A preparation method and application of carbon paper for fuel cell
The carbon paper for fuel cells is prepared by combining modified carbon fiber and graphite, which solves the problems of insufficient air permeability and electrical conductivity of existing carbon paper and realizes fuel cell materials with high air permeability, low resistivity and high tensile strength.
Patent Information
- Application Number
- CN202311814026.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-27
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-12-27
AI Technical Summary
Existing carbon paper for fuel cells has unstable air permeability, tensile strength and vertical conductive properties that are not excellent enough.
Using a combination of modified carbon fiber and modified graphite, carbon fiber base paper is prepared through steps such as ultrasound, stirring and hot pressing, and carbonized under a protective atmosphere of argon and nitrogen to form carbon for fuel cells with excellent breathability, electrical conductivity and mechanical strength. Paper.
The air permeability, electrical conductivity and mechanical strength of carbon paper for fuel cells are improved. The vertical resistivity is low, the air permeability is high, the tensile strength is significantly improved, and the stability and performance are excellent.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of fuel cells, and in particular to a preparation method of carbon paper for fuel cells and application thereof. Background Art
[0002] Fuel cell power generation technology is the fourth type of power generation technology after hydropower, thermal power and nuclear power generation, and is considered to be the preferred clean and efficient power generation technology in the 21st century. Among them, proton exchange membrane fuel cell is the most promising type of fuel cell. It has the advantages of small volume and weight, high energy density, fast startup speed, safe and reliable operation, and has attracted much attention. As one of the key components of proton exchange membrane fuel cells, the gas diffusion layer not only plays the role of supporting the catalyst layer and stabilizing the electrode structure, but also improves the gas channel, proton channel, electron channel and drainage channel for the electrode reaction, and its performance has a direct impact on the battery performance of the fuel cell. The gas diffusion layer is usually composed of a base layer and a microporous layer, and the base layer material mainly includes carbon fiber paper, carbon fiber woven cloth, non-woven fabric or carbon black paper, wherein carbon fiber paper is widely recognized for its excellent performance. CN115341407A discloses carbon fiber paper for fuel cell gas diffusion layer and its preparation method and application, but the air permeability of the carbon fiber paper for fuel cell gas diffusion layer prepared by it is unstable, and the tensile strength and vertical conductivity are not excellent enough.
[0003] In summary, after extensive searching by the applicant, it is found in the art that at least there is a problem in that the carbon paper for fuel cells prepared by the existing method for preparing carbon paper for fuel cells has unstable air permeability, and its tensile strength and vertical conductivity are not good enough. Therefore, it is necessary to develop or improve a method for preparing carbon paper for fuel cells and its application. Summary of the invention
[0004] Based on this, in order to solve the problems that the carbon paper for fuel cells prepared by the existing preparation method of carbon paper for fuel cells has unstable air permeability, and the tensile strength and vertical conductivity are not good enough, the present invention provides a preparation method for carbon paper for fuel cells and its application, and the specific technical scheme is as follows:
[0005] A method for preparing carbon paper for a fuel cell comprises the following steps:
[0006] Preparation of carbon fiber base paper: adding modified carbon fiber to water, ultrasonicating at a frequency of 50-70KHz for 1-1.5h, then adding polysorbate and polyethylene oxide, stirring at a speed of 550-650r / min for 5-7h, then adding polyvinyl alcohol, continuing to stir at a speed of 550-650r / min for 3.0-3.6h, then wet forming, drying the formed paper at 80-90°C for 50-60min, and then hot pressing to obtain the carbon fiber base paper;
[0007] Impregnation and carbonization: the carbon fiber base paper is impregnated in the impregnation liquid for 50-60 minutes, then dried at 95-105° C. under a nitrogen protective atmosphere, then heated to 250-270° C. under an argon protective atmosphere for 2-3 hours for curing, and then heated to 1800-1900° C. under an argon protective atmosphere for carbonization to obtain the carbon paper for fuel cells;
[0008] The impregnation solution includes modified graphite, conductive material, dispersant and solvent;
[0009] The raw materials for preparing the modified carbon fiber include carbon fiber, urea and melamine;
[0010] The raw materials for preparing the modified graphite include nitric acid, hydrazine hydrate and ethylenediamine;
[0011] The mass ratio of the modified carbon fiber, polysorbate, polyethylene oxide and polyvinyl alcohol is 13-17:3-5:10-15:10-15;
[0012] The length of the carbon fiber is 0.8-1.2 mm.
[0013] Furthermore, the method for preparing the modified carbon fiber comprises the following steps:
[0014] Preparation of modified carbon fiber: add carbon fiber to acetone, reflux for 2-3 hours, then wash with ethanol, and then dry at 60-70°C. After drying, add water, ultrasonicate at a frequency of 50-70KHz for 0.6-0.8 hours, then add urea, stir at a speed of 380-420r / min for 2-3 hours, then add melamine-ethylene glycol mixture, and then stir at a speed of 500-560r / min for 3.5-3.9 hours, then filter, heat the solid to 210-230°C in a nitrogen atmosphere for activation, and obtain the modified carbon fiber.
[0015] Furthermore, the preparation method of the modified graphite comprises the following steps:
[0016] Preparation of modified graphite: adding graphite to an ethanol solution, ultrasonicating at a frequency of 50-70 KHz for 5-6 hours, then adding an aqueous yttrium nitrate solution, stirring evenly, then ultrasonicating at a frequency of 50-70 KHz for 1.2-1.8 hours, continuing to stir at a speed of 250-350 r / min, then adding hydrazine hydrate, stirring evenly and adding ethylenediamine, then heating to 50-56° C., reacting for 2.2-2.8 hours, cooling and separating by centrifuge, then washing the precipitate with pure water until yttrium is not detected in the washing liquid, then washing three times with ethanol, and then placing in an oven, drying at 90-100° C. for 6-8 hours to obtain the modified graphite.
[0017] Furthermore, the mass ratio of the carbon fiber, urea and melamine is 5-7:0.8-1.2:0.8-1.2.
[0018] Furthermore, the hot pressing conditions are a temperature of 145-152° C. and a pressure of 5-7 MPa.
[0019] Furthermore, the conductive material includes at least one of carbon fiber, carbon nanotube, acetylene black, mesoporous carbon, conductive carbon black, carbon aerogel, graphite and graphene.
[0020] Furthermore, the dispersant includes at least one of polytetrafluoroethylene, polychlorotrifluoroethylene, vinylidene fluoride-chlorotrifluoroethylene copolymer, copolymer of tetrafluoroethylene and hexafluoroethylene, polyvinyl fluoride, polyvinylidene fluoride, ethylene-chlorotrifluoroethylene copolymer, tetrafluoroethylene-hexafluoropropylene copolymer, ethylene-tetrafluoroethylene copolymer and tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer.
[0021] Furthermore, the solvent includes at least one of water, ethanol, ethylene glycol, acetone, glycerol, N,N-dimethylformamide, dimethyl sulfoxide, dimethylacetamide and N-methylpyrrolidone.
[0022] Furthermore, the mass ratio of the graphite to nitric acid is 8-10:1, and the mass ratio of hydrazine hydrate to ethylenediamine is 1:0.8-1.2.
[0023] The present technical solution also provides a fuel cell, which includes a proton exchange membrane, a gas diffusion layer, a catalyst layer and a bipolar plate, wherein the gas diffusion layer is carbon paper for fuel cells prepared by the preparation method provided by the above technical solution.
[0024] The carbon paper for fuel cells prepared by the above technical solution uses carbon fibers modified with urea and melamine and graphite modified with nitric acid, hydrazine hydrate and ethylenediamine at the same time during the preparation process, so the obtained carbon paper for fuel cells has stable and excellent air permeability, electrical conductivity and mechanical strength. Specifically, since the modified carbon fibers are modified with linear urea and cyclic melamine at the same time, after activation, the modified carbon fibers are doped with nitrogen elements, and some nitrogen-containing groups can be arranged in a three-dimensional and orderly manner on the surface of the modified carbon fibers. Further, the modified carbon fibers are impregnated with an impregnation solution of modified graphite, and the embedded nitrogen-containing elements and the nitrogen-containing groups on the surface interact with the nitrogen-containing groups of the modified graphite, so that the modified graphite is evenly and orderly arranged on the surface of the modified carbon fibers, and can form an efficient electron channel in the longitudinal direction. Therefore, the air permeability, electrical conductivity and mechanical strength of the carbon paper for fuel cells prepared by the technical solution are stable and excellent. DETAILED DESCRIPTION
[0025] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with its embodiments. It should be understood that the specific implementation methods described herein are only used to explain the present invention and do not limit the protection scope of the present invention.
[0026] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0027] A method for preparing carbon paper for a fuel cell in one embodiment of the present invention comprises the following steps:
[0028] Preparation of carbon fiber base paper: adding modified carbon fiber to water by mass, ultrasonicating at a frequency of 50-70KHz for 1-1.5h, then adding polysorbate and polyethylene oxide, stirring at a speed of 550-650r / min for 5-7h, then adding polyvinyl alcohol, continuing to stir at a speed of 550-650r / min for 3.0-3.6h, then wet forming, drying the formed paper at 80-90°C for 50-60min, and then hot pressing to obtain the carbon fiber base paper;
[0029] Impregnation and carbonization: the carbon fiber base paper is impregnated in the impregnation liquid for 50-60 minutes, then dried at 95-105° C. under a nitrogen protective atmosphere, then heated to 250-270° C. under an argon protective atmosphere for 2-3 hours for curing, and then heated to 1800-1900° C. under an argon protective atmosphere for carbonization to obtain the carbon paper for fuel cells;
[0030] The impregnation solution includes modified graphite, conductive material, dispersant and solvent;
[0031] The raw materials for preparing the modified carbon fiber include carbon fiber, urea and melamine;
[0032] The raw materials for preparing the modified graphite include nitric acid, hydrazine hydrate and ethylenediamine;
[0033] The mass ratio of the modified carbon fiber, polysorbate, polyethylene oxide and polyvinyl alcohol is 13-17:3-5:10-15:10-15;
[0034] The length of the carbon fiber is 0.8-1.2 mm.
[0035] In one embodiment, the method for preparing the modified carbon fiber comprises the following steps:
[0036] Preparation of modified carbon fiber: add carbon fiber to acetone, reflux for 2-3 hours, then wash with ethanol, and then dry at 60-70°C. After drying, add water, ultrasonicate at a frequency of 50-70KHz for 0.6-0.8 hours, then add urea, stir at a speed of 380-420r / min for 2-3 hours, then add melamine-ethylene glycol mixture, and then stir at a speed of 500-560r / min for 3.5-3.9 hours, then filter, heat the solid to 210-230°C in a nitrogen atmosphere for activation, and obtain the modified carbon fiber.
[0037] In one embodiment, the method for preparing the modified graphite comprises the following steps:
[0038] Preparation of modified graphite: adding graphite to an ethanol solution, ultrasonicating at a frequency of 50-70 KHz for 5-6 hours, then adding an aqueous yttrium nitrate solution, stirring evenly, then ultrasonicating at a frequency of 50-70 KHz for 1.2-1.8 hours, continuing to stir at a speed of 250-350 r / min, then adding hydrazine hydrate, stirring evenly and adding ethylenediamine, then heating to 50-56° C., reacting for 2.2-2.8 hours, cooling and separating by centrifuge, then washing the precipitate with pure water until yttrium is not detected in the washing liquid, then washing three times with ethanol, and then placing in an oven, drying at 90-100° C. for 6-8 hours to obtain the modified graphite.
[0039] In one embodiment, the mass ratio of the carbon fiber, urea and melamine is 5-7:0.8-1.2:0.8-1.2.
[0040] In one embodiment, the hot pressing conditions are a temperature of 145-152° C. and a pressure of 5-7 MPa.
[0041] In one embodiment, the conductive material includes at least one of carbon fiber, carbon nanotube, acetylene black, mesoporous carbon, conductive carbon black, carbon aerogel, graphite and graphene.
[0042] In one embodiment, the dispersant includes at least one of polytetrafluoroethylene, polychlorotrifluoroethylene, vinylidene fluoride-chlorotrifluoroethylene copolymer, copolymer of tetrafluoroethylene and hexafluoroethylene, polyvinyl fluoride, polyvinylidene fluoride, ethylene-chlorotrifluoroethylene copolymer, tetrafluoroethylene-hexafluoropropylene copolymer, ethylene-tetrafluoroethylene copolymer and tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer.
[0043] In one embodiment, the solvent includes at least one of water, ethanol, ethylene glycol, acetone, glycerol, N,N-dimethylformamide, dimethyl sulfoxide, dimethylacetamide and N-methylpyrrolidone.
[0044] In one of the embodiments, the mass ratio of graphite to nitric acid is 8-10:1, and the mass ratio of hydrazine hydrate to ethylenediamine is 1:0.8-1.2.
[0045] In one embodiment, the present technical solution provides a fuel cell, which includes a proton exchange membrane, a gas diffusion layer, a catalyst layer and a bipolar plate, wherein the gas diffusion layer is carbon paper for fuel cells prepared by the preparation method provided by the above technical solution.
[0046] The embodiments of the present invention will be described in detail below with reference to specific examples.
[0047] Embodiment 1:
[0048] Preparation of modified graphite: add graphite to an ethanol solution, ultrasonicate at a frequency of 60KHz for 5.5 hours, then add an aqueous solution of yttrium nitrate, stir evenly, then ultrasonicate at a frequency of 60KHz for 1.5 hours, continue stirring at a speed of 300r / min, then add hydrazine hydrate, stir evenly and add ethylenediamine, then heat to 53°C, react for 2.5 hours, cool and separate by centrifuge, then wash the precipitate with pure water until yttrium is not detected in the washing liquid, then wash three times with ethanol, then place in an oven, dry at 95°C for 7 hours to obtain modified graphite, wherein the mass ratio of graphite to yttrium nitrate is 9:1, and the mass ratio of hydrazine hydrate to ethylenediamine is 1:1;
[0049] Preparation of modified carbon fiber: 1 mm carbon fiber was added to acetone, refluxed for 2.5 h, then washed with ethanol, and then dried at 65 ° C. After drying, it was added to water, ultrasonicated for 0.7 h, and then urea was added, stirred at a speed of 400 r / min for 2.5 h, and then a melamine-ethylene glycol mixture was added, and then stirred at a speed of 530 r / min for 3.7 h, and then filtered, and the solid was heated to 220 ° C under a nitrogen atmosphere for activation to obtain modified carbon fiber, wherein the mass ratio of carbon fiber, urea and melamine was 6:1:1;
[0050] Preparation of impregnation solution: conductive material carbon nanotubes, modified graphite, 60wt% polytetrafluoroethylene aqueous emulsion and water are uniformly mixed to obtain an impregnation solution, wherein the mass ratio of conductive material carbon nanotubes, modified graphite, polytetrafluoroethylene and water is 1:10:6:90;
[0051] Preparation of carbon fiber base paper: Add modified carbon fiber to water, ultrasonicate at a frequency of 60KHz for 1.3h, then add polysorbate and polyethylene oxide, stir at a speed of 600r / min for 6h, then add polyvinyl alcohol, continue to stir at a speed of 600r / min for 3.3h, then perform wet forming, dry the formed paper at 85°C for 55min, and then hot press, the hot pressing conditions are temperature 147°C, pressure 6MPa, to obtain carbon fiber base paper, wherein the mass ratio of modified carbon fiber, polysorbate, polyethylene oxide and polyvinyl alcohol is 15:4:12:13;
[0052] Impregnation and carbonization: The carbon fiber base paper is immersed in the impregnation liquid for 55 minutes, then dried at 100°C under a nitrogen protective atmosphere, then heated to 260°C under an argon protective atmosphere and maintained for 2.5 hours for curing, and then heated to 1850°C under an argon protective atmosphere for carbonization to obtain carbon paper for fuel cells.
[0053] Embodiment 2:
[0054] The other parts are the same as those in Example 1, except that the mass ratio of carbon fiber, urea and melamine is 6:1:0.8.
[0055] Embodiment 3:
[0056] The other parts are the same as those in Example 1, except that the mass ratio of carbon fiber, urea and melamine is 6:1:1.2.
[0057] Comparative Example 1:
[0058] Preparation of modified carbon fiber: 1 mm carbon fiber was added to acetone, refluxed for 2.5 h, then washed with ethanol, and then dried at 65 ° C. After drying, it was added to water, ultrasonicated for 0.7 h, and then urea was added, stirred at a speed of 400 r / min for 2.5 h, and then a melamine-ethylene glycol mixture was added, and then stirred at a speed of 530 r / min for 3.7 h, and then filtered, and the solid was heated to 220 ° C under a nitrogen atmosphere for activation to obtain modified carbon fiber, wherein the mass ratio of carbon fiber, urea and melamine was 6:1:1;
[0059] Preparation of impregnation solution: conductive materials carbon nanotubes, graphite, 60wt% polytetrafluoroethylene aqueous emulsion and water are uniformly mixed to obtain an impregnation solution, wherein the mass ratio of carbon nanotubes, graphite, polytetrafluoroethylene and water is 1:10:6:90;
[0060] Preparation of carbon fiber base paper: Add modified carbon fiber to water, ultrasonicate at a frequency of 60KHz for 1.3h, then add polysorbate and polyethylene oxide, stir at a speed of 600r / min for 6h, then add polyvinyl alcohol, continue to stir at a speed of 600r / min for 3.3h, then perform wet forming, dry the formed paper at 85°C for 55min, and then hot press, the hot pressing conditions are temperature 147°C, pressure 6MPa, to obtain carbon fiber base paper, wherein the mass ratio of modified carbon fiber, polysorbate, polyethylene oxide and polyvinyl alcohol is 15:4:12:13;
[0061] Impregnation and carbonization: The carbon fiber base paper is immersed in the impregnation liquid for 55 minutes, then dried at 100°C under a nitrogen protective atmosphere, then heated to 260°C under an argon protective atmosphere and maintained for 2.5 hours for curing, and then heated to 1850°C under an argon protective atmosphere for carbonization to obtain carbon paper for fuel cells.
[0062] Comparative Example 2:
[0063] Preparation of modified graphite: add graphite to an ethanol solution, ultrasonicate at a frequency of 60KHz for 5.5 hours, then add an aqueous solution of yttrium nitrate, stir evenly, then ultrasonicate at a frequency of 60KHz for 1.5 hours, continue stirring at a speed of 300r / min, then add hydrazine hydrate, stir evenly and add ethylenediamine, then heat to 53°C, react for 2.5 hours, cool and separate by centrifuge, then wash the precipitate with pure water until yttrium is not detected in the washing liquid, then wash three times with ethanol, then place in an oven, dry at 95°C for 7 hours to obtain modified graphite, wherein the mass ratio of graphite to yttrium nitrate is 9:1, and the mass ratio of hydrazine hydrate to ethylenediamine is 1:1;
[0064] Preparation of impregnation solution: conductive material carbon nanotubes, modified graphite, 60wt% polytetrafluoroethylene aqueous emulsion and water are uniformly mixed to obtain an impregnation solution, wherein the mass ratio of carbon nanotubes, conductive carbon black, polytetrafluoroethylene and water is 1:10:6:90;
[0065] Preparation of carbon fiber base paper: 1mm carbon fiber is added to water, ultrasonicated at a frequency of 60KHz for 1.3h, then polysorbate and polyethylene oxide are added, stirred at a speed of 600r / min for 6h, then polyvinyl alcohol is added, and stirring is continued at a speed of 600r / min for 3.3h, and then wet forming is performed, and the formed paper is dried at 85°C for 55min, and then hot pressed. The hot pressing conditions are a temperature of 147°C and a pressure of 6MPa to obtain a carbon fiber base paper, wherein the mass ratio of modified carbon fiber, polysorbate, polyethylene oxide and polyvinyl alcohol is 15:4:12:13;
[0066] Impregnation and carbonization: The carbon fiber base paper is immersed in the impregnation liquid for 55 minutes, then dried at 100°C under a nitrogen protective atmosphere, then heated to 260°C under an argon protective atmosphere and maintained for 2.5 hours for curing, and then heated to 1850°C under an argon protective atmosphere for carbonization to obtain carbon paper for fuel cells.
[0067] Comparative Example 3:
[0068] Preparation of modified graphite: add graphite to an ethanol solution, ultrasonicate at a frequency of 60KHz for 5.5 hours, then add an aqueous solution of yttrium nitrate, stir evenly, then ultrasonicate at a frequency of 60KHz for 1.5 hours, continue stirring at a speed of 300r / min, then add hydrazine hydrate, stir evenly and add ethylenediamine, then heat to 53°C, react for 2.5 hours, cool and separate by centrifuge, then wash the precipitate with pure water until yttrium is not detected in the washing liquid, then wash three times with ethanol, then place in an oven, dry at 95°C for 7 hours to obtain modified graphite, wherein the mass ratio of graphite to yttrium nitrate is 9:1, and the mass ratio of hydrazine hydrate to ethylenediamine is 1:1;
[0069] Preparation of modified carbon fiber: 1 mm carbon fiber was added to acetone, refluxed for 2.5 h, then washed with ethanol, and then dried at 65 ° C. After drying, it was added to water, ultrasonicated for 0.7 h, and then a melamine-ethylene glycol mixture was added, and then stirred at a speed of 530 r / min for 3.7 h, and then filtered. The solid was heated to 220 ° C in a nitrogen atmosphere for activation to obtain a modified carbon fiber, wherein the mass ratio of carbon fiber to melamine was 6:1;
[0070] Preparation of impregnation solution: conductive material carbon nanotubes, modified graphite, 60wt% polytetrafluoroethylene aqueous emulsion and water are uniformly mixed to obtain an impregnation solution, wherein the mass ratio of conductive material carbon nanotubes, modified graphite, polytetrafluoroethylene and water is 1:10:6:90;
[0071] Preparation of carbon fiber base paper: Add modified carbon fiber to water, ultrasonicate at a frequency of 60KHz for 1.3h, then add polysorbate and polyethylene oxide, stir at a speed of 600r / min for 6h, then add polyvinyl alcohol, continue to stir at a speed of 600r / min for 3.3h, then perform wet forming, dry the formed paper at 85°C for 55min, and then hot press, the hot pressing conditions are temperature 147°C, pressure 6MPa, to obtain carbon fiber base paper, wherein the mass ratio of modified carbon fiber, polysorbate, polyethylene oxide and polyvinyl alcohol is 15:4:12:13;
[0072] Impregnation and carbonization: The carbon fiber base paper is immersed in the impregnation liquid for 55 minutes, then dried at 100°C under a nitrogen protective atmosphere, then heated to 260°C under an argon protective atmosphere and maintained for 2.5 hours for curing, and then heated to 1850°C under an argon protective atmosphere for carbonization to obtain carbon paper for fuel cells.
[0073] Comparative Example 4:
[0074] Preparation of modified graphite: add graphite to an ethanol solution, ultrasonicate at a frequency of 60KHz for 5.5 hours, then add an aqueous solution of yttrium nitrate, stir evenly, then ultrasonicate at a frequency of 60KHz for 1.5 hours, continue stirring at a speed of 300r / min, then add hydrazine hydrate, stir evenly and add ethylenediamine, then heat to 53°C, react for 2.5 hours, cool and separate by centrifuge, then wash the precipitate with pure water until yttrium is not detected in the washing liquid, then wash three times with ethanol, then place in an oven, dry at 95°C for 7 hours to obtain modified graphite, wherein the mass ratio of graphite to yttrium nitrate is 9:1, and the mass ratio of hydrazine hydrate to ethylenediamine is 1:1;
[0075] Preparation of modified carbon fiber: 1 mm carbon fiber was added to acetone, refluxed for 2.5 h, then washed with ethanol, and then dried at 65 ° C. After drying, it was added to water, ultrasonicated for 0.7 h, and then urea was added, stirred at a speed of 400 r / min for 2.5 h, and then filtered. The solid was heated to 220 ° C in a nitrogen atmosphere for activation to obtain modified carbon fiber, wherein the mass ratio of carbon fiber to urea was 6:1;
[0076] Preparation of impregnation solution: conductive material carbon nanotubes, modified graphite, 60wt% polytetrafluoroethylene aqueous emulsion and water are uniformly mixed to obtain an impregnation solution, wherein the mass ratio of conductive material carbon nanotubes, modified graphite, polytetrafluoroethylene and water is 1:10:6:90;
[0077] Preparation of carbon fiber base paper: Add modified carbon fiber to water, ultrasonicate at a frequency of 60KHz for 1.3h, then add polysorbate and polyethylene oxide, stir at a speed of 600r / min for 6h, then add polyvinyl alcohol, continue to stir at a speed of 600r / min for 3.3h, then perform wet forming, dry the formed paper at 85°C for 55min, and then hot press, the hot pressing conditions are temperature 147°C, pressure 6MPa, to obtain carbon fiber base paper, wherein the mass ratio of modified carbon fiber, polysorbate, polyethylene oxide and polyvinyl alcohol is 15:4:12:13;
[0078] Impregnation and carbonization: The carbon fiber base paper is immersed in the impregnation liquid for 55 minutes, then dried at 100°C under a nitrogen protective atmosphere, then heated to 260°C under an argon protective atmosphere and maintained for 2.5 hours for curing, and then heated to 1850°C under an argon protective atmosphere for carbonization to obtain carbon paper for fuel cells.
[0079] The carbon papers for fuel cells of Examples 1 to 3 and Comparative Examples 1 to 4 were tested for vertical resistivity, air permeability and tensile strength. The test results are shown in Table 1.
[0080] Table 1:
[0081]
[0082] As can be seen from Table 1, the carbon papers for fuel cells in Examples 1 to 3 have stable and excellent air permeability, electrical conductivity and mechanical strength, because carbon fibers modified with urea and melamine and graphite modified with nitric acid, hydrazine hydrate and ethylenediamine are used simultaneously in the preparation process. Among them, the vertical resistivity is as low as 65mΩ·cm or less, the air permeability is stably as high as 2000ml*mm / (cm*h*mmAQ) or more, and the tensile strength is as high as 25MPa or more. Specifically, since the modified carbon fiber is modified by linear urea and cyclic melamine at the same time, after activation, the modified carbon fiber is doped with nitrogen elements, and some nitrogen-containing groups can be arranged in a three-dimensional and orderly manner on the surface of the modified carbon fiber. Furthermore, the modified carbon fiber is impregnated with an impregnation solution of modified graphite, and the embedded nitrogen-containing elements and the nitrogen-containing groups on the surface interact with the nitrogen-containing groups of the modified graphite, so that the modified graphite is evenly and orderly arranged on the surface of the modified carbon fiber, and can form an efficient electron channel in the longitudinal direction. Therefore, the air permeability, electrical conductivity and mechanical strength of the carbon paper for fuel cells prepared using this technical solution are stable and excellent.
[0083] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0084] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for preparing carbon paper for fuel cells, characterized in that: It includes the following steps: Preparation of carbon fiber base paper: adding modified carbon fiber to water, ultrasonicating at a frequency of 50-70kHz for 1-1.5h, then adding polysorbate and polyethylene oxide, stirring at a speed of 550-650r / min for 5-7h, then adding polyvinyl alcohol, continuing to stir at a speed of 550-650r / min for 3.0-3.6h, then wet forming, drying the formed paper at 80-90°C for 50-60min, and then hot pressing to obtain the carbon fiber base paper; Impregnation and carbonization: the carbon fiber base paper is impregnated in the impregnation liquid for 50-60 minutes, then dried at 95-105° C. under a nitrogen protective atmosphere, then heated to 250-270° C. under an argon protective atmosphere for 2-3 hours for curing, and then heated to 1800-1900° C. under an argon protective atmosphere for carbonization to obtain the carbon paper for fuel cells; The impregnation solution includes modified graphite, conductive material, dispersant and solvent; The raw materials for preparing the modified carbon fiber include carbon fiber, urea and melamine; The raw materials for preparing the modified graphite include yttrium nitrate, hydrazine hydrate and ethylenediamine; The mass ratio of the modified carbon fiber, polysorbate, polyethylene oxide and polyvinyl alcohol is 13-17:3-5:10-15:10-15; The length of the carbon fiber is 0.8-1.2 mm; The preparation method of the modified carbon fiber comprises the following steps: Preparation of modified carbon fiber: adding carbon fiber to acetone, refluxing for 2-3 hours, then washing with ethanol, then drying at 60-70°C, adding to water after drying, ultrasonicating at a frequency of 50-70kHz for 0.6-0.8 hours, then adding urea, stirring at a speed of 380-420r / min for 2-3 hours, then adding melamine-ethylene glycol mixture, then stirring at a speed of 500-560r / min for 3.5-3.9 hours, then filtering, heating the solid to 210-230°C under a nitrogen atmosphere for activation, and obtaining the modified carbon fiber; The preparation method of the modified graphite comprises the following steps: Preparation of modified graphite: adding graphite to an ethanol solution, ultrasonicating at a frequency of 50-70kHz for 5-6h, then adding an aqueous yttrium nitrate solution, stirring evenly, then ultrasonicating at a frequency of 50-70kHz for 1.2-1.8h, continuing to stir at a speed of 250-350r / min, then adding hydrazine hydrate, stirring evenly, adding ethylenediamine, then heating to 50-56°C, reacting for 2.2-2.8h, cooling and separating by centrifuge, then washing the precipitate with pure water until yttrium is not detected in the washing liquid, then washing three times with ethanol, and then placing in an oven, drying at 90-100°C for 6-8h to obtain the modified graphite; The dispersant includes at least one of polytetrafluoroethylene, polychlorotrifluoroethylene, vinylidene fluoride-chlorotrifluoroethylene copolymer, copolymer of tetrafluoroethylene and hexafluoroethylene, polyvinyl fluoride, polyvinylidene fluoride, ethylene-chlorotrifluoroethylene copolymer, tetrafluoroethylene-hexafluoropropylene copolymer, ethylene-tetrafluoroethylene copolymer and tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer.
2. The preparation method according to claim 1, characterized in that: The mass ratio of the carbon fiber, urea and melamine is 5-7:0.8-1.2:0.8-1.
2.
3. The preparation method according to claim 1, characterized in that: The hot pressing conditions are a temperature of 145-152° C. and a pressure of 5-7 MPa.
4. The preparation method according to claim 1, characterized in that: The conductive material includes at least one of carbon fiber, carbon nanotube, acetylene black, mesoporous carbon, conductive carbon black, carbon aerogel, graphite and graphene.
5. The preparation method according to claim 1, characterized in that: The solvent includes at least one of water, ethanol, ethylene glycol, acetone, glycerol, N,N-dimethylformamide, dimethyl sulfoxide, dimethylacetamide and N-methylpyrrolidone.
6. The preparation method according to claim 1, characterized in that: The mass ratio of the graphite to yttrium nitrate is 8-10:1, and the mass ratio of hydrazine hydrate to ethylenediamine is 1:0.8-1.
2.
7. A fuel cell comprising a proton exchange membrane, a gas diffusion layer, a catalyst layer and a bipolar plate, characterized in that: The gas diffusion layer is carbon paper for fuel cells prepared by the preparation method according to claim 1.
Citation Information
Patent Citations
Carbon fiber paper for gas diffusion layer of fuel cell as well as preparation method and application of carbon fiber paper
CN115341407A
Nitrogen-rich porous carbon desulfurizer and preparation method thereof
CN103432897A
Cross-sensitive material for benzene, toluene and ethylbenzene
CN104849402A
Gas diffusion layer material for fuel cell and preparation method thereof
CN1734812A