An epoxy resin adhesive, its preparation method and application
By adding tannin alcohol and/or its derivatives to epoxy resin adhesives, the cracking and delamination problems at the chip-silicon interface were solved, resulting in higher bond strength and packaging reliability.
Patent Information
- Application Number
- CN202311600111.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-27
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-11-27
AI Technical Summary
Existing underfill adhesives are prone to cracking or delamination at the chip-silicon interface, leading to encapsulation failure and failing to effectively improve adhesive strength.
Adding tannin alcohol and/or its derivatives to epoxy resin adhesives enhances the adhesive's ability to climb along the sides of the chip by utilizing its interaction with the hydroxyl groups on the silicon wafer surface, ensuring the side height after curing and strengthening the adhesion.
It significantly increases the adhesive's climbing height on the chip's side, ensuring the adhesive firmly wraps the chip, improving the chip's bonding strength, and preventing cracking and delamination.
Smart Images

Figure CN117625105B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of bottom-filling adhesives, specifically relating to an epoxy resin adhesive, its preparation method, and its application. Background Technology
[0002] Underfill adhesives are adhesives that flow into the bottom of a chip through capillary action and, upon curing, securely bond the chip. Because underfill adhesives need to secure the chip, it is crucial that there are no cracks or delamination between the adhesive and the chip, especially at the silicon interface between the chip and the adhesive. The silicon interface has the largest contact area with the adhesive; cracking or delamination of the silicon interface layer will lead to severe encapsulation failure, and consequently, more serious functional loss. To ensure that the underfill adhesive does not crack or split after curing at the bottom of the chip, the most important factor is to improve the adhesive strength between the underfill adhesive and the chip. Summary of the Invention
[0003] The present invention aims to provide an epoxy resin adhesive with good bonding strength to chips, its preparation method and application.
[0004] Specifically, the epoxy resin adhesive provided by the present invention contains epoxy resin, tungsten alcohol and / or tungsten alcohol derivatives, toughening resin, curing agent, filler, and optional coupling agent and colorant, wherein the mass ratio of epoxy resin to tungsten alcohol and / or tungsten alcohol derivatives is 100:(0.01-10).
[0005] In a preferred embodiment, the epoxy resin content is 10-30 parts by weight, the tungsten alcohol and / or tungsten alcohol derivative content is 0.01-1 parts by weight, the toughening resin content is 5-15 parts by weight, the curing agent content is 5-20 parts by weight, the filler content is 50-80 parts by weight, the coupling agent content is 0.1-1 parts by weight, and the colorant content is 0.1-1 parts by weight.
[0006] In a preferred embodiment, the epoxy resin is selected from at least one of bisphenol A diglycidyl ether, bisphenol F diglycidyl ether, bisphenol S diglycidyl ether, o-hydroxymethyl bisphenol A diglycidyl ether, dihydroxymethyl bisphenol A diglycidyl ether, tetrabromobisphenol A diglycidyl ether, resorcinol diglycidyl ether, pyrogallol triglycidyl ether, and pentaerythritol diglycidyl ether, preferably a mixture of bisphenol A diglycidyl ether and bisphenol F diglycidyl ether.
[0007] In a preferred embodiment, the zentonol and / or zentonol derivatives are selected from at least one of zentonol, 2-bromozentonolone, 9-(4-methoxyphenyl)zenton-9-ol and 9-phenylbenzene-9-ol.
[0008] In a preferred embodiment, the toughening resin is selected from at least one of polyurethane, cashew nut shell liquid modified phenolic resin, unsaturated polyester resin, epoxy resin active toughening agent and SBS thermoplastic elastomer.
[0009] In a preferred embodiment, the curing agent is selected from at least one of 3-dimethylaminopropylamine, 3-diethylaminopropylamine, isophorone diamine, trimethylhexanediamine, m-phenylenediamine, dimethyldiaminodiphenylmethane, diaminodiphenyl sulfone, diaminodiphenylmethane, diethyldiaminodiphenylmethane, and diaminodiphenyl ether.
[0010] In a preferred embodiment, the filler is selected from at least one of calcium carbonate, dolomite powder, calcite, quartz powder, kaolin powder, calcined kaolin powder, talc powder, mica powder, feldspar powder, wollastonite powder, silica micro powder, sepiolite powder, and glass powder, preferably silica micro powder, and the average particle size is preferably 0.1-10 μm.
[0011] In a preferred embodiment, the coupling agent is selected from at least one of 3-epoxypropoxypropyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, and 8-epoxypropoxyoctyltrimethoxysilane.
[0012] In a preferred embodiment, the pigment is carbon black.
[0013] The method for preparing epoxy resin adhesive provided by the present invention includes uniformly mixing epoxy resin, thioglycol and / or thioglycol derivatives, toughening resin, curing agent, filler, and optionally coupling agent and colorant.
[0014] Furthermore, the present invention also provides the application of the epoxy resin adhesive as an underfill adhesive.
[0015] The key to this invention lies in adding thiocyanate and / or thiocyanate derivatives to the epoxy resin adhesive. Since silicon wafers themselves contain a large number of hydroxyl groups, the unique hydroxyl groups and ether bonds in thiocyanate will strongly interact with the hydroxyl groups on the surface of the silicon wafer, which can significantly improve the climbing ability of the adhesive on the side of the chip, so that the climbing height of the adhesive on the side of the chip is maintained above 225μm. This ensures the side height after the adhesive cures, firmly wrapping the chip and thus improving the chip adhesion. Attached Figure Description
[0016] Figure 1 This is a diagram showing the climbing effect of the epoxy resin adhesive obtained in Example 1 on the silicon wafer surface;
[0017] Figure 2This is a diagram showing the climbing effect of the epoxy resin adhesive obtained in Example 2 on the silicon wafer surface;
[0018] Figure 3 This is a diagram showing the climbing effect of the epoxy resin adhesive obtained in Example 3 on the silicon wafer surface;
[0019] Figure 4 This is a diagram showing the climbing effect of the epoxy resin adhesive obtained in Example 4 on the silicon wafer surface;
[0020] Figure 5 This is a diagram showing the climbing effect of the epoxy resin adhesive obtained in Example 5 on the silicon wafer surface;
[0021] Figure 6 This is a diagram showing the climbing effect of the epoxy resin adhesive obtained in Comparative Example 1 on the silicon wafer surface. Detailed Implementation
[0022] The epoxy resin adhesive provided by this invention contains epoxy resin, thiocyanate and / or thiocyanate derivatives, toughening resin, curing agent, and filler, and preferably also contains coupling agent and colorant. The mass ratio of epoxy resin to thiocyanate and / or thiocyanate derivatives is 100:(0.01-10), such as 100:0.01, 100:0.05, 100:0.1, 100:0.2, 100:0.3, 100:0.4, 100:0.5, 100:0.6, 100:0.7, 100:0.8, 100:0.9, 100:1, 100:2, 100:3, 100:4, 100:5, 100:6, 100:7, 100:8, 100:9, 100:10, or any value between them. When the mass ratio of methyl ethyl ether and / or methyl ethyl ether derivatives to epoxy resin is less than 0.01:100, the adhesive's creep height on the chip side is low, which is detrimental to improving the bonding strength of the epoxy resin adhesive on the chip. When the mass ratio of methyl ethyl ether and / or methyl ethyl ether derivatives to epoxy resin is greater than 10:100, there is a risk of overflow at other interfaces. It should be noted that when the epoxy resin adhesive contains only methyl ethyl ether or methyl ethyl ether derivatives, the content of methyl ethyl ether and / or methyl ethyl ether derivatives refers to the content of methyl ethyl ether or methyl ethyl ether derivatives; when the epoxy resin adhesive contains both methyl ethyl ether and methyl ethyl ether derivatives, the content of methyl ethyl ether and / or methyl ethyl ether derivatives refers to the sum of the contents of methyl ethyl ether and methyl ethyl ether derivatives.
[0023] In a preferred embodiment, the mass ratio of epoxy resin, tungsten alcohol and / or tungsten alcohol derivatives, toughening resin, curing agent, filler, coupling agent and pigment is preferably (10-30):(0.01-1):(5-15):(5-20):(50-80):(0.1-1):(0.1-1). At this ratio, the components can achieve a very perfect match, which can obtain a higher adhesive climbing height on the side of the chip and is more conducive to improving the adhesion between the chip and the chip. Specifically, the content of the epoxy resin is preferably 10-30 parts by weight, such as 10, 12, 14, 16, 18, 20, 22, 25, 28, 30 parts by weight or any value between them; the content of the tonol and / or tonol derivative is preferably 0.01-1 parts by weight, such as 0.01, 0.02, 0.04, 0.06, 0.08, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1 parts by weight or any value between them; the content of the toughening resin is preferably 5-15 parts by weight. The content of the curing agent is preferably 5-20 parts by weight, such as 5, 8, 10, 12, 15, 18, 20 parts by weight, or any value between them; the content of the filler is preferably 50-80 parts by weight, such as 50, 55, 60, 65, 70, 75, 80 parts by weight, or any value between them; the content of the coupling agent and the colorant is preferably each independently 0.1-1 parts by weight, such as 0.1, 0.2, 0.4, 0.6, 0.8, 1 parts by weight, or any value between them.
[0024] In this invention, the epoxy resin may be an aliphatic epoxy resin having two or more epoxy groups, an aromatic epoxy resin having two or more epoxy groups, or a mixture of both.
[0025] The aliphatic epoxy resin can be at least one of binary epoxy resins, ternary epoxy resins, etc. Specific examples of the binary epoxy resin include, but are not limited to, at least one of: (poly)ethylene glycol diglycidyl ether, (poly)propylene glycol diglycidyl ether, butanediol diglycidyl ether, neopentyl glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, trimethylolpropane diglycidyl ether, polytetramethylene ether glycol diglycidyl ether, glycerol diglycidyl ether, neopentyl glycol diglycidyl ether, cyclohexane-type diglycidyl ether, and dicyclopentadiene-type diglycidyl ether. Specific examples of the ternary epoxy resin include, but are not limited to, trimethylolpropane triglycidyl ether and / or glycerol triglycidyl ether. Furthermore, cyclohexane-type diglycidyl ether is particularly preferred as a cyclohexane-diethanol diglycidyl ether. The aliphatic epoxy resin can be at least one of alicyclic epoxy resin, glycidylamine type epoxy resin, hydantoin type epoxy resin, or epoxy resin with a siloxane backbone. Specific examples of the alicyclic epoxy resin include, but are not limited to, vinyl(3,4-cyclohexene)dioxide and / or 2-(3,4-epoxycyclohexyl)-5,1-spiro-(3,4-epoxycyclohexyl)m-dioxane. The glycidylamine type epoxy resin can be, for example, tetraglycidylbis(aminomethyl)cyclohexane. The hydantoin type epoxy resin can be, for example, 1,3-diglycidyl-5-methyl-5-ethylhydantoin. The epoxy resin with a siloxane backbone can be, for example, 1,3-bis(3-epoxypropoxypropyl)-1,1,3,3-tetramethyldisiloxane. Furthermore, the epoxy equivalent of the aliphatic epoxy resin is preferably 90-450 g / eq, such as 90, 100, 120, 150, 180, 200, 220, 250, 280, 300, 320, 350, 380, 400, 420, 450 g / eq.
[0026] The aromatic epoxy resin can be any existing epoxy resin containing two epoxy groups and an aromatic ring structure. Specific examples include, but are not limited to, at least one of the following: bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, o-hydroxymethyl bisphenol A diglycidyl ether, dihydroxymethyl bisphenol A diglycidyl ether, tetrabromobisphenol A diglycidyl ether, resorcinol diglycidyl ether, pyrogallol triglycidyl ether, and pentaerythritol diglycidyl ether. Preferably, it is a bisphenol A type epoxy resin and / or a bisphenol F type epoxy resin, more preferably a mixture of bisphenol A type epoxy resin and bisphenol F type epoxy resin. When the epoxy resin is a mixture of bisphenol A type epoxy resin and bisphenol F type epoxy resin, the problem of excessively high viscosity can be alleviated by the bisphenol A type epoxy resin, and the modulus can be increased by the bisphenol F type epoxy resin, thereby enhancing the protection of the solder ball. When the epoxy resin is a mixture of bisphenol A type epoxy resin and bisphenol F type epoxy resin, the mass ratio of bisphenol A type epoxy resin to bisphenol F type epoxy resin is preferably 1:(1-5), such as 1:1, 1:2, 1:3, 1:4, 1:5 or any value between them. Furthermore, the epoxy equivalent of the aromatic epoxy resin is preferably 80-600 g / eq, more preferably 90-450 g / eq, such as 90, 100, 120, 150, 180, 200, 220, 250, 280, 300, 320, 350, 380, 400, 420, 450 g / eq.
[0027] In this invention, the tannin derivative preferably has the structure shown in formula (1):
[0028]
[0029] R1 and R2 are each independently H, C1-C5 substituted or unsubstituted alkyl groups or halogens; R3 is -OH and R4 is H, C1-C5 substituted or unsubstituted alkyl groups or C6-C 20 The substituted or unsubstituted aryl group; or R3 is O and R4 is absent. The substituent group can be O or S. Examples of the substituted or unsubstituted alkyl groups in C1-C5 are methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl, tert-butyl, n-pentyl, isopentyl, tert-pentyl, or neopentyl. The C6-C... 20 Examples of substituted or unsubstituted aryl groups can be phenyl, benzyl, tolyl, or methoxyphenyl. For higher adhesive strength, preferably, the zentonol derivative is selected from at least one of 2-bromozentonone, 9-(4-methoxyphenyl)zenton-9-ol, and 9-phenylstyrene-9-ol.
[0030] In this invention, specific examples of the toughening resin include, but are not limited to, at least one of: polyurethane, cashew nutshell liquid-modified phenolic resin, unsaturated polyester resin, epoxy resin active toughening agent, and SBS thermoplastic elastomer. The unsaturated polyester resin may be at least one of 182 unsaturated polyester resin, 196 unsaturated polyester resin, etc.
[0031] In this invention, specific examples of the curing agent include, but are not limited to, at least one of the following: 3-dimethylaminopropylamine, 3-diethylaminopropylamine, isophorone diamine, trimethylhexanediamine, m-phenylenediamine, dimethyldiaminodiphenylmethane, diaminodiphenyl sulfone, diaminodiphenylmethane, diethyldiaminodiphenylmethane, and diaminodiphenyl ether, preferably m-phenylenediamine.
[0032] In this invention, specific examples of the filler include, but are not limited to, at least one of the following: calcium carbonate, dolomite powder, calcite, quartz powder, kaolin powder, calcined kaolin powder, talc powder, mica powder, feldspar powder, wollastonite powder, silica micron powder, sepiolite powder, and glass powder, preferably silica micron powder. The average particle size of the filler is preferably controlled within the range of 0.1-10 μm, such as 0.1 μm, 1 μm, 2 μm, 4 μm, 6 μm, 8 μm, 10 μm, or any value between these values. Furthermore, the filler is preferably surface-treated with a silane coupling agent before use. The silane coupling agent can be any of the following: epoxy, amino, vinyl, methacrylic, acrylic, mercapto, etc., preferably selected from at least one of 3-epoxypropoxypropyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-methacryloyloxypropyltrimethoxysilane, and 8-epoxypropoxyoctyltrimethoxysilane.
[0033] In this invention, the epoxy resin adhesive also contains color powder to impart the desired color. The color powder can be black, specifically carbon black.
[0034] In this invention, the epoxy resin adhesive may also contain at least one of the following additives: flame retardant, diluent, antioxidant, adhesion promoter, defoamer, leveling agent, thixotropic agent, homogenizer, and ion scavenger. The type and amount of each additive can be conventionally chosen in the art. For example, relative to 100 parts by weight of epoxy resin, the content of the additive can be 0.1-15 parts by weight, for example, 0.1, 2, 5, 8, 10, 12, or 15 parts by weight.
[0035] The method for preparing epoxy resin adhesive provided by the present invention includes uniformly mixing epoxy resin, thioglycol and / or thioglycol derivatives, toughening resin, curing agent, filler, and optionally coupling agent and colorant.
[0036] This invention does not impose any particular limitation on the method of uniformly mixing the above materials. The materials can be added simultaneously and mixed uniformly, or some materials can be mixed uniformly in any order before adding others and mixing uniformly. In a preferred embodiment, the mixing method includes uniformly mixing epoxy resin, thiocyanate and / or thiocyanate derivatives, toughening resin, curing agent, and optionally silane coupling agent and colorant; adding filler to the resulting premix and mixing uniformly; passing the resulting mixture through a three-roll mill 1-5 times; then transferring it to a mixing tank and mixing; opening the mixing tank; scraping the tank walls every 10-20 minutes; after mixing is complete, applying vacuum for degassing while simultaneously stirring; discharging the material after vacuum degassing for 10-20 minutes; and finally sealing and storing the resulting material in a refrigerator at -40°C or below.
[0037] The present invention also provides the application of the epoxy resin adhesive as an underfill adhesive.
[0038] The present invention will be described in detail below through embodiments.
[0039] Example 1
[0040] (1) The raw materials are as follows:
[0041] Bisphenol F diglycidyl ether, 24 parts by weight;
[0042] Bisphenol A diglycidyl ether, 5 parts by weight;
[0043] SBS thermoplastic elastomer, 10 parts by weight;
[0044] m-Phenylenediamine, 9 parts by weight;
[0045] 50 parts by weight of silica micro powder (average particle size of 5.2 μm, the same below);
[0046] Carbon black, 1 part by weight;
[0047] 1 part by weight of ...
[0048] (2) Preparation method:
[0049] Bisphenol F diglycidyl ether, bisphenol A diglycidyl ether, SBS thermoplastic elastomer, m-phenylenediamine, carbon black, and thiocyanate were mixed evenly in a container to obtain a premix. Silica micro powder was added to the premix and mixed evenly. The resulting mixture was then passed through a three-roll mill twice and then transferred to a dual planetary hybrid stirring tank and stirred for 30 minutes. The walls of the tank were scraped during the 15-minute stirring time. After mixing, the mixture was subjected to vacuum degassing treatment and then discharged to obtain epoxy resin adhesive.
[0050] Example 2
[0051] (1) The raw materials are as follows:
[0052] Bisphenol F diglycidyl ether, 24 parts by weight;
[0053] Bisphenol A diglycidyl ether, 5 parts by weight;
[0054] SBS thermoplastic elastomer, 10 parts by weight;
[0055] m-Phenylenediamine, 9 parts by weight;
[0056] 50 parts by weight of silica micro powder;
[0057] Carbon black, 1 part by weight;
[0058] 9-Phenylen-8-ol, 1 part by weight.
[0059] (2) Preparation method:
[0060] Bisphenol F diglycidyl ether, bisphenol A diglycidyl ether, SBS thermoplastic elastomer, m-phenylenediamine, carbon black, and 9-phenylbenzene-8-ol were mixed evenly in a container to obtain a premix. Silica powder was added to the premix and mixed evenly. The resulting mixture was then passed through a three-roll mill twice and transferred to a dual planetary hybrid stirring tank and stirred for 30 minutes. The walls were scraped during the 15-minute stirring time. After mixing, the mixture was subjected to vacuum degassing treatment and then discharged to obtain epoxy resin adhesive.
[0061] Example 3
[0062] (1) The raw materials are as follows:
[0063] Bisphenol F diglycidyl ether, 24 parts by weight;
[0064] Bisphenol A diglycidyl ether, 5 parts by weight;
[0065] Polyurethane, 10 parts by weight;
[0066] m-Phenylenediamine, 9 parts by weight;
[0067] 50 parts by weight of silica micro powder;
[0068] Carbon black, 1 part by weight;
[0069] 9-(4-methoxyphenyl)zenton-9-ol, 1 part by mass.
[0070] (2) Preparation method:
[0071] Bisphenol F diglycidyl ether, bisphenol A diglycidyl ether, polyurethane, m-phenylenediamine, carbon black, and 9-(4-methoxyphenyl)janton-9-ol were mixed evenly in a container to obtain a premix. Silica powder was added to the premix and mixed evenly. The resulting mixture was then passed through a three-roll mill twice and transferred to a dual planetary hybrid stirring tank and stirred for 30 minutes. The walls were scraped during the 15-minute stirring time. After mixing, the mixture was subjected to vacuum degassing and then discharged to obtain epoxy resin adhesive.
[0072] Example 4
[0073] (1) The raw materials are as follows:
[0074] Bisphenol F diglycidyl ether, 20 parts by weight;
[0075] CMP-410 epoxy resin active toughening agent, 10 parts by weight;
[0076] 3-Diethylaminopropylamine, 20 parts by weight;
[0077] Calcium carbonate micro powder (average particle size 0.82 μm), 80 parts by weight;
[0078] Carbon black, 0.1 parts by weight;
[0079] 0.01 parts by weight of methyl methacrylate (McClene).
[0080] (2) Preparation method:
[0081] Bisphenol F diglycidyl ether, CMP-410 epoxy resin active toughening agent, 3-diethylaminopropylamine, carbon black, and thiocyanate were mixed evenly in a container to obtain a premix. Calcium carbonate micro powder was added to the premix and mixed evenly. The resulting mixture was then passed through a three-roll mill twice and transferred to a dual planetary hybrid stirring tank and stirred for 30 minutes. The wall was scraped during the 15-minute stirring time. After mixing, the mixture was subjected to vacuum degassing treatment and then discharged to obtain epoxy resin adhesive.
[0082] Example 5
[0083] (1) The raw materials are as follows:
[0084] Bisphenol A diglycidyl ether, 10 parts by weight;
[0085] 196 unsaturated polyester resin, 5 parts by weight;
[0086] Isophorone diamine, 5 parts by weight;
[0087] Sepiolite powder (average particle size 0.63 μm), 60 parts by weight;
[0088] Carbon black, 0.5 parts by weight;
[0089] 2-Bromo-tocopherol, 0.5 parts by weight.
[0090] (2) Preparation method:
[0091] Bisphenol A diglycidyl ether, 196 unsaturated polyester resin, isophorone diamine, carbon black, and 2-bromo-zantonone were mixed evenly in a container to obtain a premix. Sepiol powder was added to the premix and mixed evenly. The resulting mixture was then passed through a three-roll mill twice and then transferred to a dual planetary hybrid stirring tank and stirred for 30 minutes. The walls were scraped during the 15-minute stirring time. After the mixing was completed, the mixture was subjected to vacuum degassing treatment and then discharged to obtain epoxy resin adhesive.
[0092] Comparative Example 1
[0093] An epoxy resin adhesive was prepared according to the method of Example 1, except that tungsten alcohol was not used, and the other conditions were the same as in Example 1, to obtain a reference epoxy resin adhesive.
[0094] Test case
[0095] (1) Glue Climbing Height: The epoxy resin adhesives obtained in the above embodiments and the reference epoxy resin adhesive obtained in the comparative example were filled into the gap between the chip and the substrate (the gap of the sample was fixed by solder balls, and the gap width was 150μm). Then, the sample and the adhesive were cured together at 165℃ / 120min. After curing, the sample was polished and then placed under a Keyence 3D contour display at room temperature for height measurement and climbing height data recording. The results are shown in Table 1. Among them, the glue climbing results corresponding to Examples 1-5 and Comparative Example 1 are shown in Table 1. Figures 1-6 ,from Figure 1-6 As can be clearly seen from Table 1, the adhesive creep height of Examples 1-5 is significantly higher than that of Comparative Example 1, demonstrating that the interface interaction between Examples 1-5 and the chip is significantly better than that of Comparative Example 1, resulting in better wetting performance.
[0096] (2) Viscosity: The viscosity of the epoxy resin adhesives obtained in the above embodiments and the reference epoxy resin adhesives obtained in the comparative example when they were freshly prepared and after standing for 24 hours were tested using a BROOKFIELD viscometer. Specifically, the viscosity data at a speed of 5 rpm was measured after rotating a 29# rotor for 30 minutes. The results are shown in Table 1.
[0097] (3) Adhesive strength: The epoxy resin adhesives obtained in the above embodiments and the reference epoxy resin adhesives obtained in the comparative examples were coated on silicon wafers, and then covered and pressed onto FR5 substrates to make test samples. The bonding area was 2mm × 2mm, and the adhesive layer thickness was 50um. The samples were cured at 165℃ for 120min. The cured samples were then pushed sideways using a Dage 4000. The test was conducted at room temperature (30℃), and the measured force value was recorded as room temperature adhesive strength (MPa). The test was conducted at high temperature (260℃), and the measured force value was recorded as high temperature adhesive strength (MPa). The results are shown in Table 1.
[0098] Table 1
[0099]
[0100] Although embodiments of the present invention have been shown and described above, it is understood that the above embodiments are exemplary and should not be construed as limiting the present invention. Those skilled in the art can make changes, modifications, substitutions and variations to the above embodiments within the scope of the present invention without departing from the principles and spirit of the present invention.
Claims
1. An epoxy resin adhesive, characterized in that, The epoxy resin adhesive comprises epoxy resin, thionol and / or thionol derivatives, toughening resin, curing agent, filler, and optionally coupling agent and colorant, wherein the mass ratio of epoxy resin to thionol and / or thionol derivatives is 100:(0.01-10); the thionol and / or thionol derivatives are selected from at least one of thionol, 2-bromothionolone, 9-(4-methoxyphenyl)thionol-9-ol, and 9-phenylstyrene-9-ol.
2. The epoxy resin adhesive according to claim 1, characterized in that, The epoxy resin content is 10-30 parts by weight, the tungsten alcohol and / or tungsten alcohol derivative content is 0.01-1 parts by weight, the toughening resin content is 5-15 parts by weight, the curing agent content is 5-20 parts by weight, the filler content is 50-80 parts by weight, the coupling agent content is 0.1-1 parts by weight, and the colorant content is 0.1-1 parts by weight.
3. The epoxy resin adhesive according to claim 1, characterized in that, The epoxy resin is selected from at least one of bisphenol A diglycidyl ether, bisphenol F diglycidyl ether, bisphenol S diglycidyl ether, o-hydroxymethyl bisphenol A diglycidyl ether, dihydroxymethyl bisphenol A diglycidyl ether, tetrabromobisphenol A diglycidyl ether, resorcinol diglycidyl ether, pyrogallol triglycidyl ether, and pentaerythritol diglycidyl ether.
4. The epoxy resin adhesive according to claim 3, characterized in that, The epoxy resin is a mixture of bisphenol A bisglycidyl ether and bisphenol F bisglycidyl ether.
5. The epoxy resin adhesive according to claim 1, characterized in that, The toughening resin is selected from at least one of polyurethane, cashew nut shell liquid modified phenolic resin, unsaturated polyester resin, epoxy resin active toughening agent and SBS thermoplastic elastomer.
6. The epoxy resin adhesive according to claim 1, characterized in that, The curing agent is selected from at least one of 3-dimethylaminopropylamine, 3-diethylaminopropylamine, isophorone diamine, trimethylhexanediamine, m-phenylenediamine, dimethyldiaminodiphenylmethane, diaminodiphenyl sulfone, diaminodiphenylmethane, diethyldiaminodiphenylmethane, and diaminodiphenyl ether.
7. The epoxy resin adhesive according to claim 1, characterized in that, The filler is selected from at least one of calcium carbonate, dolomite powder, calcite, quartz powder, kaolin powder, calcined kaolin powder, talc powder, mica powder, feldspar powder, wollastonite powder, silica micro powder, sepiolite powder, and glass powder.
8. The epoxy resin adhesive according to claim 7, characterized in that, The filler is silica micro powder.
9. The epoxy resin adhesive according to claim 8, characterized in that, The average particle size of the silica micropowder is 0.1-10 μm.
10. The epoxy resin adhesive according to claim 1, characterized in that, The coupling agent is selected from at least one of 3-epoxypropoxypropyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-methacryloyloxypropyltrimethoxysilane, and 8-epoxypropoxyoctyltrimethoxysilane; the pigment is carbon black.
11. A method for preparing the epoxy resin adhesive according to any one of claims 1-10, characterized in that, The method involves uniformly mixing epoxy resin, tungsten alcohol and / or tungsten alcohol derivatives, toughening resin, curing agent, filler, and optionally coupling agent and colorant.
12. The use of the epoxy resin adhesive according to any one of claims 1-10 as an underfill adhesive.
Citation Information
Patent Citations
Curable, partially advanced epoxy resins
US4594291A