene monomer used in Example 1, and BPO was used instead of DCP used in Example 1. Thus, the foaming particles of Example 3 contain the modified polymer P3, which is obtained by end-capping the polymer obtained by the polymerization reaction of MA monomer with sPS resin under the action of initiator BPO.

[0157] In Example 3, the synthesis reaction formula of the modified polymer P3 involved in the preparation of foaming particles is as follows:

[0158]

[0159] The melting point of the foaming particles containing the modified polymer P3 was measured to be 274°C, the melting range was 28°C, and the relaxation time was approximately 36 seconds.

[0160] According to the method described in Example 1, the foaming particles obtained in Example 3 were prepared into a foamed molded body.

[0161] The average cell size of the foamed molded body obtained in Example 3 was measured to be 50 μm, the closed-cell rate was 54.5%, and the density of the foamed molded body was 0.32 g / cm³. 3 The water absorption rate is 0.61%, and the flexural strength is 3.8 MPa. The dielectric constant Dk of the foamed molded body under electromagnetic waves at a frequency of 10 GHz is 1.5, and the dielectric loss Df is 0.0005.

[0162] Example 4

[0163] The difference between Example 4 and Example 1 is that, in preparing the foamed molded body, the product to be foamed obtained by foaming particle molding in Example 1 is impregnated with CO2 for 40 minutes at a foaming temperature of 275°C.

[0164] The average cell size of the foamed molded body obtained in Example 4 was measured to be 5 μm, the closed-cell rate was 75%, and the density of the foamed molded body was 0.7 g / cm³. 3 The water absorption rate is 0.15%, and the flexural strength is 10 MPa. The dielectric constant Dk of the foamed molded body under electromagnetic waves at a frequency of 10 GHz is 1.9, and the dielectric loss Df is 0.0006.

[0165] Example 5

[0166] The difference between Example 5 and Example 2 is that, in the preparation of the foamed molded body, the foaming particle to be foamed product of Example 2 was impregnated with CO2 for 40 minutes at a foaming temperature of 275°C.

[0167] The average cell size of the foamed molded body obtained in Example 5 was measured to be 8 μm, the closed-cell rate was 65%, and the density of the foamed molded body was 0.65 g / cm³. 3 The water absorption rate is 0.35%, and the flexural strength is 7.5 MPa. The dielectric constant Dk of the foamed molded body under electromagnetic waves at a frequency of 10 GHz is 1.8, and the dielectric loss Df is 0.0006.

[0168] Example 6

[0169] The difference between Example 6 and Example 1 is that the weight ratio of sPS, initiator and styrene monomer is 100:0.1:0.2 when preparing the foaming particles.

[0170] The melting point of the foaming particles obtained in Example 6 was measured to be 274°C, the melting range was 27°C, and the relaxation time was approximately 35 seconds.

[0171] According to the method described in Example 1, the foaming particles obtained in Example 6 were prepared into a foamed molded body. The average cell size of the foamed molded body obtained in Example 6 was measured to be 25 μm, the cell closed-cell rate was 59%, and the density of the foamed molded body was 0.35 g / cm³. 3 The water absorption rate is 0.57%, and the flexural strength is 3.4 MPa. The dielectric constant Dk of the foamed molded body under electromagnetic waves at a frequency of 10 GHz is 1.7, and the dielectric loss Df is 0.0007.

[0172] To highlight the beneficial effects of the embodiments of this application, the following comparative examples 1-3 are also provided.

[0173] Comparative Example 1

[0174] Preparation of foaming particles: 100 parts by weight of SPS resin particles, 0.25 parts by weight of antioxidant 1010 and 0.25 parts by weight of antioxidant 168 were added to an aluminum foil bag and stirred evenly. The mixture was then added to a Hacker mixer for melt blending (the speed of the Hacker mixer, the temperature of melt blending and the total time were the same as in Example 1). After melt blending, the sample was taken out from the Hacker mixer and cut into fragments with a length and width of 3mm × 3mm. These fragments are the foaming particles required.

[0175] Preparation of foamed molded body: The foaming particles of Comparative Example 1 were processed into a foamed molded body in accordance with the method described in Example 1. The difference between Comparative Example 1 and Example 1 is that the foaming particles were immersed at a foaming temperature of 265°C for 40 min.

[0176] Among them, the melting point of the foaming particles obtained in Comparative Example 1 was measured to be 271℃, the melting range was 8.6℃, and the relaxation time was approximately 9s.

[0177] The foamed body obtained in Comparative Example 1 was found to have mostly open cells, and the foamed body exhibited delamination (see...). Figure 5 The closed-cell ratio of the foam is as low as 20%. The density of this foamed molded body is 0.44 g / cm³. 3 It has a water absorption rate as high as 13.84% and a bending strength of only 2MPa; the dielectric constant Dk of this foamed molded body is 1.5 and the dielectric loss Df is 0.0004 under electromagnetic waves at a frequency of 10GHz.

[0178] Comparative Example 2 – Set according to Example 1

[0179] The difference between Comparative Example 2 and Example 1 is that, in the preparation of foaming particles, sPS, initiator DCP and styrene monomer were simultaneously added to a Hacker internal mixer for melt blending.

[0180] In Comparative Example 2, the foaming particles had a melting point of 273℃, a melting range of 13.9℃, and a relaxation time of approximately 21 seconds. Furthermore, the foamed body obtained in Comparative Example 2 was found to have mostly open-cell structures, with a closed-cell rate of only 20%, and a density of 0.40 g / cm³. 3 The water absorption rate is 14.60%, and the flexural strength is 1.7 MPa. The dielectric constant Dk of the foamed molded body under electromagnetic waves at a frequency of 10 GHz is 1.6, and the dielectric loss Df is 0.0006.

[0181] Comparative Example 3 – Set according to Example 2

[0182] The difference between Comparative Example 3 and Example 2 is that, in the preparation of foaming particles, sPS, initiator DCP, and pentaerythritol triacrylate (PETA) were simultaneously added to the Hacker internal mixer for melt blending.

[0183] The foaming particles obtained in Comparative Example 3 had a melting point of 273℃, a melting range of 14.5℃, and a relaxation time of approximately 21 seconds. Furthermore, the foamed molded body obtained in Comparative Example 3 was found to have mostly open-cell structures, with a closed-cell rate of only 20%, and a density of 0.47 g / cm³. 3 The water absorption rate is 13.10%, and the flexural strength is 2.2 MPa. The dielectric constant Dk of the foamed molded body under electromagnetic waves at a frequency of 10 GHz is 1.7, and the dielectric loss Df is 0.0006.

[0184] A comparison of the embodiments of this application with Comparative Example 1 reveals that the foaming particles containing the modified polymer of this application have a significantly higher melting range than those of Comparative Example 1, exceeding 15°C and even reaching above 20°C; their relaxation time can be increased to over 30 seconds. This indicates that the foaming particles of this application are particularly suitable for producing foamed molded articles through supercritical foaming, eliminating the need to control the temperature within a particularly narrow range during the foaming process, thus reducing the difficulty of temperature control; and the longer relaxation time of the foaming particles helps to improve the uniformity of the cell structure in the resulting foamed molded article.

[0185] Furthermore, a comparison between Comparative Example 2 and Example 1, and between Comparative Example 3 and Example 2, reveals that when crystalline thermoplastic resin (such as SPS) is melt-blended with initiator and unsaturated monomer simultaneously, rather than first melting and mixing crystalline thermoplastic resin with initiator and then adding unsaturated monomer, the modified polymer with the novel structure of this application is not obtained in the foaming particles obtained in the comparative examples. Therefore, the melting range of the foaming particles is still relatively narrow, and the open cell ratio of the foamed molded body obtained by foaming is relatively high.

Claims

1. A pre-foamed material, characterized in that, The pre-foamed material comprises a modified polymer, wherein the modified polymer has a first structural unit derived from an unsaturated monomer, and the ends of the molecular chains of the modified polymer are capped with a crystalline thermoplastic resin, wherein the crystalline thermoplastic resin comprises one or more of syndiotactic polystyrene, polytetrafluoroethylene, polyvinylidene fluoride, and perfluoroalkoxy vinyl ether polymers, and the pre-foamed material has a melting range of above 15°C and a melting point of above 270°C at a heating rate of 10°C / min based on differential scanning calorimetry.

2. The pre-foamed material as described in claim 1, characterized in that, The unsaturated monomers include one or more of styrene, maleic anhydride, pentaerythritol triacrylate, methacrylate, glycidyl methacrylate, and ethyl acrylate.

3. The pre-foamed material according to any one of claims 1-2, characterized in that, The modified polymer has the structural formula shown in formula (Ⅰ): Equation (I) In formula (Ⅰ), M1 represents the first structural unit derived from an unsaturated monomer, m represents the degree of polymerization of M1, and P1 is independently selected from crystalline thermoplastic resins.

4. The pre-foamed material as described in claim 1, characterized in that, The pre-foamed material is obtained by reacting the following raw materials in parts by weight: 100 parts of crystalline thermoplastic resin matrix, 0.1-5 parts of unsaturated monomer, and 0.1-5 parts of initiator.

5. The pre-foamed material as described in claim 4, characterized in that, The initiator includes one or more of dicumyl peroxide, di(tert-butylperoxide)benzene, 2,5-dimethyl-2,5-bis(tert-butylperoxide)hexane, 2-(tert-butylperoxide)benzene, butanone peroxide, benzoyl peroxide, and dodecyl peroxide.

6. The pre-foamed material as described in claim 1, characterized in that, The pre-foamed material also contains antioxidants.

7. The pre-foamed material as described in claim 6, characterized in that, The mass of the antioxidant is 0.09wt%-1wt% of the mass of the modified polymer.

8. A foamed molded body, characterized in that, The foamed body is obtained by foaming the pre-foamed material as described in any one of claims 1-7.

9. The foamed molded article as described in claim 8, characterized in that, The closed-cell ratio of the foamed molded body is above 50%.

10. The foamed molded article as described in claim 8, characterized in that, The average cell size of the foamed molded body is in the range of 5-100 μm.

11. The foamed molded article according to any one of claims 8-10, characterized in that, The water absorption rate of the foamed molded body after being placed in water for 24 hours at a temperature of 23°C and a relative humidity of 50% is less than 1%.

12. The foamed molded article according to any one of claims 8-10, characterized in that, The density of the foamed molded body is 1 g / cm³. 3 the following.

13. The foamed molded article according to any one of claims 8-10, characterized in that, The dielectric constant of the foamed body measured by the resonant cavity method under electromagnetic waves at a frequency of 10 GHz is below 2.0, and the dielectric loss is below 0.0015.

14. A foamed molded body, characterized in that, The foamed body is obtained by foaming a pre-foamed material; wherein the pre-foamed material includes a modified polymer, the modified polymer has a first structural unit derived from an unsaturated monomer, the ends of the molecular chains of the modified polymer are capped with a crystalline thermoplastic resin, the crystalline thermoplastic resin includes one or more of syndiotactic polystyrene, polytetrafluoroethylene, polyvinylidene fluoride, and perfluoroalkoxy vinyl ether polymers, and the closed-cell ratio of the foamed body is above 50%.

15. The foamed molded article as described in claim 14, characterized in that, The average cell size of the foamed molded body is in the range of 5-100 μm.

16. The foamed molded article according to any one of claims 14-15, characterized in that, The water absorption rate of the foamed molded body after being placed in water for 24 hours at a temperature of 23°C and a relative humidity of 50% is less than 1%.

17. The foamed molded article according to any one of claims 14-15, characterized in that, The density of the foamed molded body is 1 g / cm³. 3 the following.

18. The foamed molded article according to any one of claims 14-15, characterized in that, The dielectric constant of the foamed body measured by the resonant cavity method under electromagnetic waves at a frequency of 10 GHz is below 2.0, and the dielectric loss is below 0.0015.

19. A method for preparing a pre-foamed material, characterized in that, Includes the following steps: First, a crystalline thermoplastic resin is melt-blended with an initiator, and then an unsaturated monomer is added and melt-blended again to obtain a pre-foamed material containing a modified polymer. Under the action of the initiator, the crystalline thermoplastic resin can end-cap the polymer obtained by the polymerization reaction of the unsaturated monomer to obtain the modified polymer. The crystalline thermoplastic resin includes one or more of syndiotactic polystyrene, polytetrafluoroethylene, polyvinylidene fluoride, and perfluoroalkoxy vinyl ether polymers. The pre-foamed material has a melting range of over 15°C and a melting point of over 270°C at a heating rate of 10°C / min using differential scanning calorimetry.

20. The preparation method according to claim 19, characterized in that, Based on 100 parts by weight of the crystalline thermoplastic resin, the initiator is 0.1-5 parts by weight and the unsaturated monomer is 0.1-5 parts by weight.

21. The use of the pre-foamed material as described in any one of claims 1-7, or the foamed molded body as described in any one of claims 9-14, or the foamed molded body as described in any one of claims 14-18, in the preparation of printed circuit boards, cushioning materials, shock-absorbing materials, heat-insulating materials, and sound-absorbing materials.

22. The use of the pre-foamed material as described in any one of claims 1-7 in the preparation of foamed molded articles.

23. A laminate, characterized in that, The laminate includes a dielectric layer sheet and a metal foil on the surface of the dielectric layer sheet. The dielectric layer sheet includes a foamed body, which is obtained by foaming a pre-foamed material. The pre-foamed material includes a modified polymer having a first structural unit derived from an unsaturated monomer, and the ends of the molecular chains of the modified polymer are capped with a crystalline thermoplastic resin. The crystalline thermoplastic resin includes one or more of syndiotactic polystyrene, polytetrafluoroethylene, polyvinylidene fluoride, and perfluoroalkoxy vinyl ether polymers.

24. A laminate, characterized in that, The laminate includes a dielectric layer sheet and a metal foil located on the surface of the dielectric layer sheet, wherein the dielectric layer sheet includes a foamed body as described in any one of claims 8-13, or a foamed body as described in any one of claims 14-18.

25. A printed circuit board, characterized in that, The printed circuit board includes at least one laminate as claimed in claim 23, or at least one laminate as claimed in claim 24.

26. An electronic component, characterized in that, The electronic component includes the printed circuit board of claim 25.

27. An electronic device, characterized in that, The electronic device includes the electronic component of claim 26 or the printed circuit board of claim 25.

28. A modified polymer, characterized in that, The modified polymer has the structural formula shown in formula (Ⅰ): Equation (I) In formula (I), M1 represents the first structural unit derived from an unsaturated monomer, m represents the degree of polymerization of M1, and P1 is independently selected from crystalline thermoplastic resins, including one or more of syndiotactic polystyrene, polytetrafluoroethylene, polyvinylidene fluoride, and perfluoroalkoxy vinyl ether polymers; the modified polymer has a melting range of above 15°C and a melting point of above 270°C at a heating rate of 10°C / min based on differential scanning calorimetry.

29. The use of the modified polymer as described in claim 28 in the preparation of foam materials, molding materials, and adhesives.

30. The use of the modified polymer as described in claim 28 in the preparation of resin compositions.

Citation Information

Patent Citations

  • Method for preparing polylactic acid foaming material subjected to radiation modification by utilizing supercritical fluid CO2

    CN102911392A

  • Crystal polymer foaming particle molding body and preparation method thereof

    CN107556513A

  • Thermoplastic resin porous foaming body as well as preparation method and application thereof

    CN114479224A

  • Method of making thermoplastic foamed articles using supercritical fluid

    US5670102A

  • Grafting of ethylenically unsaturated monomers onto polymers in supercritical carbon dioxide

    WO2009065774A1