A high-density, high-carbon cobalt-based alloy and its preparation method
By combining electron beam selective melting technology with preheating treatment, the forming problem of high-carbon cobalt-based alloys in laser selective melting and laser cladding technology has been solved, realizing the preparation of cobalt-based alloys with high density and high carbon content, meeting the application needs of aerospace, energy and power and other fields.
Patent Information
- Application Number
- CN202311780832.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-21
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-12-21
AI Technical Summary
In existing technologies, selective laser melting and laser cladding technologies face technical challenges in preparing high-carbon cobalt-based alloys, such as high sensitivity to carbon content, unavoidable cracks, and limited forming thickness. These challenges fail to meet the high density and mechanical performance requirements of fields such as aerospace and energy.
By employing electron beam selective melting technology combined with preheating treatment, and by strictly controlling the particle size, sphericity, and loose packing density of the powder, and by combining preheating with electron beam heating, a cobalt-based alloy with high density and high carbon content is prepared. This process controls the temperature gradient and material bonding force to avoid crack formation.
It has achieved crack-free forming of high-carbon cobalt-based alloys with a density of up to 98.89% and excellent mechanical properties. It can be used to prepare alloys with large size and complex geometry, and is suitable for aerospace, energy and power and other fields.
Smart Images

Figure CN117721349B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of additive manufacturing technology for metallic materials, and specifically relates to a cobalt-based alloy with high density and high carbon content and its preparation method. Background Technology
[0002] Cobalt-based alloys are a class of alloys that use cobalt as the main element, with the addition of significant amounts of nickel, chromium, tungsten, and small amounts of other elements to strengthen the matrix. Due to their high strength at high temperatures, good resistance to thermal fatigue, hot corrosion, and wear, and compared to nickel-based superalloys, cobalt-based alloys exhibit higher thermal conductivity and lower thermal expansion, making them widely used in aerospace, energy and power, shipbuilding, mining, and other industries.
[0003] Metal additive manufacturing technology refers to a manufacturing technology based on the discrete-stacking principle, using digital model files as a basis, and using software and CNC systems to stack special metal materials layer by layer through methods such as extrusion, sintering, melting, photopolymerization, and spraying to directly produce physical objects.
[0004] Currently, the most commonly used cobalt-based alloys in the additive manufacturing field are cobalt-chromium alloys, represented by CoCrMo materials. The melting technologies used are generally selective laser melting and laser cladding.
[0005] Among them, selective laser melting (SLM) technology meets the performance requirements, has high equipment and technology availability, low forming cost, and short cycle time, and is widely used in the preparation of cobalt-based alloys. However, SLM technology has limitations due to its limited preheating temperature (≤200℃) and excessively fast cooling and solidification rate (10... 6 Factors such as K / s result in significant residual stress during use, thus limiting its application to manufacturing cobalt-based alloys with low carbon content (≤0.35wt%) and excellent laser welding performance (primarily used in the medical field). However, it cannot form cobalt-based alloys with high carbon content (≥0.50wt%) and poor laser welding performance, resulting in a considerable number of microcracks or even macroscopic cracking.
[0006] Although laser cladding technology can achieve the forming of cobalt-based alloys with high carbon content (≥0.50wt%) and poor weldability by maintaining a certain preheating temperature through remelting, the material still shows a lot of microcracks once the cladding thickness increases and the temperature gradient rises, because the technology cannot achieve continuous preheating. Therefore, in actual use, the cladding thickness is generally maintained in the range of ≤3mm. This reason means that laser cladding technology can only be used for coatings of some cobalt-based alloys and cannot manufacture products or components of a certain thickness.
[0007] In summary, the laser selective melting forming technology and laser cladding technology currently widely used in the preparation of cobalt-based alloys both have technical challenges such as high sensitivity to carbon content, unavoidable cracks, and limited forming thickness. Further exploration is needed to explore the possibility of additive forming cobalt-based alloys with high carbon content using other technologies. Summary of the Invention
[0008] The present invention aims to overcome the shortcomings of the prior art and provide a cobalt-based alloy with high density and high carbon content and its preparation method, so as to solve the technical problems of cobalt-based alloys prepared in the prior art, such as high sensitivity to carbon content, unavoidable cracks, and limited forming thickness.
[0009] To achieve the above objectives, the present invention adopts the following technical solution:
[0010] A highly dense, high-carbon cobalt-based alloy, comprising the following components by mass fraction:
[0011] The alloy comprises 0.10 ≤ C ≤ 3.00 wt.%, 8.00 ≤ Cr ≤ 33.00 wt.%, Fe ≤ 5.00 wt.%, Mn ≤ 2.00 wt.%, Mo ≤ 30.00 wt.%, Ni ≤ 25.00 wt.%, Si ≤ 3.50 wt.%, W ≤ 15.00%, with the remainder being Co; the alloy is prepared using electron beam selective melting technology.
[0012] The alloy prepared in this invention incorporates a high carbon content, resulting in a cobalt-based alloy with high carbon content and high density. This cobalt-based alloy can be widely used in aerospace, energy, and power industries. Furthermore, by limiting the content of each component, the prepared alloy exhibits characteristics such as high density, absence of internal cracks, high mechanical properties, high hardness, and no technical limitations on forming thickness, effectively overcoming the technical shortcomings of existing laser cladding and selective laser melting technologies.
[0013] Preferably, the cobalt-based alloy comprises the following components by mass fraction:
[0014] 0.90≤C≤3.00wt.%, 28.00≤Cr≤30.00wt.%, Fe≤3.00wt.%, Mn≤0.50wt.%, Mo≤2.00wt.%, Ni≤3.00wt.%, 0.70≤Si≤1.55wt.%, 3.50≤W≤5.50%, the remainder being Co.
[0015] Preferably, the average grain size of the alloy is between 1 μm and 20 μm. More preferably, the average grain size of the alloy is between 1 μm and 5 μm. The smaller the grain size of the prepared alloy, the better the mechanical properties of the material.
[0016] The microstructure of the alloy prepared above is a mixture of equiaxed crystals, columnar crystals, and dendrites. The width of the primary dendrite branches is between 1 μm and 15 μm, and the length is between 0.03 mm and 1.5 mm. The tips of the secondary dendrites are smooth and spherical. More preferably, the microstructure of the alloy is a mixture of equiaxed crystals, columnar crystals, and a small amount of dendrites. The width of the primary dendrite branches is between 1 μm and 5 μm, and the length is between 0.01 mm and 0.2 mm. The tips of the secondary dendrites are smooth and spherical. The reduction in dendrite content, as well as the decrease in dendrite branch width and length, indicates a more uniform composition within the material. This reduces segregation, and fewer and smaller dendrites also result in fewer microcracks within the material, improving its mechanical properties and enhancing its suitability for engineering applications.
[0017] The hardness of the above alloy is 33-48 HRC; the room temperature tensile strength is 800-1300 MPa, the yield strength is 450-800 MPa, and the elongation is 5%-11%.
[0018] Furthermore, to achieve the above objectives, the present invention also provides a method for preparing a cobalt-based alloy with high density and high carbon content, comprising the following steps:
[0019] S1. The spherical powder is sieved, dried, and then filled into the manufacturing environment containing the matrix;
[0020] S2. Preheat the bottom of the substrate and / or the surrounding manufacturing environment;
[0021] S3. After starting the preheating, powder is spread on the substrate surface, and then the powder-spreading layer area is heated by electron beam scanning.
[0022] S4. The single-layer cobalt-based alloy is formed by electron beam scanning according to the set process parameters;
[0023] S5. After electron beam scanning, the forming area is kept warm for a certain period of time.
[0024] S6. Repeat steps S3 to S5 until the three-dimensional printing of the cobalt-based alloy component is completed;
[0025] S7. Perform subsequent processing on the three-dimensional components to obtain a near-fully dense cobalt-based alloy.
[0026] The technology for preparing spherical powder is any one or a combination of vacuum atomization powder preparation technology, rotating electrode powder preparation technology, plasma atomization powder preparation technology, and plasma spheroidization powder preparation technology.
[0027] In existing technologies, electron beam selective melting (EBM) is rarely used in cobalt-based alloys due to the highly restricted parameters of imported equipment and the low technological maturity of domestically produced equipment. Even when it is used, it is mostly applied to alloys with low carbon content and those used in the medical field. Its application in the preparation of high-carbon cobalt-based alloys results in low density, poor interlayer bonding, and extremely poor surface quality.
[0028] Unlike the medical field, cobalt-based alloys used in aerospace, energy, and power industries have higher requirements in terms of hardness, mechanical properties, and density. Currently, electron beam selective melting technology has not been successfully applied to prepare high-carbon alloys for use in aerospace, energy, and power industries.
[0029] This invention is the first to apply electron beam selective melting technology to the preparation of high-carbon cobalt-based alloys for applications in aerospace, energy, and power industries. The resulting alloys possess high hardness and superior mechanical properties, and their geometries can be designed to be more complex, offering broad application prospects and suitable for industrial-scale mass production. Compared to laser selective melting technology, it can achieve the forming of high-carbon cobalt-based alloys without introducing microcracks. Compared to laser cladding and arc additive manufacturing technologies, it can produce alloys with unlimited thickness.
[0030] During the research and development process, it was discovered that preheating can reduce the temperature gradient and thus reduce the risk of cracking. However, the reduction in temperature gradient caused by preheating is insufficient to enable crack-free forming of high-carbon cobalt-based alloys. Under the influence of preheating alone, the material will still form through-cracks that develop from the boundary.
[0031] Therefore, this invention, based on preheating, also has the following technical problems: the reduced temperature gradient brought about by preheating can only suppress crack growth to a limited extent, and is insufficient to prevent the generation of crack initiation. The material bonding strength is lower than the internal thermal stress of the material, and high-carbon cobalt-based alloys will still crack. Furthermore, the heating capacity of the heating element in the equipment itself is limited and cannot provide a substrate temperature sufficient to resolve cracking during molding. Therefore, considering the heating capacity of the equipment itself, it is necessary to use the electron beam itself as an energy source to heat a single layer of powder without sintering, so that the powder raw material reaches a high temperature of over 500°C before sintering.
[0032] In summary, the present invention uses a combination of preheating and electron energy beam heating, which can effectively ensure that the prepared cobalt-based alloy is not limited by thickness and will not have cracking problems.
[0033] The technical specifications of the spherical powder are as follows: particle size 10–300 μm, sphericity ≥70%, and loose density ≥4.10 g / cm³. 3The hollow powder content is ≤0.2%. More preferably, the particle size is 45–150 μm, the sphericity is ≥80%, and the bulk density is ≥4.30 g / cm³. 3 The hollow powder content is ≤0.1%. During alloy preparation, powder specifications are subject to very strict requirements to ensure better material properties.
[0034] Preferably, in step S2, the preheating temperature is 200–550°C. More preferably, the preheating temperature is 300–550°C.
[0035] Preheating temperature is extremely important in alloy preparation. If the preheating temperature is insufficient, even if electron beam heating is used, cracks will still exist in the prepared alloy.
[0036] Preferably, in step S3, the thickness of the powder layer is 0.03–0.2 mm. More preferably, the thickness of the powder layer is 0.03–0.1 mm.
[0037] Preferably, in step S3, the heating temperature is 500–1200°C. More preferably, the heating temperature is 950–1100°C.
[0038] Preferably, in step S3, the parameters for heating the powder layer area by electron beam scanning are: electron beam input current of 30-40mA, scanning speed of 20-22m / s, and scanning spacing of 0.5-1mm.
[0039] Preferably, in step S4, the process parameters are: input current of 5–50 mA; scanning speed of 0.5–10.5 m / s; and scanning spacing of 0.09–0.2 mm. More preferably, the input current is 10–15 mA; the scanning speed is 1–6 m / s; and the scanning spacing is 0.1–0.15 mm.
[0040] Preferably, in step S5, the heat preservation time is 5 to 20 seconds.
[0041] Preferably, in step S7, the post-processing includes, but is not limited to, auxiliary structure removal, heat treatment, surface treatment, repair, welding, and machining.
[0042] Preferably, in step S7, the dimensions of the three-dimensional component are: length ≥ 1.0 mm, width ≥ 1.0 mm, and height ≥ 1.0 mm.
[0043] ≥1.0mm.
[0044] Compared with the prior art, the present invention has the following beneficial effects:
[0045] 1. The cobalt-based alloy prepared by this invention has the characteristics of being crack-free, having unlimited forming thickness, high density, and fine grains, with a density of not less than 98.89%, which significantly improves the hardness and room temperature mechanical properties of additively manufactured cobalt-based alloys.
[0046] 2. This invention uses a combination of preheating and electron beam selective melting technology to prepare cobalt-based alloys, which can achieve the forming of cobalt-based alloys with larger size and more complex geometry. Compared with laser selective melting technology, it can achieve the forming of cobalt-based alloys with high carbon content and will not produce microcracks. At the same time, compared with laser cladding technology, it can prepare alloys with unlimited thickness.
[0047] 3. The alloy prepared by this invention possesses high mechanical and tribological properties, such as high hardness and strength, excellent adhesion and wear resistance, and outstanding resistance to cavitation erosion. These properties enable the alloy to be applied in various industries, especially in non-lubricated systems or high-temperature environments. Additive manufacturing further endows the alloy with the ability to be shaped into more complex and lighter structures. Therefore, the application scenarios of the alloy are compatible with various applications in aerospace, energy and power, shipbuilding, and mining industries. For example, the alloy can be efficiently used to manufacture various valve bodies, valves, valve seats, valves, blades, push rods, hooks, and other parts, and can operate in high-temperature and high-pressure environments. Attached Figure Description
[0048] Figure 1 This is an uncorroded metallographic photograph of the cobalt-based alloy in Example 1 of the present invention;
[0049] Figure 2 The image shows a metallographic photograph of the cobalt-based alloy in Example 1 of this invention after being etched with aqua regia.
[0050] Figure 3 The XRD pattern of the cobalt-based alloy in Example 2 of this invention;
[0051] Figure 4 This is an EBSD image of the cobalt-based alloy in Example 2 of the present invention;
[0052] Figure 5 This is a TEM image of the cobalt-based alloy in Example 2 of the present invention;
[0053] Figure 6 This is a diffraction photograph of the precipitated phase in the TEM image of the cobalt-based alloy in Example 2 of the present invention;
[0054] Figure 7 This is a diffraction photograph of the matrix in the TEM image of the cobalt-based alloy in Example 2 of the present invention;
[0055] Figure 8 This is an uncorroded metallographic photograph of the cobalt-based alloy in Comparative Example 1 of this invention;
[0056] Figure 9 The image shows a metallographic photograph of the cobalt-based alloy in Comparative Example 1 of this invention after being etched with aqua regia.
[0057] Figure 10Comparative images of porosity analysis of cobalt-based alloys under different input currents and scanning speeds;
[0058] Figure 11 This is a photograph of the macroscopic through-cracks generated in the cobalt-based alloy in Comparative Example 2 of this invention;
[0059] Figure 12 This is a diagram of the alloy that failed to be formed in Comparative Example 3 of this invention;
[0060] Figure 13 Metallographic photograph of the alloy in Comparative Example 3 of this invention;
[0061] Figure 14 This is a diagram of the alloy prepared in Comparative Example 5 of the present invention;
[0062] Figure 15 This is a metallographic photograph of the alloy in Comparative Example 5 of the present invention. Detailed Implementation
[0063] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings, embodiments, and comparative examples. It should be understood that the specific embodiments and comparative examples described herein are merely illustrative of the invention and are not intended to limit the invention.
[0064] Conversely, this invention encompasses any substitutions, modifications, equivalent methods, and solutions made within the spirit and scope of the invention as defined in the claims. Furthermore, to provide a better understanding of the invention, certain specific details are described in detail below. However, those skilled in the art will fully understand the invention even without these detailed descriptions.
[0065] Example 1
[0066] S1. Cobalt-based alloy rods are prepared into spherical powder using vacuum atomization powdering technology. The particle size range of the spherical powder is 45–105 μm, the sphericity is 88%, and the bulk density is 4.21 g / cm³. 3 The hollow pasta content was 0.06%.
[0067] S2. The spherical powder is dried in an environment with a vacuum degree not exceeding 10. —1 Pa, drying temperature is 80℃, drying time is 10h; after drying, the spherical powder is sieved in an argon atmosphere; then the sieved spherical powder is filled into the manufacturing environment containing the matrix, and the bottom of the matrix is preheated to 200℃.
[0068] S3. After starting the preheating, powder is spread on the substrate surface with a thickness of 0.09 mm. Then, the powder-spreading area is heated to 1100℃ by an electron beam. The electron beam heating parameters are: input current of 35 mA, scanning speed of 20 m / s, and scanning interval of 0.7 mm.
[0069] S4. Shape the slice file according to the set process parameters. The specific process parameters are: input current 10.4mA, scanning speed 1.2m / s.
[0070] S5. After processing, keep the formed area warm for 10 seconds.
[0071] S6. Repeat steps S3 to S5 until the printing of the 3D component is complete.
[0072] S7. Sandblast the three-dimensional component to obtain a 10mm×10mm×10mm cobalt-based alloy product.
[0073] The composition analysis of the cobalt-based alloy obtained in this embodiment is as follows: C = 1.15 wt.%, Cr = 28.95 wt.%, Si = 1.12 wt.%, W = 3.96 wt.%, Fe = 2.98 wt.%, Mo = 0.98 wt.%, Ni = 2.79 wt.%, Mn = 0.50 wt.%, with the balance being Co.
[0074] The cobalt-based alloy obtained in Example 1 has a density of 99.98%, a tensile strength of 967 MPa, a yield strength of 503 MPa, and an elongation of 5.5%.
[0075] The metallographic image of the alloy obtained in Example 1 is shown below. Figure 1 As shown, the obtained cobalt-based alloy is crack-free and has low porosity. By combining preheating with electron beam heating to reduce the temperature gradient, and by optimizing the electron beam scanning parameters, the problem of numerous macroscopic cracks generated when forming the alloy using techniques such as selective laser melting was solved.
[0076] The metallographic image of the alloy obtained in Example 1 after etching with aqua regia is shown below. Figure 2 As shown, the microstructure of the alloy is a mixture of equiaxed crystals, columnar crystals, and a small amount of dendrites. The width of the primary dendrite branches is between 1 μm and 5 μm, and the length is between 0.01 mm and 0.05 mm. The tips of the secondary dendrites are smooth and spherical. The alloy grains are fine, exhibiting excellent mechanical properties.
[0077] Example 2
[0078] S1. Cobalt-based alloy rods are prepared into spherical powder using vacuum atomization powdering technology. The particle size range of the spherical powder is 45–105 μm, the sphericity is 88%, and the bulk density is 4.21 g / cm³. 3 The hollow pasta content was 0.06%.
[0079] S2. The spherical powder is dried in an environment with a vacuum degree not exceeding 10. —1 Pa, drying temperature is 80℃, drying time is 10h; after drying, the spherical powder is sieved in an argon atmosphere; then the sieved spherical powder is filled into the manufacturing environment containing the matrix, and the bottom of the matrix is preheated to 200℃.
[0080] S3. After starting the preheating, powder is spread on the substrate surface with a thickness of 0.09 mm. Then, the powder-spreading area is heated to 1100℃ by an electron beam. The electron beam heating parameters are: input current of 35 mA, scanning speed of 20 m / s, and scanning interval of 0.7 mm.
[0081] S4. Shape the slice file according to the set process parameters. The specific process parameters are: input current 7.0mA, scanning speed 2.4m / s;
[0082] S5. After processing, keep the forming area warm for 20 seconds;
[0083] S6. Repeat steps S3 to S5 until the printing of the 3D component is complete;
[0084] S7. Sandblast the three-dimensional component to obtain a near-fully dense cobalt-based alloy product with a diameter of 10mm×10mm×10mm.
[0085] The composition analysis of the cobalt-based alloy obtained in Example 2 is as follows: C = 1.10 wt.%, Cr = 29.65 wt.%, Si = 0.96 wt.%, W = 4.30 wt.%, Fe = 2.98 wt.%, Mo = 1.08 wt.%, Ni = 2.95 wt.%, Mn = 0.45 wt.%, with the balance being Co.
[0086] The cobalt-based alloy obtained in Example 2 has a density of 98.89%, a tensile strength of 898 MPa, a yield strength of 485 MPa, and an elongation of 5.0%.
[0087] The cobalt-based alloy microstructure obtained in Example 2 consisted of equiaxed and columnar crystals, with an average grain size of 3.62 μm. The size difference between the equiaxed and columnar crystals was significant. Some equiaxed crystals were very small, with a minimum size of 1.55 μm. Grains smaller than 2 μm accounted for 19.54%, and grains smaller than 3 μm accounted for 56.62%. Columnar crystals, on the other hand, had very large sizes. The maximum value was 20.25 μm, and even this is an extreme mislabeled value; a significant amount of grains were still present at 14.45 μm.
[0088] The cobalt-based alloy matrix obtained in Example 2 is an α-Co solid solution matrix. The lamellar precipitates near the grain boundaries are Cr-rich phases, while the circular precipitates appearing between dendrites and in the solid solution are mainly Cr- and Co-rich M7C3 and M... 23 C6 type carbides.
[0089] The XRD pattern of the alloy obtained in Example 2 is as follows: Figure 3 As shown, by comparing the experimental data with standard PDF cards using MDI JADE6 software and referring to relevant literature, it can be seen that the main phases in the alloy manufactured by electron beam additive manufacturing are α-Co, M23C6, and M7C3 (M = Cr, W, Co) carbides. The EBSD image of the alloy described in this embodiment is shown below. Figure 4 As shown, the analysis can reveal the grain type and size information of the alloy, as mentioned above.
[0090] TEM images of the alloy obtained in Example 2, diffraction images of the precipitates, and diffraction images of the matrix are shown below. Figure 5-7 As shown above, based on EDS, XRD, and TEM results, the matrix should be an α-Co solid solution. The blocky precipitates near the grain boundaries are Cr-rich carbides, and the circular precipitates encased within them are Cr- and Co-rich carbides. The carbides that may be present in the alloy include M7C3 and M... 23 Multiple phases, including C6, M6C, and MC, were identified. To further confirm the phase composition of the samples, the diffraction patterns were calibrated using standard PDF cards. After calibration, it was confirmed that the matrix phase was mainly α-Co with an FCC structure. The diffraction patterns of the precipitates at the grain edges were also calibrated, and M7C3 type carbides could be identified after calibration.
[0091] In actual research and development, with other conditions remaining unchanged, nine sets of experiments were conducted with different input currents and scanning speeds than in Example 2. The density of the resulting alloys is shown in Table 1, and the porosity analysis comparison photographs are shown below. Figure 10 As shown. Parameter number 7 corresponds to the parameters in Example 2. All parameters were successfully tested, with the highest relative density reaching 99.98% and the overall density not less than 98.89%.
[0092] Table 1
[0093]
[0094]
[0095] This demonstrates that strictly following the preheating temperature, electron beam heating temperature, and other process parameters in this invention to prepare alloys can result in alloys with extremely high density, and all alloys can be successfully formed, thus showcasing the superiority of the process in this invention.
[0096] Example 3
[0097] S1. Cobalt-based alloy rods are prepared into spherical powder using vacuum atomization powdering technology. The particle size range of the spherical powder is 45–105 μm, the sphericity is 87%, and the bulk density is 4.20 g / cm³. 3 The hollow pasta content was 0.08%.
[0098] S2. The spherical powder is dried in an environment with a vacuum degree not exceeding 10. —1 Pa, drying temperature is 80℃, drying time is 10h; after drying, the spherical powder is sieved in an argon atmosphere; then the sieved spherical powder is filled into the manufacturing environment containing the matrix, and the bottom of the matrix is preheated to 300℃.
[0099] S3. After starting the preheating, powder is spread on the substrate surface with a thickness of 0.09 mm. Then, the powder-spreading area is heated to 1100℃ by an electron beam. The electron beam heating parameters are: input current of 35 mA, scanning speed of 20 m / s, and scanning interval of 0.7 mm.
[0100] S4. Shape the slice file according to the set process parameters. The specific process parameters are: input current 17.6mA, scanning speed 2.6m / s.
[0101] S5. After processing, keep the formed area warm for 10 seconds.
[0102] S6. Repeat steps S3 to S5 until the printing of the 3D component is complete.
[0103] S7. Sandblast the three-dimensional component to obtain a near-fully dense cobalt-based alloy product with a diameter of 10mm×10mm×10mm.
[0104] The composition analysis of the cobalt-based alloy obtained in Example 3 is as follows: C = 2.96 wt.%, Cr = 29.04 wt.%, Si = 0.97 wt.%, W = 4.12 wt.%, Fe = 2.11 wt.%, Mo = 0.75 wt.%, Ni = 2.16 wt.%, Mn = 0.42 wt.%, with the remainder being Co.
[0105] The cobalt-based alloy obtained in Example 3 had a density of 99.08%, a tensile strength of 982 MPa, a yield strength of 491 MPa, and an elongation of 5.1%.
[0106] As demonstrated in Examples 1-3, by limiting the steps and parameters in the preparation process, it is possible to prepare cobalt-based alloys with high carbon content and high density, while also achieving the goal of forming cobalt-based alloys with larger dimensions, more complex geometries, and without microcracks. Specifically, the obtained cobalt-based alloys have a density of not less than 98.89%, a tensile strength of not less than 898 MPa, a yield strength of not less than 485 MPa, and an elongation of not less than 5.0%.
[0107] Comparative Example 1
[0108] S1. Cobalt-based alloy rods are prepared into spherical powder using vacuum atomization powdering technology. The particle size range of the spherical powder is 45–105 μm, the sphericity is 88%, and the bulk density is 4.21 g / cm³. 3 The hollow pasta content was 0.06%.
[0109] S2. The spherical powder is dried in an environment with a vacuum degree not exceeding 10. -1 Pa, drying temperature is 80℃, drying time is 10h; after drying, the spherical powder is sieved in an argon atmosphere; then the sieved spherical powder is filled into the manufacturing environment containing the matrix, and the bottom of the matrix is preheated to 200℃.
[0110] S3. After starting the preheating, powder is spread on the substrate surface with a thickness of 0.09 mm. Then, the powder-spreading area is heated to 400°C by an electron beam. The electron beam heating parameters are: input current of 35 mA, scanning speed of 20 m / s, and scanning interval of 0.7 mm.
[0111] S4. Shape the slice file according to the set process parameters. The specific process parameters are: input current 10.4mA, scanning speed 1.2m / s;
[0112] S5. After processing, keep the forming area warm for 10 seconds;
[0113] S6. Repeat steps S3 to S5 until the printing of the 3D component is complete;
[0114] S7. Sandblast the three-dimensional component to obtain a cobalt-based alloy product of approximately 10mm×10mm×10mm.
[0115] The density of the cobalt-based alloy obtained in Comparative Example 1 was 92.59%, which was much lower than that in Examples 1-3. This shows that if the electron beam heating temperature is difficult to reach the range specified in this application, the density will be greatly affected.
[0116] Furthermore, the metallographic diagram of the alloy obtained in Comparative Example 1 is as follows: Figure 8 As shown, through Figure 8 It can be seen that the cobalt-based alloy obtained in Comparative Example 1 has hot cracks, and the main microstructure is equiaxed crystals and dendrites.
[0117] After etching with aqua regia, the metallographic image of the alloy is as follows: Figure 9 As shown, through Figure 9 It can be seen that the cobalt-based alloy obtained in Comparative Example 1 has uneven corrosion. The high-magnification metallographic images show a large number of over-corroded areas, indicating that there is serious segregation inside the cobalt-based alloy obtained in Comparative Example 1.
[0118] Comparative Example 2
[0119] Compared with Example 1, other conditions remained the same, except that the preheating temperature was 200°C and electron beam heating was not used, and the final powder bed temperature reached 200°C.
[0120] The resulting alloy exhibited macroscopic cracking, such as... Figure 11 As shown, it is evident that a preheating composite electron beam heating method must be employed to address the macroscopic cracking problem in the material.
[0121] Comparative Example 3
[0122] S1. The cobalt-based alloy rod described in this comparative example was prepared into spherical powder using vacuum atomization powder preparation technology. The particle size range of the spherical powder was 45–105 μm, the sphericity was 89%, and the bulk density was 4.34 g / cm³. 3 The hollow pasta content was 0.09%.
[0123] S2. The spherical powder is dried in an environment with a vacuum degree not exceeding 10. -1 Pa, drying temperature is 80℃, drying time is 10h; after drying, the spherical powder is sieved in an argon atmosphere; then the sieved spherical powder is filled into the manufacturing environment containing the matrix, and the bottom of the matrix is preheated to 200℃.
[0124] S3. After starting the preheating, powder is spread on the substrate surface with a thickness of 0.09 mm. Then, the powder-spreading area is heated to 1100℃ by an electron beam. The electron beam heating parameters are: input current of 35 mA, scanning speed of 20 m / s, and scanning interval of 0.7 mm.
[0125] S4. Shape the slice file according to the set process parameters. The specific process parameters are: input current 7.0mA, scanning speed 2.4m / s;
[0126] S5. After processing, keep the forming area warm for 20 seconds;
[0127] S6. Repeat steps S3 to S5 until the printing of the 3D component is completed or partially completed;
[0128] S7. Sandblast the three-dimensional component to obtain a cobalt-based alloy product of approximately 10mm×10mm×10mm.
[0129] The composition analysis of the cobalt-based alloy obtained in Comparative Example 3 was as follows: C = 3.45 wt.%, Cr = 26.18 wt.%, Si = 0.32 wt.%, W = 15.10 wt.%, Fe = 1.74 wt.%, Mo = 0.24 wt.%, Ni = 1.17 wt.%, with the balance being Co.
[0130] The alloy obtained in Comparative Example 3 has a high carbon and tungsten content. Although this increases the material's hardness, it also presents a greater risk of cracking. When molding using the process parameters defined in this invention, severe cracking of the block occurs, and even molding failure may result. Figure 12 As shown. In addition, a sample was taken for metallographic observation (e.g. Figure 13 As shown in the figure, the metallographic photographs show a large number of cracks and pores. Therefore, the material obtained in Comparative Example 3 is not a dense cobalt-based alloy and cannot be put into practical application.
[0131] As can be seen from Comparative Example 3, the proportional relationship of each component in the alloy is extremely important. Only by using the preparation method of the present invention within the proportion range protected in the present invention can a crack-free alloy with high density be prepared. Otherwise, the prepared alloy will have low density, microcracks inside, poor overall surface quality, or even be unable to be formed into a block.
[0132] Comparative Example 4
[0133] Compared to Example 1, directly heating with an electron beam without preheating results in severe powder layer adhesion, or even complete clumping or curling of the powder layer before sintering, making printing impossible. This is because the preheating step before electron beam heating ensures the overall temperature uniformity of the powder in the forming space, while electron beam heating only heats the surface powder inside the forming cylinder, causing a large temperature difference to quickly form between the surface powder and the powder below. Without preheating, the excessive temperature gradient between the upper and lower layers of powder in the powder cylinder leads to powder layer curling.
[0134] Comparative Example 5
[0135] Compared to Example 1, with other conditions remaining unchanged, the preheating temperature was changed to 100 degrees Celsius. The final block can then be formed. Figure 14 However, microcracks exist. Figure 15 This highlights the importance of preheating temperature.
[0136] The applicant declares that the detailed method of the present invention is illustrated by the above embodiments, but the present invention is not limited to the above detailed method, that is, it does not mean that the present invention must rely on the above detailed method to be implemented. Those skilled in the art should understand that any improvements to the present invention, equivalent substitutions of the raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for preparing a cobalt-based alloy with high density and high carbon content, characterized in that, The cobalt-based alloy comprises the following components by mass fraction: 0.10≤C≤3.00 wt.%, 8.00≤Cr≤33.00 wt.%, Fe≤5.00 wt.%, Mn≤2.00 wt.%, Mo≤30.00 wt.%, Ni≤25.00 wt.%, Si≤3.50 wt.%, W≤15.00%, the rest is Co; The preparation method of cobalt-based alloys includes the following steps: S1. The powder is sieved, dried, and then filled into the manufacturing environment containing the matrix; S2, Preheating; S3. Powder is spread on the substrate surface, and then the powder-spreading layer area is heated by electron beam scanning; S4. A single layer of the cobalt-based alloy is formed by electron beam scanning; S5. Keep the molding area warm for a certain period of time; S6. Repeat steps S3 to S5 until the three-dimensional printing of the cobalt-based alloy component is completed; S7. Perform subsequent processing on the three-dimensional component to obtain the cobalt-based alloy; In step S2, the preheating temperature is 200–550°C; In step S3, the heating temperature is 500–1200°C; The above alloy has a hardness of 33-48 HRC, a room temperature tensile strength of 800-1300 MPa, and an elongation of 5%-11%.
2. The method for preparing a cobalt-based alloy with high density and high carbon content according to claim 1, characterized in that, By mass fraction, it includes the following components: 0.90≤C≤3.00 wt.%, 28.00≤Cr≤30.00 wt.%, Fe≤3.00 wt.%, Mn≤0.50 wt.%, Mo≤2.00 wt.%, Ni≤3.00 wt.%, 0.70≤Si≤1.55 wt.%, 3.50≤W≤5.50%, the rest is Co.
3. The method for preparing a cobalt-based alloy with high density and high carbon content according to claim 1, characterized in that, The average grain size of the alloy is between 1 μm and 20 μm.
4. The method for preparing a high-density, high-carbon cobalt-based alloy according to claim 1, characterized in that, The technical specifications of the powder are as follows: particle size 10–300 μm, sphericity ≥70%, and loose density ≥4.10 g / cm³. 3 Hollow starch content ≤ 0.2%.
5. The method for preparing a high-density, high-carbon cobalt-based alloy according to claim 1, characterized in that, The preheating temperature is 300-550℃.
6. The method for preparing a high-density, high-carbon cobalt-based alloy according to claim 1, characterized in that, In step S3, the heating parameters are: electron beam input current of 30-40mA, scanning speed of 20-22m / s, and scanning interval of 0.5-1mm.
7. The method for preparing a high-density, high-carbon cobalt-based alloy according to claim 1, characterized in that, In step S4, the process parameters are: input current of 5-50mA, scanning speed of 0.5-10.5m / s, and scanning spacing of 0.09-0.2mm.
Citation Information
Patent Citations
High-hardness cobalt-based alloy powder for laser cladding and preparation technology of high-hardness cobalt-based alloy powder for laser cladding
CN104195546A
Preparation method of nickel-based alloy single crystal or directional solidified parts
CN111872395A