A kind of degradable plastic and its preparation method and its application in improving acidified soil

By using degradable plastic films or particles modified with degradable plastic matrix and alkaline materials, the problem of soil acidification is solved, significantly improving soil pH value and reducing harmful ion content, improving soil health, and achieving the dual effect of soil improvement.

CN117700960BActive Publication Date: 2024-12-06ZHEJIANG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311719042.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-14
Publication Date
2024-12-06
Estimated Expiration
2043-12-14

AI Technical Summary

Technical Problem

Soil acidification poses a threat to 40% of the world's farmland and 70% of potential farmland, affecting soil ecosystems and crop growth. It is difficult for existing technology to effectively improve acidic soil, increase soil pH and reduce harmful ion content.

Method used

Use a degradable plastic matrix with alkaline materials such as egg shell powder and calcium carbide slag, and add titanium dioxide for modification and treatment, and prepare it into a degradable plastic film or granules, covering it on acidic soil, and then blown by heating, melting and extrusion and granulation. Film forming or crushing, used for soil improvement.

Benefits of technology

Significantly increase the soil pH value, reduce the exchangeable hydrogen and aluminum content, improve soil health, achieve effective improvement of acidified soil, and improve soil fertility and crop yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117700960B_ABST
    Figure CN117700960B_ABST
Patent Text Reader

Abstract

The invention discloses a degradable plastic, a preparation method and an application in acidified soil improvement, and belongs to the technical field of degradable plastic in agricultural soil improvement. The degradable plastic includes 40-60 parts of a degradable plastic base, 5-50 parts of an alkaline material, 10-30 parts of a plasticizer and 1-2 parts of titanium dioxide in percentage by mass. The present invention adopts a degradable plastic matrix to cooperate with alkaline materials such as harmless waste eggshells and carbide slag, and uses titanium dioxide for modification to accelerate the photolysis rate of the plastic, prepare it into a plastic film, or process it into particles or powder (including recycling the plastic residual film of the present invention that has not been degraded in time after agricultural use to prepare it into particles or powder), cover the acidic soil with a plastic film or directly apply plastic particles or powder, which can significantly improve the soil pH value, reduce the content of exchangeable hydrogen and exchangeable aluminum, etc., thereby achieving the improvement of acidified soil.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of agricultural soil improvement using degradable plastics, and relates to a degradable plastic, a preparation method and application in acidified soil improvement. Background Art

[0002] Soil acidification refers to the process by which, under the influence of a humid climate, soil absorptive complexes accept a certain amount of exchangeable hydrogen or aluminum ions, leading to the leaching of alkaline (base) ions from the soil. Alternatively, due to human influence, acidic substances in the soil increase, soil pH decreases, and the soil becomes acidic or strongly acidic. Soil acidification is a form of land degradation affecting 40% of farmland and over 70% of potential farmland worldwide. In recent years, human activities such as acid deposition and excessive nitrogen fertilizer application have exacerbated soil acidification, posing a significant threat to soil ecosystems. Soil acidification can affect the activity of soil organisms, alter the form of nutrients in the soil, reduce nutrient availability, and promote the dissolution of free manganese and aluminum ions into the soil solution, which can be toxic to crops. Therefore, strengthening the improvement of acidified soils and improving the quality of cultivated land are crucial for maintaining soil health.

[0003] Traditional agricultural production processes add alkaline substances such as quicklime, slaked lime, limestone, and dolomite, containing calcium and magnesium oxides, hydroxides, and carbonates, to acidic soils to maintain or increase soil pH. Currently, plastic film mulching technology, combined with traditional agronomy, is being applied to various crop cultivations, demonstrating advantages in increasing temperature, yield, and income. Therefore, given the widespread agricultural application of plastic film, there is a need to develop a biodegradable plastic that can serve both agricultural production and the amelioration of acidified soils. Summary of the Invention

[0004] The purpose of the present invention is to overcome the defects in the prior art and provide a degradable plastic and a preparation method and application in improving acidified soil.

[0005] The specific technical solutions adopted in the present invention are as follows:

[0006] In a first aspect, the present invention provides a degradable plastic comprising, by mass percentage, 40 to 60 parts of a degradable plastic base, 5 to 50 parts of an alkaline material, 10 to 30 parts of a plasticizer, and 1 to 2 parts of titanium dioxide.

[0007] Preferably, the degradable plastic base is at least one of polybutylene succinate resin, polylactic acid, polyhydroxyalkanoate, polyvinyl alcohol and polyvinyl chloride.

[0008] Preferably, the alkaline material is eggshell powder and / or carbide slag.

[0009] Furthermore, when the alkaline material is eggshell powder, the number of parts is 5 to 20 parts; when the alkaline material is carbide slag, the number of parts is 10 to 30 parts.

[0010] Preferably, the particle size of the alkaline material is less than 150 μm.

[0011] In a second aspect, the present invention provides a method for preparing a degradable plastic, as follows:

[0012] 40-60 parts of a degradable plastic base, 5-50 parts of an alkaline material, 10-30 parts of a plasticizer and 1-2 parts of titanium dioxide are mixed uniformly in percentage by mass, then heated and melted at 180-220° C., and extruded and granulated to obtain a degradable plastic.

[0013] Preferably, the heating and melting is carried out in the barrel of a twin-screw extruder.

[0014] In a third aspect, the present invention provides a use of any of the degradable plastics described in the first aspect or the degradable plastics obtained by the preparation method described in the second aspect in improving acidified soil, as follows:

[0015] S1: Grind and sieve the acidified soil to be treated, and then add water to keep the maximum field water holding capacity of the soil at 40% to 70%;

[0016] S2: forming the degradable plastic into a film by blow molding and covering the surface of the acidified soil treated in step S1, or mixing the degradable plastic particles or powder with the acidified soil treated in step S1;

[0017] S3: Cultivating the acidified soil treated in step S2 at room temperature and natural light for at least 30 days to complete the improvement of the acidified soil.

[0018] Preferably, the particle size of the acidified soil after grinding and sieving is less than 2 mm.

[0019] Preferably, in step S2, the thickness of the degradable plastic after film blowing is 0.1 mm; the degradable plastic particles or powder are mixed with the soil in an amount of 0.1% to 0.5% of the dry weight of the acidified soil to be treated.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] The present invention uses a degradable plastic matrix in combination with alkaline materials such as harmless waste eggshells and carbide slag, and uses titanium dioxide for modification to accelerate the photolysis rate of the plastic, to prepare it into a plastic film, or process it into particles or powder (including recycling the plastic residual film of the present invention that has not been degraded in time after agricultural use to prepare it into particles or powder). Covering the acidic soil with plastic film or directly applying plastic particles or powder can significantly increase the soil pH value and reduce the content of exchangeable hydrogen and exchangeable aluminum, thereby achieving the improvement of acidified soil. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 Electron microscopic image of degradable plastic in Example 1;

[0023] Figure 2 Electron microscopy image of the degradable plastic in Example 2. DETAILED DESCRIPTION

[0024] The present invention will be further described and illustrated below with reference to the accompanying drawings and specific embodiments. The technical features of each embodiment of the present invention may be combined accordingly, provided that there is no conflict between them.

[0025] The invention provides a degradable plastic, which mainly comprises, by mass percentage, 40-60 parts of a degradable plastic base, 5-50 parts of an alkaline material, 10-30 parts of a plasticizer and 1-2 parts of titanium dioxide.

[0026] In actual use, the biodegradable plastic base can be at least one of polybutylene succinate resin, polylactic acid, polyhydroxyalkanoate, polyvinyl alcohol, and polyvinyl chloride. The alkaline material can be at least one of eggshell powder and carbide slag. When eggshell powder is used as the alkaline material, the proportion is 5 to 20 parts; when carbide slag is used as the alkaline material, the proportion is 10 to 30 parts. The particle size of the alkaline material (eggshell powder and / or carbide slag) is preferably less than 150 μm.

[0027] Based on the above-mentioned degradable plastic, the present invention also provides a preparation method, which is as follows:

[0028] 40-60 parts of a degradable plastic base, 5-50 parts of an alkaline material, 10-30 parts of a plasticizer and 1-2 parts of titanium dioxide are mixed uniformly (this can be done in a blender), then heated and melted at 180-220°C (this can be done in the barrel of a twin-screw extruder), and extruded and granulated to obtain a degradable plastic, which can then be blown into a film or crushed into granules or powder for use as needed.

[0029] When using the above-mentioned degradable plastics for improving acidified soil, the following steps can be followed:

[0030] S1: After the acidified soil to be treated is ground and sieved (for example, through a 2 mm sieve), water (distilled water may be used) is added to maintain the maximum field water holding capacity of the soil at 40% to 70%.

[0031] S2: Blowing the degradable plastic of the present invention into a film (the thickness can be 0.1 mm) and covering it on the surface of the acidified soil treated in step S1, or mixing the degradable plastic particles or powder of the present invention with the acidified soil treated in step S1 (here, the residual degradable plastic film of the present invention that has not been degraded in time after agricultural use can also be recycled and processed into particles or powder for use, thereby improving the recycling rate).

[0032] In actual application, the degradable plastic particles or powder are mixed with the soil according to 0.1% to 0.5% of the dry weight of the acidified soil to be treated.

[0033] S3: Cultivate the acidified soil treated in step S2 at room temperature and natural light for at least 30 days (generally 30 to 90 days) to complete the improvement of the acidified soil.

[0034] Example 1

[0035] This embodiment provides a method for preparing a degradable plastic and its application in reducing acidity and controlling aluminum in acidified soil, comprising the following steps:

[0036] (1) 20 parts of polylactic acid, 27 parts of polyhydroxyalkanoate, 12 parts of eggshell powder, 20 parts of calcium carbide slag, 20 parts of plasticizer, and 1 part of titanium dioxide were mixed uniformly in a mixer, added to the barrel of a twin-screw extruder, heated and melted at 200°C, extruded into granules, and then blown into film to obtain a finished film with a thickness of 0.1 mm.

[0037] like Figure 1 As shown in FIG, it is an electron microscope image of the degradable plastic prepared in this embodiment. It can be seen from the image that the surface ductility of the degradable plastic is good, and some areas show a certain pore structure due to the addition of alkaline substances.

[0038] (2) The degradable plastic film prepared in this example was covered on the surface of acidified soil with a soil pH of 5.23 and a maximum field water holding capacity of 45%. The soil was then cultured at room temperature and under natural light for 90 days. After the experiment, it was found that the plastic film was degraded by 63%, and the pH value of the covered surface soil increased to 5.47.

[0039] Example 2

[0040] This embodiment provides a method for preparing a degradable plastic and its application in reducing acidity and controlling aluminum in acidified soil, comprising the following steps:

[0041] (1) 40 parts of polyvinyl chloride, 10 parts of eggshell powder, 29 parts of calcium carbide slag, 20 parts of plasticizer and 1 part of titanium dioxide are mixed uniformly in a mixer, added into the barrel of a twin-screw extruder, heated and melted at 190° C., extruded into granules, and crushed to a particle size of less than 250 μm to obtain biodegradable plastic powder.

[0042] like Figure 2 As shown in FIG, it is an electron microscope image of the degradable plastic prepared in this embodiment. It can be seen from the image that the degradable plastic is granular and has diverse surface morphology and structure.

[0043] (2) Two acidified soils A and B to be treated were selected. Properties of soil A: pH 5.39, exchangeable hydrogen 0.37 cmol / kg, exchangeable aluminum 0.16 cmol / kg; properties of soil B: pH 5.08, exchangeable hydrogen 0.86 cmol / kg, exchangeable aluminum 0.12 cmol / kg. To simulate the cumulative effect of long-term use of plastic film, the degradable plastic powder prepared in this example was added to soils A and B at 0.1%, 0.2%, and 0.5% of the soil dry weight, respectively. The soil had a maximum field water holding capacity of 60%, and was incubated at room temperature under natural light for 30 days. After incubation, the soil was air-dried and ground through a 2 mm sieve, and the soil pH, exchangeable hydrogen, and aluminum content were measured. The results showed that the addition of degradable plastic powder increased the pH values ​​of soils A and B by 0.36 to 1.17 and 0.30 to 1.24 units, respectively. The exchangeable hydrogen and aluminum contents in soils A and B decreased significantly, with the high addition levels remaining below the detection limit. Table 1 shows the soil pH, exchangeable hydrogen, and aluminum contents after treatment with degradable plastic powder.

[0044] Table 1 Soil pH, exchangeable hydrogen and aluminum content after treatment with degradable plastic powder

[0045]

[0046] Note: ND, No detection, not detected.

[0047] Example 3

[0048] This embodiment provides a method for preparing a degradable plastic and its application in reducing acidity and controlling aluminum in acidified soil, comprising the following steps:

[0049] (1) 60 parts of polylactic acid, 20 parts of eggshell powder, 19 parts of plasticizer and 1 part of titanium dioxide were mixed uniformly in a mixer, added to the barrel of a twin-screw extruder, heated and melted at 190°C, extruded into granules, and crushed to a particle size of less than 250 μm to obtain biodegradable plastic powder.

[0050] (2) The test soil had a pH of 5.05, exchangeable hydrogen of 0.59 cmol / kg, and exchangeable aluminum of 0.24 cmol / kg. Biodegradable plastic powder was added to the acidic soil at a maximum field capacity of 60% at room temperature under natural light for 30 days. After incubation, the soil was air-dried and ground through a 2 mm sieve. The soil pH after treatment with biodegradable plastic powder increased to 5.57, exchangeable hydrogen decreased to 0.11 cmol / kg, and exchangeable aluminum decreased to 0.05 cmol / kg.

[0051] Example 4

[0052] This embodiment provides a method for preparing a degradable plastic and its application in reducing acidity and controlling aluminum in acidified soil, comprising the following steps:

[0053] (1) 55 parts of polylactic acid, 29 parts of carbide slag, 14 parts of plasticizer and 2 parts of titanium dioxide were mixed uniformly in a mixer, added to the barrel of a twin-screw extruder, heated and melted at 190° C., extruded into granules, and crushed to a particle size of less than 250 μm to obtain biodegradable plastic powder.

[0054] (2) The test soil had a pH of 5.05, exchangeable hydrogen of 0.59 cmol / kg, and exchangeable aluminum of 0.24 cmol / kg. Biodegradable plastic powder was added to the acidic soil at a maximum field capacity of 60% at room temperature under natural light for 30 days. After incubation, the soil was air-dried and ground through a 2 mm sieve. The soil pH after treatment with biodegradable plastic powder increased to 5.87, exchangeable hydrogen decreased to 0.02 cmol / kg, and exchangeable aluminum was below the detection limit.

[0055] The embodiment described above is merely a preferred embodiment of the present invention and is not intended to limit the present invention. Persons skilled in the art may make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, any technical solution obtained by equivalent substitution or equivalent transformation falls within the scope of protection of the present invention.

Claims

1. An application of degradable plastic in improving acidified soil, characterized in that: The details are as follows: S1: Grind and sieve the acidified soil to be treated, and add water to keep the maximum field water holding capacity of the soil at 40%~70%; S2: mixing the degradable plastic particles or powder with the acidified soil treated in step S1; S3: Cultivating the acidified soil treated in step S2 at room temperature and natural light conditions for at least 30 days to complete the improvement of the acidified soil; The particle size of the acidified soil after grinding and sieving is less than 2 mm; The degradable plastic comprises, by mass percentage, 40-60 parts of a degradable plastic base, 10-30 parts of an alkaline material, 10-30 parts of a plasticizer, and 1-2 parts of titanium dioxide; The degradable plastic base is at least one of polylactic acid, polyhydroxyalkanoate and polyvinyl alcohol; the alkaline material is carbide slag; The degradable plastic particles or powder are mixed with the soil according to 0.1% to 0.5% of the dry weight of the acidified soil to be treated.

2. The use of the degradable plastic in improving acidified soil according to claim 1, characterized in that: The particle size of the alkaline material is less than 150 μm.

3. The use of the degradable plastic in improving acidified soil according to claim 1, characterized in that: The preparation method of the degradable plastic is as follows: 40-60 parts of a degradable plastic base, 10-30 parts of an alkaline material, 10-30 parts of a plasticizer and 1-2 parts of titanium dioxide are uniformly mixed in percentage by mass, then heated to melt at 180-220° C., and extruded and granulated to obtain a degradable plastic.

4. The use of the degradable plastic in improving acidified soil according to claim 3, characterized in that: The heating and melting is carried out in the barrel of a twin-screw extruder.