Co-production of polyaluminium ferric chloride using white carbon black prepared from gold mine tailings and method thereof
By pretreating and acid-base treatment of gold mine tailings, white carbon black and polymeric ferrous aluminum chloride were successfully prepared, solving the problem of inefficient resource utilization of gold mine tailings and achieving high efficiency of aluminum and silicon elements Extraction improves tailings utilization efficiency and environmental safety.
Patent Information
- Application Number
- CN202311745841.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-18
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-12-18
AI Technical Summary
The resource utilization method of gold mine tailings is inefficient, which leads to the accumulation of tailings occupying land, polluting the environment, and posing safety hazards, and failing to effectively coordinate the extraction of aluminum and silicon elements.
After pretreatment with gold tailings, it is mixed with hydrochloric acid to obtain polymerized ferrous aluminum chloride by microwave thermal polymerization, and white carbon black is obtained through alkaline melting treatment and water-soluble aging, achieving efficient extraction of ferrous aluminum and silicon elements.
The resource utilization and high-value utilization of gold tailings have been achieved, and high-purity white carbon black and polymer aluminum chloride have been prepared, which has improved the utilization efficiency of tailings and is of great economic and environmental significance.
Smart Images

Figure CN117699810B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of resource utilization of gold mine tailings, and in particular to co-production of polyaluminium ferric chloride by using white carbon black prepared from gold mine tailings and a method thereof. Background Art
[0002] As an important silicon-based inorganic fine chemical raw material, white carbon black is widely used in rubber, medicine, plastics, papermaking, coatings and daily necessities. At present, most of the white carbon black produced in China uses sodium silicate obtained by the reaction of quartz sand and soda ash as the silicon source, and then undergoes acidification treatment with inorganic acids (including sulfuric acid, hydrochloric acid and nitric acid, etc.) or CO2.
[0003] Polyaluminium ferric chloride (PAFC) is an inorganic polymer coagulant formed by the coagulation and hydrolysis of aluminium salts and iron salts. At present, the domestic method for preparing polyaluminium ferric chloride is mainly to use various iron-containing waste materials generated in the factory production process, which are crushed and roasted, and then acid-leached with sulfuric acid or hydrochloric acid. After filtering, the aluminium-iron molar ratio and alkalinity in the solution are adjusted, and then the PAFC liquid is prepared by the heating polymerization method. The PAFC liquid is concentrated, evaporated and ground to obtain PAFC solid.
[0004] Gold tailings refer to the solid waste discharged after gold or other useful components are recovered from gold ore through the mineral processing process. According to incomplete statistics, the stockpile of gold tailings in China is nearly 270 million tons, and the tailings discharged by gold mines each year have exceeded 24.5 million tons. A large amount of tailings cannot be recycled and are piled up in tailings ponds, which not only occupies land resources and pollutes the atmosphere, surface water and groundwater, but also poses huge safety hazards. The disposal of gold tailings has become a major factor restricting the sustainable economic development of gold mines.
[0005] Gold mine tailings are composed of composite minerals mainly composed of aluminum silicate minerals. They are usually alkaline and have fine particle size. The tailings have a high content of silicon dioxide, and also contain some aluminum oxide, iron oxide and a small amount of metal elements such as silver, copper and lead. The current resource utilization of gold mine tailings is inefficient. At the same time, there are a large number of silicon and aluminum elements in gold mine tailings, which are a secondary resource with great utilization value. The coordinated extraction and utilization of aluminum, iron and silicon elements has become an important direction for the resource utilization and high-value utilization of gold mine tailings. Summary of the invention
[0006] The present invention provides a method for co-producing polyaluminium ferric chloride by using gold mine tailings to prepare white carbon black, so as to solve the problem of inefficient resource utilization of existing gold mine tailings. The gold mine tailings are used as raw materials to extract aluminium and iron elements and high-purity silicon slag, and the aluminium and iron elements and high-purity silicon slag are used to prepare polyaluminium ferric chloride and white carbon black.
[0007] In order to achieve the above object, the present invention adopts the following technical solutions:
[0008] A method for preparing white carbon black and co-producing polyaluminium ferric chloride by using gold mine tailings comprises the following steps:
[0009] The pretreated gold tailings are mixed with hydrochloric acid, and after sufficient reaction, solid-liquid separation is performed to obtain an acid leaching solution rich in aluminum and iron elements and an acid leaching residue rich in silicon dioxide;
[0010] Controlling the ratio of aluminum and iron elements in the acid leaching solution rich in aluminum and iron elements, adjusting the alkalinity of the acid leaching solution rich in aluminum and iron elements, and then performing microwave thermal polymerization to obtain polyaluminum ferric chloride;
[0011] The acid leaching residue rich in silicon dioxide is subjected to alkali melting treatment to obtain alkali melted residue;
[0012] The alkali-melted slag is dissolved in water and aged in a water bath, and then solid-liquid separation is performed to obtain a sodium silicate solution;
[0013] After diluting the sodium silicate solution, the pH value of the diluted sodium silicate solution is adjusted, and finally the solution is aged, filtered, washed, dried and ground to obtain white carbon black.
[0014] Furthermore, the pretreated gold mine tailings are obtained by the following steps:
[0015] The gold mine tailings are crushed and screened step by step, and finally calcined and activated to obtain the pre-treated gold mine tailings;
[0016] The temperature of the calcination activation is 600° C. to 1000° C., and the insulation time of the calcination activation is 0.5 h to 3 h.
[0017] Furthermore, it is characterized in that the concentration of the hydrochloric acid is 5% to 30%.
[0018] Furthermore, the pretreated gold tailings are mixed with hydrochloric acid at a solid-liquid ratio of 1 g: (3-10) mL; and the full reaction is carried out at a temperature of 60° C. to 110° C.
[0019] Furthermore, the molar ratio of aluminum and iron in the acid leaching solution rich in aluminum and iron is controlled to be aluminum: iron = (3-10): 1; and the alkalinity of the acid leaching solution rich in aluminum and iron is adjusted to be 0.1-1.5.
[0020] Furthermore, the temperature of the microwave thermal polymerization is 50° C. to 100° C., the power of the microwave thermal polymerization is 500 W, and the insulation time of the microwave thermal polymerization is 0.5 h to 3 h.
[0021] Furthermore, when the acid leaching residue rich in silicon dioxide is subjected to alkali melting treatment, the acid leaching residue rich in silicon dioxide and the alkaline solution are subjected to alkali melting treatment in a mass ratio of 1:(1-3); the temperature of the alkali melting treatment is 500°C-700°C.
[0022] Furthermore, when the alkali-molten slag is subjected to water-soluble aging in a water bath, the alkali-molten slag and distilled water are dissolved in water at a solid-liquid ratio of 1 g: (3-10) mL; the temperature of the alkali-molten slag water bath is 50° C.-110° C., and the water bath time is 0.5 h-3 h; the aging time of the alkali-molten slag subjected to water-soluble aging in a water bath is 6 h-20 h.
[0023] Furthermore, the mass fraction of silicon dioxide in the diluted sodium silicate solution is 0.5% to 7%; the pH value of the diluted sodium silicate solution is adjusted to 6.8 to 7.2; and the temperature when adjusting the pH value of the diluted sodium silicate solution is 50° C. to 90° C.
[0024] A method for preparing white carbon black and co-producing polyaluminium ferric chloride by using gold mine tailings is disclosed. The method is used to prepare white carbon black and co-produce polyaluminium ferric chloride by using gold mine tailings.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] The present invention provides a method for preparing white carbon black and co-producing polyaluminum ferric chloride by utilizing gold mine tailings. The pretreated gold mine tailings are used as raw materials, and an acid leaching solution rich in aluminum and iron elements is obtained by acid treatment, and polyaluminum ferric chloride is obtained by microwave thermal polymerization. Meanwhile, an acid leaching residue rich in silicon dioxide is obtained by acid treatment, and a sodium silicate solution is obtained by alkali melting treatment, water dissolution aging, and solid-liquid separation in sequence. Finally, the sodium silicate solution is diluted and its pH value is adjusted, and white carbon black is obtained by aging, filtering, washing, and drying and grinding in sequence. The present invention prepares high-value products white carbon black and polyaluminum ferric chloride by utilizing abandoned gold mine tailings, and aluminum, iron and silicon elements in the gold mine tailings are extracted efficiently and synergistically, thereby realizing the resource utilization and high-value utilization of the gold mine tailings, and has important significance for the resource utilization and high-value utilization of the gold mine tailings and the development of the white carbon black industry. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 A process roadmap for the method of preparing white carbon black and co-producing polyaluminium ferric chloride from gold mine tailings provided in an embodiment of the present invention;
[0028] Figure 2 This is the infrared analysis spectrum of the polyaluminium ferric chloride prepared in Example 1 of the present invention;
[0029] Figure 3 This is a physical picture of white carbon black prepared in Example 1 of the present invention;
[0030] Figure 4 This is the XRD analysis spectrum of the white carbon black prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0031] The technical solution of the present invention is described in detail below:
[0032] Step 1: Pre-pretreatment of the gold tailings raw materials, including calcination and activation of the crushed and screened gold tailings to obtain pre-treated gold tailings;
[0033] Specifically, the gold tailings raw material is crushed at a rotation speed of 500 rpm using a planetary ball mill for 30 minutes and then sieved step by step. Then, the gold tailings slag passing through a 100-mesh sieve is calcined and activated at 600° C. to 1000° C. for a holding time of 0.5 h to 3 h to obtain pretreated gold tailings.
[0034] Step 2: subjecting the pretreated gold tailings obtained in step 1 to acid treatment, including mixing the pretreated gold tailings with hydrochloric acid of a certain concentration and reacting them fully at a certain temperature to obtain acid leaching residues rich in silicon dioxide and acid leaching liquid rich in aluminum and iron elements;
[0035] Specifically, the concentration of the hydrochloric acid is 5% to 30%, the pretreated gold tailings and the hydrochloric acid are mixed at a solid-liquid ratio of 1 g: (3 to 10) mL, and stirred in a water bath at 60° C. to 110° C. for full reaction, and then the solid-liquid separation is performed to obtain an acid leaching solution rich in aluminum and iron elements and an acid leaching residue rich in silicon dioxide;
[0036] Specifically, the silicon dioxide content of the silicon dioxide-rich acid leaching residue is 70% to 92%.
[0037] Step 3: using the acid leaching solution rich in aluminum and iron elements obtained in step 2 as a raw material, adjusting the aluminum-iron molar ratio and alkalinity in the acid leaching solution, and finally obtaining polyaluminum-ferric chloride by microwave thermal polymerization;
[0038] Specifically, the aluminum-iron molar ratio in the acid leaching solution rich in aluminum and iron elements is adjusted to Al:Fe=(3-10):1, and NaOH solution is added dropwise to adjust the alkalinity of the acid leaching solution rich in aluminum and iron elements to 0.1-1.5, and then the acid leaching solution is purified and subjected to microwave thermal polymerization reaction at a temperature of 50°C-100°C, the microwave power is 500W, the insulation time is 0.5h-3h, and finally aged for 20h to obtain a polyaluminum ferric chloride solution, and the polyaluminum ferric chloride solution is evaporated and dried to obtain polyaluminum ferric chloride.
[0039] Step 4: using the silicon dioxide-rich acid leaching residue obtained in step 2 as a raw material, first washing and drying the residue, and then adjusting the slag alkali mass ratio to perform high-temperature alkali melting treatment in a muffle furnace to obtain alkali-melted slag;
[0040] Specifically, the mass ratio of the acid leaching residue rich in silicon dioxide to the alkaline solution is 1:(1-3), and the alkaline melting treatment is carried out in a muffle furnace at a temperature of 500° C. to 700° C., and the insulation time is 0.5 h to 3 h.
[0041] Step 5: using the alkali-melted slag obtained in step 4 as a raw material, performing water dissolution aging and solid-liquid separation treatment in a high-temperature water bath to obtain a sodium silicate solution and a residue;
[0042] Specifically, distilled water is added to the alkali molten slag when it is dissolved in water, the solid-liquid ratio between the alkali molten slag and the distilled water is 1g: (3-10)mL, and the alkali molten slag is stirred in a high temperature water bath at 50°C-110°C, the reaction time is 0.5h-3h, and after the reaction is completed, the aging and filtering treatment is performed, and the aging time is 6h-20h;
[0043] Step 6: diluting the sodium silicate solution obtained in step 5 so that its silicon dioxide concentration reaches a certain range, then adding an acidic substance under high temperature water bath conditions to make the solution reach a certain pH value, and finally performing aging, filtering and washing treatments, and drying and grinding the filtered residue to obtain a white carbon black product;
[0044] Specifically, the mass fraction of silicon dioxide in the diluted sodium silicate solution is 0.5% to 7%, and then the diluted sodium silicate solution is adjusted to a pH of 6.8 to 7.2 at a temperature of 50° C. to 90° C., and then filtered and washed after standing for about 2 hours, and the washed filter residue is dried and ground at 105° C. to obtain a white powder as a white carbon black product.
[0045] The present invention will be described in detail below in conjunction with embodiments. It should be noted that the embodiments and features in the embodiments of the present application can be combined with each other without conflict.
[0046] The following detailed description is the description of the embodiments, and is intended to provide further detailed description of the present invention. Unless otherwise specified, all technical terms used in the present invention have the same meaning as those generally understood by those skilled in the art to which the present application belongs. The terms used in the present invention are only for describing specific embodiments, and are not intended to limit the exemplary embodiments according to the present invention.
[0047] The present invention provides a method for preparing white carbon black and co-producing polyaluminium ferric chloride by using gold mine tailings. The gold mine tailings that have been pre-treated and processed are used as raw materials, and the aluminium and iron elements in the gold mine tailings are extracted by acid treatment to prepare polyaluminium ferric chloride, and the acid leaching residue obtained by acid treatment is washed with water and used as raw material to prepare white carbon black.
[0048] The gold mine tailings used in the implementation of each example of the present invention are all taken from a gold mine in Shaanxi. The gold mine tailings are subjected to chemical composition analysis, and the results are shown in Table 1 below:
[0049] Table 1 Chemical composition of gold mine tailings (%)
[0050]
[0051] In the flocculation experiments of the homemade polyaluminium ferric chloride flocculant involved in the embodiments of the present invention, the target water samples are all simulated wastewater with a turbidity of 74 NTU prepared by using kaolin and tap water;
[0052] The steps of the flocculation experiment are as follows: take 100 ml of the target water sample and add it into a beaker and stir rapidly. At the same time, add a certain amount of homemade polyaluminium ferric chloride flocculant, stir rapidly for 1 minute, then stir slowly for 5 minutes, let it stand for 3 minutes, and take the supernatant for turbidity detection.
[0053] Embodiment 1
[0054] This embodiment provides a method for preparing white carbon black and co-producing polyaluminium ferric chloride using gold mine tailings, which specifically comprises the following steps:
[0055] 1) The gold tailings were crushed and passed through a 100-mesh sieve to obtain powdered gold tailings. 12 g of the gold tailings powder was calcined at 850° C. and kept warm for 2 h to obtain calcined slag.
[0056] 2) Take 10 g of the calcined gold tailings powder in 1) and add it to 100 ml of 10% hydrochloric acid, place it in a 70° C. water bath for 1 hour, and filter to obtain a filtrate and a filter residue.
[0057] 3) Take the filtrate obtained in 2), add distilled water to 100 ml, add 6.613 g of anhydrous AlCl3 to make the Al:Fe molar ratio of the solution 9:1, and at the same time add an appropriate amount of NaOH to make its alkalinity 0.1, then separate and purify the solution, microwave heat to 90°C at a power of 500 W for polymerization for 1 hour, and age for 20 hours to obtain a polyaluminum ferric chloride solution. After the solution is evaporated and dried, solid polyaluminum ferric chloride can be obtained.
[0058] 4) 5 g of the filter residue obtained in 2) was washed and dried, and then mixed and ground with 10.5 g of NaOH. The mixture was placed in a muffle furnace and kept at 500° C. for 1 h to obtain 14.12 g of alkali-melted slag;
[0059] 5) Take 10 g of the alkali-melted slag in 4) and add 100 ml of distilled water to a 250 ml beaker. Stir in a water bath at 80°C for 1.5 h, then age for 12 h, and filter to obtain 92 ml of a sodium silicate solution with a modulus of 2.21 and a residue.
[0060] 6) Take 50 ml of the sodium silicate solution with a modulus of 2.21 in 5) and add 50 ml of distilled water to dilute it, adjust its pH to 7.0 at 80°C, age it for 2 hours, then filter and wash it, dry and grind the filter residue at 105°C to obtain 3.2 g of white powder, and perform XRD analysis on the white powder as follows: Figure 3 As shown in the figure, there is only one diffuse diffraction peak near 22°, and the peak intensity is small and the width is large, indicating that the sample is amorphous and there are no other impurity peaks in the spectrum. It is confirmed to be a white carbon black product. The whiteness of the white carbon black product prepared under this condition is 93 and the specific surface area is 182.7754m 2 / g, DBP oil absorption value is 2.66ml / g.
[0061] Fourier transform infrared spectrometer was used to detect the characteristic peak position and intensity of polyaluminium ferric chloride (PAFC) and analyze the internal structural characteristics, such as Figure 2 As shown, at 3410cm -1 There is a strong absorption peak at 1630cm -1 There is a medium absorption peak at 1120cm, which is a bending vibration peak caused by the vibration of physical water absorption; -1 With 590cm -1 There is a weak absorption peak at the position. Based on this absorption peak and its intensity, it is shown that the homemade PAFC contains both iron and aluminum polymers bridged by hydroxyl groups, indicating that the polyaluminium ferric chloride flocculant has been successfully prepared.
[0062] By measuring the aluminum and iron contents in the filtrate obtained after acid leaching, it was found that the leaching rates of aluminum and iron elements were 64.6% and 91.2% respectively, and the turbidity removal rate of simulated wastewater was 92%. The final measured aluminum oxide content of the obtained solid polyaluminum ferric chloride was 30.1%, which met the HG / T 5359-2018 content standard.
[0063] Embodiment 2
[0064] This embodiment provides a method for preparing white carbon black and co-producing polyaluminium ferric chloride from gold mine tailings. The method comprises the following steps:
[0065] 1) The gold tailings were crushed and passed through a 100-mesh sieve to obtain powdered gold tailings. 12 g of the gold tailings powder was calcined at 950° C. and kept warm for 2 h to obtain calcined slag.
[0066] 2) Take 10 g of the calcined gold tailings powder in 1) and add it to 80 ml of 15% hydrochloric acid, place it in a water bath at 80° C. for 2 h, and filter to obtain a filtrate and a residue.
[0067] 3) Take the filtrate obtained in 2), add distilled water to 100 ml, add 7.023 g of anhydrous AlCl3 dropwise to make its Al:Fe molar ratio 10:1, and at the same time add an appropriate amount of NaOH dropwise to make its alkalinity 0.6, separate and purify the solution, microwave heat to 85°C at a power of 500 W for polymerization for 1 hour, and then age for 20 hours to obtain a polyaluminum ferric chloride solution, and evaporate the solution to dryness to obtain solid polyaluminum ferric chloride.
[0068] 4) Take 5 g of the filter residue obtained in 2), wash with water until neutral and dry, then mix and grind with 14.7 g of NaOH, put the mixture into a muffle furnace and keep it at 600° C. for 2 h to obtain 19.3 g of alkali-melted slag;
[0069] 5) Take 10 g of the alkali-melted slag in 4) into a 250 ml beaker, add 50 ml of distilled water, stir in a water bath at 107°C for 1 hour, then age for 20 hours, and filter to obtain 47 ml of sodium silicate solution with a modulus of 2.38 and residue.
[0070] 6) Take 50 ml of the sodium silicate solution with a modulus of 2.38 in 5) and add 65 ml of distilled water to dilute it. Adjust its pH to 6.8 at 90°C and age it for 2 hours. Then filter and wash it. Dry and grind the filter residue at 105°C to obtain 3.34 g of white powder, which is confirmed to be white carbon black after XRD test. The whiteness of the white carbon black product prepared under this condition is 95 and the specific surface area is 189.662 m 2 / g, DBP oil absorption value is 2.356ml / g.
[0071] After determining the aluminum and iron contents in the filtrate obtained after acid leaching, it was found that the leaching rates of aluminum and iron elements were 68.7% and 87.2% respectively, and the turbidity removal rate of simulated wastewater was 94.4%. The final measured aluminum oxide content of the obtained solid polyaluminum ferric chloride was 30.02%, which met the HG / T5359-2018 content standard.
[0072] Embodiment 3
[0073] This embodiment provides a method for preparing white carbon black and co-producing polyaluminium ferric chloride from gold mine tailings. The method comprises the following steps:
[0074] 1) The gold tailings were crushed and passed through a 100-mesh sieve to obtain powdered gold tailings. 12 g of the gold tailings powder was calcined at 600° C. and kept warm for 2.5 h to obtain calcined slag.
[0075] 2) Take 10 g of the calcined gold tailings powder in 1) and add it to 35 ml of 20% hydrochloric acid, place it in a water bath at 105° C. for 2 h, and filter to obtain a filtrate and a residue.
[0076] 3) Take the filtrate obtained in 2), add distilled water to 100 ml, add 0.0286 g of anhydrous AlCl3 to make its Al:Fe molar ratio 3:1, and at the same time add an appropriate amount of NaOH to make its alkalinity 1, separate and purify the solution, microwave heat to 60°C at a power of 500 W for polymerization for 0.5 h, and age for 20 h to obtain a polyaluminum ferric chloride solution. After the solution is evaporated and dried, solid polyaluminum ferric chloride can be obtained.
[0077] 4) Take 5 g of the filter residue obtained in 2), wash it with water until neutral and dry it, then mix and grind it with 6 g of NaOH, put the mixture into a muffle furnace and keep it at 650° C. for 2 h to obtain 10.12 g of alkali-melted slag;
[0078] 5) Take 10 g of the alkali-melted slag in 4) into a 250 ml beaker, add 70 ml of distilled water, stir in a 60°C water bath for 3 h, then age for 10 h, and filter to obtain 68 ml of a sodium silicate solution with a modulus of 1.94 and a residue.
[0079] 6) Take 50 ml of the sodium silicate solution with a modulus of 1.94 in 5) and add 30 ml of distilled water to dilute it, adjust its pH to 6.9 at 60°C, age it for 2 hours, then filter and wash it, dry and grind the filter residue at 105°C to obtain 2.88 g of white powder, which is confirmed to be white carbon black after XRD test. The whiteness of the white carbon black product prepared under this condition is 95 and the specific surface area is 184.7 m 2 / g, DBP oil absorption value is 2.951ml / g.
[0080] By measuring the aluminum and iron contents in the filtrate obtained after acid leaching, it was found that the leaching rates of aluminum and iron elements were 59.7% and 79.4% respectively, and the turbidity removal rate of simulated wastewater was 88.2%. The final measured aluminum oxide content of the obtained solid polyaluminum ferric chloride was 27.8%, which met the HG / T 5359-2018 content standard.
[0081] Embodiment 4
[0082] This embodiment provides a method for preparing white carbon black and co-producing polyaluminium ferric chloride using gold mine tailings, which specifically comprises the following steps:
[0083] 1) The gold tailings were crushed and passed through a 100-mesh sieve to obtain powdered gold tailings. 12 g of the gold tailings powder was calcined at 700° C. and kept warm for 0.5 h to obtain calcined slag.
[0084] 2) Take 10 g of the calcined gold tailings powder in 1) and add it to 100 ml of 5% hydrochloric acid, place it in a water bath at 60° C. for 3 h, and filter to obtain a filtrate and a filter residue, respectively.
[0085] 3) Take the filtrate obtained in 2) and add distilled water to 100 ml, then add 2.187g of anhydrous AlCl3 to make the Al:Fe molar ratio of the solution 5:1, and at the same time add an appropriate amount of NaOH to make its alkalinity 1.5, then separate and purify the solution, microwave heat to 50°C at a power of 500W for polymerization for 1h, and age for 20h to obtain a polyaluminum ferric chloride solution, and evaporate the solution to dryness to obtain solid polyaluminum ferric chloride.
[0086] 4) 5 g of the acid leaching residue obtained in 2) was mixed with 8.5 g of NaOH and ground. The mixture was placed in a muffle furnace and kept at 600° C. for 2 h to obtain 12.41 g of alkali-melted slag.
[0087] 5) Take 10 g of the alkali-melted slag in 4) and add 30 ml of distilled water to a 250 ml beaker. Stir in a 50°C water bath for 2 h, then age for 12 h, and filter to obtain 29 ml of a sodium silicate solution with a modulus of 2.1 and a residue.
[0088] 6) Take 50 ml of the sodium silicate solution with a modulus of 2.1 in 5) and add 70 ml of distilled water to dilute it. Adjust its pH to 7.2 at 50°C and age it for 2 hours. Then filter and wash it. Dry and grind the filter residue at 105°C to obtain 2.97 g of white powder, which is determined to be white carbon black by XRD analysis. Under this condition, the whiteness of the white carbon black product is 93 and the specific surface area is 202.6312 m 2 / g, DBP oil absorption value is 2.6114ml / g.
[0089] By measuring the aluminum and iron contents in the filtrate obtained after acid leaching, it was found that the leaching rates of aluminum and iron elements were 36.7% and 66.4% respectively, and the turbidity removal rate of simulated wastewater was 89.4%. The final measured aluminum oxide content of the obtained solid polyaluminum ferric chloride was 28.4%, which met the HG / T 5359-2018 content standard.
[0090] Embodiment 5
[0091] This embodiment provides a method for preparing white carbon black and co-producing polyaluminium ferric chloride using gold mine tailings, which specifically comprises the following steps:
[0092] 1) The gold tailings were crushed and passed through a 100-mesh sieve to obtain powdered gold tailings. 12 g of the gold tailings powder was calcined at 850° C. and kept warm for 2 h to obtain calcined slag.
[0093] 2) Take 10 g of the calcined gold tailings powder in 1) and add it to 50 ml of 30% hydrochloric acid, place it in a water bath at 110° C. for 1 hour, and filter to obtain a filtrate and a filter residue, respectively.
[0094] 3) Take the filtrate obtained in 2), add distilled water to 100 ml, add 4.371 g of anhydrous AlCl3 to make the Al:Fe molar ratio of the solution 7:1, and at the same time add an appropriate amount of NaOH to make its alkalinity 1.2, then separate and purify the solution, microwave heat to 100°C at a power of 500 W for polymerization for 3 hours, and age for 20 hours to obtain a polyaluminum ferric chloride solution. After the solution is evaporated and dried, solid polyaluminum ferric chloride can be obtained.
[0095] 4) 5 g of the filter residue obtained in 2) was washed and dried, and then mixed and ground with 9 g of NaOH. The mixture was placed in a muffle furnace and kept at 700° C. for 1 h to obtain 13.27 g of alkali-melted slag;
[0096] 5) Take 10 g of the alkali-melted slag in 4) and add 70 ml of distilled water to a 250 ml beaker. Stir in a water bath at 80°C for 0.5 h, then age for 6 h, and filter to obtain 68 ml of a sodium silicate solution with a modulus of 2.04 and a residue.
[0097] 6) Take 50 ml of the sodium silicate solution with a modulus of 2.04 in 5) and add 50 ml of distilled water to dilute it, adjust its pH to 7.0 at 80°C, age it for 2 hours, then filter and wash it, dry and grind the filter residue at 105°C to obtain 3.04 g of white powder, which was confirmed to be white carbon black after XRD testing.
[0098] Under this condition, the whiteness of the white carbon black product is 93 and the specific surface area is 196.2594m 2 / g, DBP oil absorption value is 2.4223ml / g.
[0099] By measuring the aluminum and iron contents in the filtrate obtained after acid leaching, it was found that the leaching rates of aluminum and iron elements were 68.4% and 92% respectively, and the turbidity removal rate of simulated wastewater was 91.4%. The final measured aluminum oxide content of the obtained solid polyaluminum ferric chloride was 29.6%, which met the HG / T 5359-2018 content standard.
[0100] The embodiments described above are only preferred technical solutions of the present invention and should not be regarded as limitations of the present invention. The embodiments and features in the embodiments of the present application can be arbitrarily combined with each other without conflict. The protection scope of the present invention shall be the technical solutions recorded in the claims, including the equivalent replacement solutions of the technical features in the technical solutions recorded in the claims. That is, equivalent replacement improvements within this scope are also within the protection scope of the present invention.
Claims
1. A method for preparing white carbon black and co-producing polyaluminium ferric chloride using gold mine tailings, characterized in that: The following steps are involved: The gold mine tailings are crushed and screened step by step, and finally calcined and activated to obtain the pre-treated gold mine tailings; The pretreated gold tailings are mixed with hydrochloric acid, and after sufficient reaction, solid-liquid separation is performed to obtain an acid leaching solution rich in aluminum and iron elements and an acid leaching residue rich in silicon dioxide; Controlling the ratio of aluminum and iron elements in the acid leaching solution rich in aluminum and iron elements, adjusting the alkalinity of the acid leaching solution rich in aluminum and iron elements, and then performing microwave thermal polymerization to obtain polyaluminum ferric chloride; The acid leaching residue rich in silicon dioxide is subjected to alkali melting treatment to obtain alkali melted residue; The alkali-melted slag is dissolved in water and aged in a water bath, and then solid-liquid separation is performed to obtain a sodium silicate solution; After diluting the sodium silicate solution, adjusting the pH value of the diluted sodium silicate solution, and finally aging, filtering, washing, drying and grinding in sequence to obtain white carbon black; The temperature of the microwave thermal polymerization is 50° C. to 100° C., the power of the microwave thermal polymerization is 500 W, and the insulation time of the microwave thermal polymerization is 0.5 h to 3 h; When the acid leaching residue rich in silicon dioxide is subjected to alkali melting treatment, the acid leaching residue rich in silicon dioxide and sodium hydroxide are subjected to alkali melting treatment at a mass ratio of 1: (1-3); The temperature of the alkali melting treatment is 500°C to 700°C.
2. The method for preparing white carbon black and co-producing polyaluminium ferric chloride by using gold mine tailings according to claim 1, characterized in that: The temperature of the calcination activation is 600° C. to 1000° C., and the insulation time of the calcination activation is 0.5 h to 3 h.
3. The method for preparing white carbon black and co-producing polyaluminium ferric chloride by using gold mine tailings according to claim 1, characterized in that: The concentration of the hydrochloric acid is 5% to 30%.
4. The method for preparing white carbon black and co-producing polyaluminium ferric chloride by using gold mine tailings according to claim 1, characterized in that: The pretreated gold tailings are mixed with hydrochloric acid at a solid-liquid ratio of 1 g: (3-10) mL; The full reaction is carried out at a temperature of 60°C to 110°C.
5. The method for preparing white carbon black and co-producing polyaluminium ferric chloride by using gold mine tailings according to claim 1, characterized in that: The molar ratio of aluminum and iron in the acid leaching solution rich in aluminum and iron is controlled to be aluminum: iron = (3-10): 1; The alkalinity of the acid leaching solution rich in aluminum and iron elements is adjusted to 0.1-1.
5.
6. The method for preparing white carbon black and co-producing polyaluminium ferric chloride by using gold mine tailings according to claim 1, characterized in that: When the alkali-melted slag is subjected to water dissolution aging in a water bath, the alkali-melted slag and distilled water are dissolved in water at a solid-liquid ratio of 1 g: (3-10) mL; The temperature of the alkali slag water bath is 50°C to 110°C, and the water bath time is 0.5h to 3h; The aging time of the alkali-melted slag in water bath is 6h~20h.
7. The method for preparing white carbon black and co-producing polyaluminium ferric chloride by using gold mine tailings according to claim 1, characterized in that: The mass fraction of silicon dioxide in the diluted sodium silicate solution is 0.5% to 7%; The pH value of the sodium silicate solution after adjustment and dilution is 6.8-7.2; The temperature for adjusting the pH value of the diluted sodium silicate solution is 50°C to 90°C.
8. A method for preparing white carbon black and co-producing polyaluminium ferric chloride using gold mine tailings, characterized in that: The method for preparing white carbon black and co-producing polyaluminium ferric chloride by using gold mine tailings as described in any one of claims 1 to 7 is adopted.