Degradable barrier film and its preparation method and application

By processing materials such as modified graphene oxide and polylactic acid, a degradable barrier film is prepared, which solves the problems of the existing release film being unable to degrade and having insufficient barrier performance, achieving more efficient protection of asphalt waterproofing membranes and extending the Extended service life and improved waterproof performance.

CN117736471BActive Publication Date: 2024-10-18KESHUN WATERPROOF TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202311489065.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-09
Publication Date
2024-10-18
Estimated Expiration
2043-11-09

AI Technical Summary

Technical Problem

The existing release film cannot be degraded after use, causing environmental pollution, and its barrier properties are insufficient to effectively protect the weather resistance of asphalt waterproofing membranes.

Method used

Modified graphene oxide, polypropylene carbonate, antioxidants and opening agents are used for granulation treatment, then mixed with polylactic acid and extruded into a cast film, and then coated with silicone oil to prepare a degradable barrier type membrane. The method operates at lower temperatures, reducing thermal decomposition of polypropylene carbonate and improving material mixing uniformity.

Benefits of technology

The prepared degradable barrier membrane has good barrier properties, significantly reduces the penetration of oxygen and moisture, extends the service life of the asphalt waterproofing membrane, and improves its durability and waterproof performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004540655130000071
    Figure BDA0004540655130000071
  • Figure BDA0004540655130000081
    Figure BDA0004540655130000081
  • Figure BDA0004540655130000101
    Figure BDA0004540655130000101
Patent Text Reader

Abstract

The present invention relates to the technical field of waterproofing coiled materials, and discloses a degradable barrier film and a preparation method and application thereof. The method comprises: (1) granulation: introducing modified graphene oxide and polypropylene carbonate into a kneader for a first stirring treatment to obtain a mixture I; subjecting the mixture I to a second stirring treatment with polylactic acid to obtain a mixture II; extruding and granulating the mixture II in a kneader to obtain a granulated material; the temperature of the second stirring treatment is higher than the temperature of the first stirring treatment by more than 10°C; (2) preparing a cast film; (3) coating with silicon. The degradable barrier film provided by the present invention can effectively reduce the penetration of oxygen and moisture, extend the service life of asphalt waterproofing coiled materials, and improve their durability and waterproofing performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of waterproof coiled materials, and in particular to a degradable barrier film and a preparation method and application thereof. Background Art

[0002] Release films are widely used in the fields of construction and building materials, especially in the production of asphalt waterproofing membranes. In the production of asphalt waterproofing membranes, release films are mainly used to prevent asphalt materials from adhering to the surface of waterproofing membranes during hardening. The use of release films can effectively separate asphalt and auxiliary materials, ensuring the smoothness and flatness of the surface of waterproofing membranes.

[0003] Release film not only plays a key role in waterproof membrane, but is also widely used in the production of other products, such as fireproof materials, composite materials, shipbuilding and other fields.

[0004] Existing release films are usually made of plastic films such as polyethylene and polyester, which cannot be degraded after use, and thus will cause pollution to the environment during post-use disposal.

[0005] The weather resistance of asphalt membrane is one of the important indicators to ensure its long-term use, and the barrier performance of release film plays a key protective role. The existing release film has poor barrier performance and cannot well protect the weather resistance of asphalt waterproof membrane.

[0006] CN112409946A discloses a dyed self-adhesive asphalt coil release film. The release film includes an isolation layer, an EVOH barrier layer, a silicone oil carrier film and a dyed silicone oil layer from top to bottom; and the isolation layer is a PP (polypropylene) or PE (polyethylene) film. The release film can effectively prevent the aging and damage of the asphalt material and effectively prevent the oil precipitated in the asphalt from seeping into the outer layer of the film. However, the polypropylene film or polyethylene film that must be used in the prior art cannot be degraded, and will cause obvious environmental pollution after use. Summary of the invention

[0007] The purpose of the invention is to prepare a degradable release film with good barrier properties.

[0008] In order to achieve the above object, the first aspect of the present invention provides a method for preparing a degradable barrier film, the method comprising:

[0009] (1) Granulation

[0010] S11: introducing modified graphene oxide, polypropylene carbonate, an antioxidant and an opening agent into a kneader for a first stirring treatment to obtain a mixture I; the contact angle of the modified graphene oxide is 65°-80°;

[0011] S12: subjecting the mixture I and polylactic acid to a second stirring treatment to obtain a mixture II;

[0012] S13: extruding and granulating the mixture II in a kneader to obtain granulated material;

[0013] The temperature of the second stirring treatment is higher than the temperature of the first stirring treatment by more than 10° C.; and the weight ratio of the modified graphene oxide, the polypropylene carbonate, and the polylactic acid is 1:2-40:10-70;

[0014] (2) Preparation of cast film

[0015] The granulated material is introduced into a cast film extruder for processing to obtain a cast film;

[0016] (3) Silicon coating

[0017] Silicone oil is coated on any side of the cast film, and the release film is obtained after drying.

[0018] The second aspect of the present invention provides a degradable barrier film prepared by the method described in the first aspect.

[0019] The third aspect of the present invention provides a use of the degradable barrier film described in the second aspect in an asphalt waterproofing membrane.

[0020] The degradable barrier film prepared by the solution provided by the present invention has good barrier properties, can more effectively reduce the penetration of oxygen and moisture (water vapor permeability and oxygen permeability), extend the service life of the asphalt waterproof membrane, and improve its durability and waterproof performance.

[0021] In addition, the method for preparing a degradable barrier release film provided by the present invention can be operated at a relatively low temperature (e.g., 100-170°C, preferably 110-150°C, and more preferably 120-140°C), that is, the present invention can obtain a release film with good performance at a relatively low operating temperature, thereby reducing the thermal decomposition of polypropylene carbonate in the release film.

[0022] Moreover, in the scheme of the present invention, even under the strong shearing and friction of the kneader, the modified graphene oxide with smaller particle size is not easy to agglomerate and is easier to be evenly mixed with other components. DETAILED DESCRIPTION

[0023] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0024] As mentioned above, the first aspect of the present invention provides a method for preparing a degradable barrier film, the method comprising:

[0025] (1) Granulation

[0026] S11: introducing modified graphene oxide, polypropylene carbonate, an antioxidant and an opening agent into a kneader for a first stirring treatment to obtain a mixture I; the contact angle of the modified graphene oxide is 65°-80°;

[0027] S12: subjecting the mixture I and polylactic acid to a second stirring treatment to obtain a mixture II;

[0028] S13: extruding and granulating the mixture II in a kneader to obtain granulated material;

[0029] The temperature of the second stirring treatment is higher than the temperature of the first stirring treatment by more than 10° C.; and the weight ratio of the modified graphene oxide, the polypropylene carbonate, and the polylactic acid is 1:2-40:10-70;

[0030] (2) Preparation of cast film

[0031] The granulated material is introduced into a cast film extruder for processing to obtain a cast film;

[0032] (3) Silicon coating

[0033] Silicone oil is coated on any side of the cast film, and the release film is obtained after drying.

[0034] Preferably, in step S11, the weight average molecular weight of the polypropylene carbonate is 40,000-60,000.

[0035] Preferably, in step S11, the conditions of the first stirring treatment include: a temperature of 100-130°C and a time of 0.5-2h.

[0036] According to a preferred specific implementation, in step S11, the modified graphene oxide is a product prepared by a method comprising the following steps:

[0037] S1a: ultrasonically dispersing water, ethanol and graphene oxide to obtain dispersion I;

[0038] S1b: mixing and contacting the dispersion liquid I with a silane coupling agent, and drying the obtained precipitated material to obtain the modified graphene oxide.

[0039] Preferably, in step S1a, the weight ratio of the water, the ethanol and the graphene oxide is 100-200:50-100:1.

[0040] Preferably, in step S1a, the conditions of the ultrasonic dispersion treatment include: a frequency of 30-50 kHz, a temperature of 70-80°C, and a time of 20-60 min.

[0041] The present invention has no special requirements on the type of the water, and has no special requirements on the type of the ethanol. Exemplarily, the water is distilled water, and the ethanol is anhydrous ethanol.

[0042] The present invention has no special requirements on the source of the graphene oxide, and those skilled in the art can synthesize it by adopting technical means known in the art or obtain it through commercial purchase.

[0043] Preferably, in step S1b, the silane coupling agent is γ-aminopropyltriethoxysilane.

[0044] Preferably, in step S1b, the weight ratio of the silane coupling agent to the graphene oxide is 1.5-5:1.

[0045] Preferably, in step S1b, the mixed contact conditions include: temperature of 60-80°C and time of 6-24h.

[0046] The present invention has no particular requirement for the heating method of the mixed contact, for example, an oil bath or a water bath can be used, and heating is exemplarily performed in a water bath.

[0047] It should be noted that, in step S1b, the dispersion I and the silane coupling agent may be mixed and contacted and then filtered, and may be washed before the drying process. The present invention has no special requirements for the filtering, and those skilled in the art may perform the filtering by adopting technical means known in the art. The present invention has no special requirements for the washing, and illustratively, the precipitation material may be washed with anhydrous ethanol and distilled water in sequence.

[0048] Preferably, in step S12, the conditions of the second stirring treatment include: a temperature of 140-170° C. and a time of 0.1-1.5 h.

[0049] Preferably, in step S13, the conditions for extrusion granulation include: a stirring speed of 30-50 rpm and a temperature of 140-180°C.

[0050] Preferably, the weight ratio of the modified graphene oxide, the opening agent and the antioxidant is 1:0.1-2:0.06-1.

[0051] Preferably, in step (2), the processing conditions include: the main engine temperature of the extruder is 130-180°C, the main engine speed is 30-40rpm, and the die head temperature is 150-180°C.

[0052] As mentioned above, the second aspect of the present invention provides a degradable barrier film prepared by the method described in the first aspect.

[0053] As mentioned above, the third aspect of the present invention provides the use of the degradable barrier film described in the second aspect in an asphalt waterproofing membrane.

[0054] The present invention will be described in detail below by way of examples. In the following examples, unless otherwise specified, all the instruments and raw materials used are commercially available.

[0055] Graphene oxide: purchased from Xianfeng Nanotechnology Co., Ltd., brand XF002-1.

[0056] Polypropylene carbonate: the average weight average molecular weight is 48,000, purchased from Henan Tianguan Enterprise Group Co., Ltd.

[0057] Polylactic acid: purchased from Hisun Biomaterials Co., Ltd., brand name REVODE110.

[0058] Opening agent: Opening agent (oleic acid amide) was purchased from Dongguan Kangjin New Material Technology Co., Ltd.

[0059] Antioxidant: pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, purchased from Tianjin Li'anlong New Materials Co., Ltd., brand RIANOX1010.

[0060] Silane coupling agent: γ-aminopropyltriethoxysilane, purchased from Hangzhou Jessica Chemical Co., Ltd., brand KH550.

[0061] Titanate coupling agent: propyl dioleate acyloxy (dioctyl phosphate acyloxy) titanate, purchased from Hangzhou Jessica Chemical Co., Ltd., brand HY-101.

[0062] Silicone oil: purchased from Dow Corning Zhangjiagang Silicone Co., Ltd., brand PMX200CST.

[0063] Kneading machine: Model is NHL-500L, purchased from Nantong Internal Mixing and Kneading Machinery Co., Ltd.

[0064] Cast film extruder: Model CJWH75-44D, purchased from JWELL Machinery Manufacturing Co., Ltd.

[0065] Different raw material formulations are used in the following preparation examples of the present invention. The amounts of raw materials are all parts by weight unless otherwise specified, and each part by weight represents 100 g.

[0066] The contact angle is tested using the test method specified in the GBT30447-2013 standard.

[0067] Preparation Example 1: Preparation of modified graphene oxide X1

[0068] S1: ultrasonically dispersing distilled water, anhydrous ethanol and graphene oxide to obtain a dispersion liquid I;

[0069] The amount of distilled water is 100 parts by weight, the amount of anhydrous ethanol is 50 parts by weight, and the amount of graphene oxide is 1 part by weight;

[0070] The conditions of ultrasonic dispersion treatment were as follows: ultrasonic frequency was 40 KHz, temperature was 80 °C, and time was 30 min;

[0071] S2: mixing the dispersion I with the silane coupling agent, filtering to obtain a precipitate, and washing the precipitate with anhydrous ethanol and distilled water in turn, and drying to obtain modified graphene oxide X1.

[0072] The silane coupling agent is γ-aminopropyltriethoxysilane, and the amount used is 4 parts by weight;

[0073] Mixing contact conditions: water bath heating temperature 80 ° C, time 12h;

[0074] The contact angle was measured to be 77.3°.

[0075] Preparation Example 2: Preparation of modified graphene oxide X2

[0076] S1: ultrasonically dispersing distilled water, anhydrous ethanol and graphene oxide to obtain dispersion liquid I;

[0077] The amount of distilled water is 150 parts by weight, the amount of anhydrous ethanol is 75 parts by weight, and the amount of graphene oxide is 1 part by weight;

[0078] The conditions of ultrasonic dispersion treatment were as follows: ultrasonic frequency was 30 KHz, temperature was 70 °C, and time was 40 min;

[0079] S2: mixing the dispersion I with the silane coupling agent, filtering to obtain a precipitate, and washing the precipitate with anhydrous ethanol and distilled water in turn, and drying to obtain modified graphene oxide X1.

[0080] The silane coupling agent is γ-aminopropyltriethoxysilane, and the amount used is 2 parts by weight;

[0081] Mixing contact conditions: water bath heating temperature 70 ° C, time 14h;

[0082] The contact angle was measured to be 77.8°.

[0083] Preparation Example 3: Preparation of modified graphene oxide X3

[0084] This preparation example was carried out using a method similar to that of Preparation Example 1, except that the silane coupling agent used in this preparation example was an equal weight of a titanate coupling agent (specifically propyl dioleyl (dioctyl phosphate) titanate).

[0085] The rest were the same as in Preparation Example 1, and modified graphene oxide X3 was obtained, and its contact angle was measured to be 68.5°.

[0086] Different raw material formulations are used in the following examples of the present invention. The raw material amounts are all parts by weight unless otherwise specified, and each part by weight represents 100 g. The specific raw material formulations are shown in Table 1 (unless otherwise specified, the types of substances in Table 1 are listed in the previous text).

[0087] Table 1

[0088]

[0089]

[0090] Example 1

[0091] In this example, a degradable barrier film was prepared according to the following method.

[0092] The method for preparing a degradable barrier film comprises the following steps:

[0093] (1) Granulation

[0094] S11: introducing modified graphene oxide, polypropylene carbonate, an antioxidant and an opening agent into a kneader, and performing a first stirring treatment to obtain a mixture I;

[0095] S12: subjecting the mixture I and polylactic acid to a second stirring treatment to obtain a mixture II;

[0096] S13: extruding and granulating the mixture II in a kneader to obtain granulated material;

[0097] (2) Preparation of cast film

[0098] The granulated material is introduced into a cast film extruder for processing to obtain a cast film;

[0099] (3) Silicon coating

[0100] Silicone oil is coated on any side of the cast film, and after drying, a degradable barrier film is obtained.

[0101] The specific process parameters in this embodiment are shown in Table 2.

[0102] Unless otherwise specified, the remaining embodiments are carried out using the same process as in Example 1, except that the raw material formulations and process parameters are different, as shown in Table 2. The unlisted parts are the same as in Example 1.

[0103] Example 5

[0104] This example is carried out in the same manner as in Example 1, except that in this example, Formula 5 of the same weight portion is used to replace Formula 1 in Example 1.

[0105] The rest is the same as in Example 1, and a degradable barrier film is obtained.

[0106] Example 6

[0107] This example is carried out in the same manner as in Example 1, except that in this example, Formula 6 of the same weight portion is used to replace Formula 1 in Example 1.

[0108] The rest is the same as in Example 1, and a degradable barrier film is obtained.

[0109] Example 7

[0110] This embodiment is carried out in a similar manner to that of Embodiment 1, except that the temperature of the first stirring treatment in this embodiment is adjusted from 110° C. in Embodiment 1 to 140° C.

[0111] The rest is the same as in Example 1, and a degradable barrier film is obtained.

[0112] Comparative Example 1

[0113] This comparative example is carried out in the same manner as in Example 1, except that the polypropylene carbonate in Example 1 is not used in this comparative example, that is, the formula in this comparative example is the comparative formula D1 listed above.

[0114] The rest is the same as in Example 1, and a degradable barrier film is obtained.

[0115] Comparative Example 2

[0116] This comparative example was carried out in the same manner as in Example 1, except that the modified graphene oxide in Example 1 was not used in this comparative example, that is, the formula in this comparative example was the comparative formula D2 listed above.

[0117] The rest is the same as in Example 1, and a degradable barrier film is obtained.

[0118] Comparative Example 3

[0119] The same method as in Example 1 was used in this comparative example, except that the same weight of graphene oxide (the contact angle of graphene oxide was 41.2°) was used to replace the modified graphene oxide in Example 1, that is, the formula in this comparative example was the comparative formula D3 listed above.

[0120] The rest is the same as in Example 1, and a degradable barrier film is obtained.

[0121] Comparative Example 4

[0122] This comparative example is carried out in the same manner as Example 1, except that the polypropylene carbonate in this comparative example is adjusted from 40 parts by weight in Example 1 to 1 part by weight, that is, the formula in this comparative example is the comparative formula D4 listed above.

[0123] The rest is the same as in Example 1, and a degradable barrier film is obtained.

[0124] Comparative Example 5

[0125] This comparative example was carried out in the same manner as in Example 1, except that the second stirring temperature in this comparative example was adjusted from 160° C. in Example 1 to 110° C.

[0126] The rest is the same as in Example 1, and a degradable barrier film is obtained.

[0127] Table 2

[0128]

[0129]

[0130] Table 2 (Continued)

[0131]

[0132] Test Case

[0133] The barrier properties (oxygen transmission rate (OTR) and water vapor transmission rate (WVTR)) of the degradable barrier isolation type film prepared in the example were tested by the test methods specified in ISO15105-2 and ISO15106-3 standards; the degradation performance (biodegradation rate) of the degradable barrier isolation type film was tested by the methods specified in GB / T19277.1 and GB / T19277.2 standards. The specific results are shown in Table 3.

[0134] Table 3

[0135]

[0136] From the results in Table 3, it can be seen that the release film prepared by the present invention has a high biodegradability, a low oxygen permeability and a low water vapor permeability, indicating that the release film prepared by the present invention has high degradability and good barrier properties. The release film of the present invention is applied to asphalt waterproofing membrane, which can effectively reduce the penetration of oxygen and water, extend the service life of the asphalt waterproofing membrane, and has a significantly better effect.

[0137] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A method for preparing a degradable barrier film, characterized in that: The method includes: (1) Granulation S11: introducing modified graphene oxide, polypropylene carbonate, an antioxidant and an opening agent into a kneader for a first stirring treatment to obtain a mixture I; the contact angle of the modified graphene oxide is 65°-80°; S12: subjecting the mixture I and polylactic acid to a second stirring treatment to obtain a mixture II; S13: extruding and granulating the mixture II in a kneader to obtain granulated material; The temperature of the second stirring treatment is higher than the temperature of the first stirring treatment by more than 10° C.; and the weight ratio of the modified graphene oxide, the polypropylene carbonate, and the polylactic acid is 1:2-20:10-35; (2) Preparation of cast film The granulated material is introduced into a cast film extruder for processing to obtain a cast film; (3) Silicon coating Applying silicone oil on any one side of the cast film and drying it to obtain the release film; In step S11, the conditions of the first stirring treatment include: temperature of 100-130°C and time of 0.5-2h; In step S12, the conditions of the second stirring treatment include: temperature of 140-170°C and time of 0.1-1.5h; In step S13, the conditions for extrusion granulation include: stirring speed of 30-50 rpm, temperature of 140-180°C; In step (2), the processing conditions include: the main engine temperature of the extruder is 130-180°C, the main engine speed is 30-40rpm, and the die head temperature is 150-180°C.

2. The method according to claim 1, wherein: In step S11, the modified graphene oxide is a product prepared by a method comprising the following steps: S1a: ultrasonically dispersing water, ethanol and graphene oxide to obtain dispersion I; S1b: mixing and contacting the dispersion liquid I with a silane coupling agent, and drying the obtained precipitated material to obtain the modified graphene oxide.

3. The method according to claim 2, wherein: In step S1a, the weight ratio of the water, the ethanol and the graphene oxide is 100-200:50-100:1; And / or, in step S1a, the conditions of the ultrasonic dispersion treatment include: a frequency of 30-50 kHz, a temperature of 70-80° C., and a time of 20-60 min.

4. The method according to claim 2 or 3, wherein: In step S1b, the silane coupling agent is γ-aminopropyltriethoxysilane; And / or, the weight ratio of the silane coupling agent to the graphene oxide is 1.5-5:1; And / or, the mixed contact conditions include: temperature of 60-80° C. and time of 6-24 h.

5. The method according to any one of claims 1 to 3, wherein: The weight ratio of the modified graphene oxide, the opening agent and the antioxidant is 1:0.1-2:0.06-1.

6. A degradable barrier film prepared by the method according to any one of claims 1 to 5.

7. Use of the degradable barrier film according to claim 6 in asphalt waterproofing membrane.

Citation Information

Patent Citations

  • Dyed self-adhesive asphalt coiled material release film

    CN112409946A

  • Renewable high-barrier polyester packaging material and preparation method thereof

    CN113185810A

  • Polylactic acid film with high barrier property and preparation method thereof

    CN116769206A

  • A biodegradable mobile phone screen protector

    CN218842024U