A high-efficiency N-type back-contact solar cell preparation process
By adopting a low-cost process flow in the preparation process of N-type back contact solar cells and optimizing the passivation film structure and metal contact area design, the problems of high cost and complex process in the existing technology are solved, and high efficiency and low cost are achieved. The preparation of N-type back contact batteries improves the conversion efficiency and cost-effectiveness of the battery.
Patent Information
- Application Number
- CN202311834474.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-28
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-12-28
AI Technical Summary
The preparation process of existing N-type back contact solar cells is high-cost and complex, making it difficult to achieve high efficiency in industrialization. In particular, there are great challenges between improving conversion efficiency and reducing costs.
A low-cost process is adopted, including double-sided polishing of N-type silicon wafers, boron diffusion, phosphorus diffusion, thermal oxidation, silicon nitride and aluminum oxide film deposition, laser patterning, and deposition of silicon oxide and doped polysilicon layers. And printing silver aluminum paste to form P/N interdigitated interlaced patterns and different passivation film structures to improve battery efficiency.
By optimizing the passivation film structure and the design of the metal contact area, the conversion efficiency and cost-effectiveness of the battery are improved, achieving efficiency comparable to that of Sunpower's bipolar contact passivation battery, while reducing process complexity and cost.
Smart Images

Figure CN117712229B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a high-efficiency N-type back-contact solar cell preparation process, belongs to the technical field of solar photovoltaic power generation, and is particularly suitable for the production and manufacture of solar photovoltaic cells. Background Art
[0002] Back-contact solar cells are a type of cell structure where both the positive and negative electrodes are on the back and there is no grid line on the front. Generally, the cell conversion efficiency is high, but the process is difficult and the cost is relatively high, which limits its development to a certain extent. In recent years, with the application of contact passivation technology, the cell conversion efficiency has been greatly improved, and the open circuit voltage and fill factor have almost reached the theoretical limit. It is becoming increasingly difficult to further improve the cell efficiency. Since there is no grid line blocking the front of the back contact, the short-circuit current will be greatly increased. In addition, the back-contact cell has single-sided high efficiency, unique appearance, and is easier to lighten, which makes it more suitable for distributed photovoltaic systems. The industry has set off a research boom on back-contact cells.
[0003] There are many types of back-contact battery structures. Which structural design can be industrialized depends on its cost and conversion efficiency. Different structural designs have different process complexity and efficiency. The industrialized back-contact batteries include those based on N-type silicon wafers, represented by Sunpower and Aixu. The metallization is achieved by electroplating, and both the positive and negative electrodes are contact passivated, which is relatively expensive. The process of the Yellow River Hydropower Company requires low-temperature silver paste, which is relatively expensive and has a complex process flow. The other type is based on P-type silicon wafers, represented by Longi. Since the positive electrode uses aluminum paste, the cost is relatively low, and the efficiency is comparable to the current mainstream N-type batteries such as N-TOPCon and HJT batteries. It is difficult to further improve the efficiency. Summary of the invention
[0004] Purpose of the invention: In view of the problems and shortcomings in the prior art, the present invention proposes a preparation process for an efficient N-type back-contact battery, which realizes the preparation process of an efficient N-type back-contact battery in a low-cost manner. The process flow is highly compatible with the current N-TOPCon battery, has low cost, and its efficiency is comparable to that of the bipolar contact passivation batteries of Sunpower and Aixu.
[0005] Technical solution: A process for preparing a high-efficiency N-type back contact cell, comprising the following steps:
[0006] Step 1, performing double-sided polishing on the N-type silicon wafer;
[0007] Step 2: Boron diffusion is performed on the N-type silicon wafer in a high-temperature furnace tube to form p + layer;
[0008] Step 3, performing single-sided texturing on the non-boron diffusion surface of the N-type silicon wafer;
[0009] Step 4, diffusing phosphorus on the textured surface of the N-type silicon wafer;
[0010] Step 5, cleaning and removing the PSG / BSG layer on the front and back sides of the N-type silicon wafer;
[0011] Step 6, thermally oxidizing the N-type silicon wafer in a high temperature furnace;
[0012] Step 7, depositing silicon nitride on the front side of the N-type silicon wafer, depositing an aluminum oxide film on the back side, and stacking silicon nitride;
[0013] Step 8, patterning the N region of the back side of the N-type silicon wafer with a laser to form a P / N interdigitated pattern, and then etching and polishing the N region with the laser in an alkaline solution;
[0014] Step 9, depositing silicon oxide and doped polysilicon layers in sequence on the back side of the N-type silicon wafer by controlling the gas type and flow rate;
[0015] Step 10, etching in an alkaline solution to remove the front winding of the N-type silicon wafer;
[0016] Step 11, depositing silicon nitride on the back side of the N-type silicon wafer;
[0017] Step 12, opening the silicon nitride / doped polysilicon layer on the P region on the back side of the N-type silicon wafer;
[0018] Step 13, printing silver-aluminum paste on the P region of the N-type silicon wafer and printing silver paste on the N region.
[0019] In the step 1, an N-type silicon wafer with a resistivity of 0.3-3Ω.cm is selected and double-sided polishing is performed.
[0020] In step 2, BBr3 or BCl3 is used to diffuse boron into the silicon wafer in a high-temperature furnace tube to form p + layer.
[0021] In step 4, phosphorus is diffused on the textured surface, POCl3 is used as a diffusion source, and the high temperature diffusion is 800-950°C.
[0022] In step 6, the temperature in the high temperature furnace is 550-850°C.
[0023] In step 7, silicon nitride is deposited on the front side of the N-type silicon wafer by PECVD, and an aluminum oxide film is deposited on the back side by ALD / PECVD or the like, and silicon nitride is superimposed.
[0024] In step 9, PECVD, LPCVD, PVD, APCVD, etc. are used to sequentially deposit silicon oxide and doped polysilicon layers on the back side by controlling the gas type and flow rate. The thickness of the deposited silicon oxide is 0.5-2nm, and the thickness of the doped polysilicon is 50-400nm.
[0025] Beneficial effects: Compared with the prior art, the high-efficiency N-type back-contact solar cell preparation process provided by the present invention has the following advantages:
[0026] (1) Through the design of the front surface field and the contact passivation structure of silicon oxide + doped polysilicon layer, the collection of back-side carriers is increased, thus improving the battery conversion efficiency;
[0027] (2) In step 9, the back N region adopts the same contact passivation structure as the N-TOPCon battery. In step 2, the back P region adopts the same structure as the front N-TOPCon. Combined with laser induced sintering, the recombination of the metal contact area is reduced. Compared with N-TOPCon, the cost is not increased, but the positive electrode of N-TOPCon is moved to the back. There is no light shielding on the front, the current will increase significantly, and the conversion efficiency will be improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 is a process flow chart of an embodiment of the present invention;
[0029] Figure 2 It is a schematic diagram of the structure of a solar cell realized by the process of an embodiment of the present invention. DETAILED DESCRIPTION
[0030] The present invention is further explained below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. After reading the present invention, various equivalent forms of modifications to the present invention by those skilled in the art all fall within the scope defined by the claims attached to this application.
[0031] like Figure 1 As shown, a preparation process of a high-efficiency N-type back contact battery includes the following steps:
[0032] Step 1, selecting an N-type silicon wafer with a resistivity of 0.3-3Ω.cm, and performing double-sided polishing on the N-type silicon wafer;
[0033] Step 2: Use BBr3 or BCl3 to diffuse boron into the N-type silicon wafer in a high-temperature furnace tube to form p + layer;
[0034] Step 3, single-sided texturing of the non-boron diffusion surface of the N-type silicon wafer is performed, using POCl3 as a diffusion source, and high-temperature diffusion at 800-950°C;
[0035] Step 4, diffusing phosphorus on the textured surface of the N-type silicon wafer;
[0036] Step 5, cleaning and removing the PSG / BSG layer on the front and back sides of the N-type silicon wafer;
[0037] Step 6, thermally oxidizing the N-type silicon wafer in a high temperature furnace at a temperature of 550-850° C.;
[0038] Step 7, silicon nitride is deposited on the front side of the N-type silicon wafer by PECVD, and aluminum oxide film is deposited on the back side by ALD / PECVD and other methods, and silicon nitride is superimposed;
[0039] Step 8, patterning the N region of the back side of the N-type silicon wafer with a laser to form a P / N interdigitated pattern, and then etching and polishing the N region with the laser in an alkaline solution;
[0040] Step 9, using PECVD, LPCVD, PVD, APCVD or the like to sequentially deposit silicon oxide and doped polysilicon layers on the back side of the N-type silicon wafer by controlling the type and flow of gas;
[0041] Step 10, etching in an alkaline solution to remove the front winding of the N-type silicon wafer;
[0042] Step 11, depositing silicon nitride on the back side of the N-type silicon wafer;
[0043] Step 12, opening the silicon nitride / doped polysilicon layer on the P region on the back side of the N-type silicon wafer;
[0044] Step 13, printing silver-aluminum paste on the P region of the N-type silicon wafer and printing silver paste on the N region.
[0045] like Figure 2 As shown, the solar cell uses an N-type silicon wafer as a substrate, and has an n+ region formed by phosphorus diffusion on the front side as the front surface field, and then uses a silicon oxide / silicon nitride laminated film for surface passivation and anti-reflection; the negative electrode P region on the back of the battery is a p+ layer formed by boron diffusion, and uses an aluminum oxide / silicon nitride laminated film on the surface, and the positive electrode N region uses a silicon oxide / doped polysilicon contact passivation structure, and the surface uses a silicon oxide / silicon nitride laminated structure for passivation and anti-reflection. The negative electrode is silver aluminum paste, and the positive electrode material is silver paste.
Claims
1. A process for preparing a high-efficiency N-type back contact battery, characterized in that: The steps include: Step 1, performing double-sided polishing on the N-type silicon wafer; Step 2: Boron diffusion is performed on the N-type silicon wafer in a high-temperature furnace tube to form p + layer; Step 3, performing single-sided texturing on the non-boron diffusion surface of the N-type silicon wafer; Step 4, diffusing phosphorus on the textured surface of the N-type silicon wafer; Step 5, cleaning and removing the PSG / BSG layer on the front and back sides of the N-type silicon wafer; Step 6, thermally oxidizing the N-type silicon wafer in a high temperature furnace; Step 7, depositing silicon nitride on the front side of the N-type silicon wafer, depositing an aluminum oxide film on the back side, and stacking silicon nitride; Step 8, patterning the N region of the back side of the N-type silicon wafer with a laser to form a P / N interdigitated pattern, and then etching and polishing the N region with the laser in an alkaline solution; Step 9, depositing silicon oxide and N-type doped polysilicon layer in sequence on the back side of the N-type silicon wafer by controlling the gas type and flow rate; Step 10, etching and removing the plating on the front side of the N-type silicon wafer in an alkaline solution; Step 11, depositing silicon nitride on the back side of the N-type silicon wafer; Step 12, opening the silicon nitride / doped polysilicon layer on the P region on the back side of the N-type silicon wafer; Step 13, printing silver-aluminum paste on the P region of the N-type silicon wafer and printing silver paste on the N region.
2. The preparation process of a high-efficiency N-type back contact battery according to claim 1, characterized in that: In the step 1, an N-type silicon wafer with a resistivity of 0.3-3Ω.cm is selected and double-sided polishing is performed.
3. The preparation process of a high-efficiency N-type back contact battery according to claim 1, characterized in that: In step 2, BBr3 or BCl3 is used to diffuse boron into the silicon wafer in a high-temperature furnace tube to form p + layer.
4. The preparation process of a high-efficiency N-type back contact battery according to claim 1, characterized in that: In step 4, phosphorus is diffused on the textured surface, POCl3 is used as a diffusion source, and the high temperature diffusion is 800-950°C.
5. The preparation process of a high-efficiency N-type back contact battery according to claim 1, characterized in that: In step 6, the temperature in the high temperature furnace is 550-850°C.
6. The process for preparing a high-efficiency N-type back contact battery according to claim 1, characterized in that: In step 7, silicon nitride is deposited on the front side of the N-type silicon wafer by PECVD, and an aluminum oxide film is deposited on the back side by ALD / PECVD to overlay silicon nitride.
7. The process for preparing a high-efficiency N-type back contact cell according to claim 1, characterized in that: In step 9, PECVD, LPCVD, PVD, and APCVD are used to sequentially deposit silicon oxide and doped polysilicon layers on the back side by controlling the gas type and flow rate.
Citation Information
Patent Citations
A preparation method of a low-cost P-type all-back-electrode crystalline silicon solar cell
CN109244194A
Back contact solar cell with various tunnel junction structures and preparation method thereof
CN110838536A
Patterned passivation contact solar cell and manufacturing method thereof
CN112164728A
P-type double-sided PERC solar cell and preparation method and application thereof
CN113113510A
HBC solar cell with back passivation contact structure and preparation method of HBC solar cell
CN114242801A