A hydraulic end forging optimization process method

By establishing the temperature-density curve and balanced phase diagram of the hydraulic end material, optimizing the forging process parameters, the problems of melting point and grain growth of the hydraulic end material are solved, and the mechanical properties and internal tissue density of the material are improved. It is suitable for steel metallurgy industry.

CN117753907BActive Publication Date: 2024-11-19NANJING DEV ADVANCED MFG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311852967.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-29
Publication Date
2024-11-19
Estimated Expiration
2043-12-29

AI Technical Summary

Technical Problem

The existing hydraulic forging process cannot effectively optimize the melting point and grain growth of the material, resulting in insufficient mechanical properties of the material and internal defects such as pores, shrinkage pores and dendrites, affecting its mechanical properties.

Method used

Through high-temperature volume measurement and thermodynamic balance test, the temperature-density curve and balanced phase diagram of the hydraulic end material are established, and the melting point of the material, the Ac3 phase change point and the optimization of forging process parameters, such as the initial forging temperature, the final forging temperature, and the heating coefficient. and deformation amount, optimize the forging process to control grain growth.

Benefits of technology

It improves the plasticity and forging of materials, ensures the strength and mechanical properties of forgings, eliminates internal defects, forms dense tissue, and has potential application prospects in the steel and metallurgy industry.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117753907B_ABST
    Figure CN117753907B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for optimizing the forging process of a hydraulic end. The method establishes a temperature-density curve according to the upper, middle and lower limits of the range of the chemical composition of the hydraulic end material through a high-temperature volume measurement test; establishes a carbon equivalent-melting point / liquidus curve and a carbon equivalent-Ac3 temperature point curve according to the different carbon equivalents of the chemical composition of the material, fits the relevant function, and determines the initial forging temperature and final forging temperature range of the hydraulic end material; and optimizes and controls the forging process parameters such as the heating temperature, the holding time, the heating coefficient, the deformation amount and the forging ratio at the same time, so that the hydraulic end forging is easier to deform and the growth and size of its grains are effectively controlled. The present invention can effectively improve the plasticity and forgeability of the material through the optimization of the forging process of the hydraulic end, thereby ensuring the mechanical properties such as the strength and toughness of the hydraulic end forging, and has potential application prospects and practical value in the field of iron and steel metallurgy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a hydraulic end forging optimization process method and belongs to the technical field of metallurgical industry. Background Art

[0002] The hydraulic end is a method of using fluid power to drive mechanical devices. It is an accurate, efficient and reliable mechanical transmission solution that can help mechanical equipment save more power consumption and effectively improve its working efficiency. The principle of the hydraulic end is a physical principle that can be used to explain the behavior of the body under the action of gravity, the flow behavior of the liquid, the pressure change of the liquid, and the interaction between bubbles in the liquid. Therefore, learning the principle of the hydraulic end can help people better understand the characteristics of liquids and thus better apply the characteristics of liquids.

[0003] Appropriate forging can improve the internal structure of materials and enhance mechanical properties. After forging, the structure and performance of the forging blank are improved and enhanced. Forging can eliminate defects such as pores, shrinkage cavities and dendrites inside the metal ingot, and due to the plastic deformation and recrystallization of the metal, the coarse grains can be refined to obtain a dense metal structure, thereby improving the mechanical properties of the forging. The melting point is obtained through the temperature-density curve, and the constant forging temperature range of the liquid end material is determined; the forging process parameters such as heating temperature, holding time, heating coefficient, deformation and forging ratio are optimized and controlled to make the liquid end forging easier to deform, and effectively control the growth and size of its grains. It has potential application prospects and practical value in the field of steel metallurgy.

[0004] Therefore, a new hydraulic end forging optimization process method is needed to solve the above problems. Summary of the invention

[0005] The object of the present invention is to provide a method for optimizing the process of forging a hydraulic end to solve the problems raised in the above-mentioned background technology.

[0006] A method for optimizing the forging process of a hydraulic end comprises the following steps:

[0007] Step 1: The temperature-density curve of the hydraulic end material is established by a high-temperature volume measurement test for hydraulic end materials with different carbon equivalents, and the equilibrium phase diagram is established by a thermodynamic equilibrium test;

[0008] Step 2: Using the temperature-density curve and equilibrium phase diagram of the liquid end material, establish the carbon equivalent and liquidus curve, the carbon equivalent and melting point curve, and the carbon equivalent and Ac3 temperature point curve of the liquid end material to obtain the melting point temperature and Ac3 phase transition point temperature of the liquid end material;

[0009] Step 3, using the melting point temperature and Ac3 phase transition point temperature of the liquid end material obtained in step 2, determine the initial forging temperature and the final forging temperature of the liquid end material;

[0010] Step 4: According to step 3, the initial forging temperature and the final forging temperature of the liquid end material are obtained, and the forging process of the liquid end material is optimized.

[0011] Furthermore, the mass percentages of the components in the liquid end material are: C≤0.07%, Si≤1.0%, Mn≤1.00%, P≤0.040%, S≤0.030%, Cr: 14.00-15.50%, Ni: 3.50-5.50%, Mo≤0.50%, Cu: 2.50-4.50%, and the rest is Fe.

[0012] Furthermore, the melting point curve of the liquid end material in step 2 is expressed by the following formula:

[0013] z = -54.164x + 1599.8, R 2 =0.9979

[0014] Where: z is the melting point temperature; x is the carbon equivalent, the carbon equivalent range is [3.28, 4.19], R 2 Indicates the goodness of fit.

[0015] Furthermore, the liquidus curve of the liquid end material in step 2 is represented by the following formula:

[0016] y=-49.763x+1639.7,R 2 =0.9848

[0017] Where: y is the liquidus temperature; x is the carbon equivalent, the carbon equivalent range is [3.28, 4.19], R 2 Indicates the goodness of fit.

[0018] Furthermore, the temperature-density curve of the liquid end material in step 1 is expressed by the following formula:

[0019] δ=-5E-08t 2 -0.0003t+7.866, R 2 =1

[0020] Where: δ is material density; t is temperature, the temperature range is [20, 1200], R 2 Indicates the degree of fit.

[0021] Furthermore, the relationship curve between the carbon equivalent of the liquid end material in step 2 and the Ac3 temperature point is expressed by the following formula:

[0022] u=4.1284x 2+60.805x+634.98, R 2 =0.9953

[0023] Where: u is the Ac3 temperature point; x is the carbon equivalent, 3.28≤x≤4.18; R 2 represents the goodness of fit;

[0024] Furthermore, the initial forging temperature of the fluid end material in step 3 is expressed by the following formula:

[0025] T 始 =T 熔 -v 常

[0026] Among them, T 常 Calculated by the following formula:

[0027] T 常 =28.274x 2 -158.32x+365.92, R 2 =0.9933

[0028] Where, T 始 is the initial forging temperature, T 熔 is the melting point temperature, T 常 is a constant, T 常 The range is [150, 200], x is the carbon equivalent, the carbon equivalent range is [3.28, 4.19], R 2 Indicates the degree of fit.

[0029] Furthermore, the final forging temperature of the fluid end material in step 3 is expressed by the following formula:

[0030] T 终 =Ac3+K

[0031] The K value is calculated by the following formula:

[0032] K = 3.6217x 2 -65.376x+225.32, R 2 =0.9992

[0033] Where, T 终 is the final forging temperature, Ac3 is the austenite phase transformation temperature, K is a constant, K range is [15, 50], x is the carbon equivalent, the carbon equivalent range is [3.28, 4.19], R 2 Indicates the degree of fit.

[0034] Furthermore, in step 4, the hydraulic end material is forged according to the initial forging temperature and final forging temperature of the hydraulic end material obtained in step 3, specifically: the forging preheating temperature of the hydraulic end material is 850°C ± 50°C, the heating coefficient is 0.2-0.3min / mm, the forging heating temperature is 1170-1270°C, the heating coefficient is 0.3-0.4min / mm, and the heat preservation is 4-6 hours. The final forging temperature is 923-995°C, and the heat preservation is 4-6 hours. After being taken out of the furnace, it is upset on the free forging hammer, and the temperature is controlled at the same time, and the deformation is 30%-40%.

[0035] Furthermore, the deformation amount of upsetting and drawing in each working step is an upsetting ratio of 1:2 to 2.5 and a drawing ratio of 1.5 to 2:1.

[0036] Furthermore, the forging preheating temperature of the liquid end material is 860° C., and the heating coefficient is 0.2 min / mm.

[0037] Beneficial effects: The hydraulic end forging optimization process method of the present invention can effectively improve the plasticity and forgeability of the material by optimizing the forging process of the hydraulic end, thereby ensuring the mechanical properties such as strength and toughness of the hydraulic end forging, and has potential application prospects and practical value in the field of steel metallurgical industry. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 It is a flow chart of the forging optimization method of the hydraulic end forging of the present invention;

[0039] Figure 2 It is a schematic diagram of the hydraulic end forging product of the present invention;

[0040] Figure 3 The carbon equivalent-melting point / liquidus / initial forging temperature curve of the hydraulic end forging of the present invention;

[0041] Figure 4 The carbon equivalent-Ac3 temperature point curve of the hydraulic end forging of the present invention;

[0042] Figure 5 is the carbon equivalent of the hydraulic end forging of the present invention -T 常 Relationship curve;

[0043] Figure 6 The carbon equivalent-K value relationship curve of the hydraulic end forging of the present invention;

[0044] Figure 7 It is the temperature-density curve diagram of the hydraulic end forging of the present invention;

[0045] Figure 8 This is a grain size morphology diagram of the hydraulic end forging of the present invention. DETAILED DESCRIPTION

[0046] The present invention is further explained below in conjunction with the accompanying drawings and specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. After reading the present invention, various equivalent forms of modifications to the present invention by those skilled in the art all fall within the scope defined by the claims attached to this application.

[0047] See also Figure 1 and Figure 2 As shown, the hydraulic end forging optimization process method of the present invention comprises the following steps:

[0048] Step 1: The temperature-density curve of the hydraulic end material is established by a high-temperature volume measurement test for hydraulic end materials with different carbon equivalents, and the equilibrium phase diagram is established by a thermodynamic equilibrium test;

[0049] The temperature-density curve of the liquid end material is expressed by the following formula:

[0050] δ=-5E-08t 2 -0.0003t+7.866, R 2 =1

[0051] Where: δ is material density; t is temperature, the temperature range is [20, 1200], R 2 Indicates the goodness of fit.

[0052] Step 2: Using the temperature-density curve and equilibrium phase diagram of the liquid end material, establish the carbon equivalent and liquidus curve, the carbon equivalent and melting point curve, and the carbon equivalent and Ac3 temperature point curve of the liquid end material to obtain the melting point temperature and Ac3 phase transition point temperature of the liquid end material;

[0053] The melting point curve of the liquid end material is expressed by the following formula:

[0054] z = -54.164x + 1599.8, R 2 =0.9979

[0055] Where: z is the melting point temperature; x is the carbon equivalent, the carbon equivalent range is [3.28, 4.19], R 2 Indicates the goodness of fit.

[0056] The liquidus curve of the liquid end material is expressed by the following formula:

[0057] y=-49.763x+1639.7,R 2 =0.9848

[0058] Where: y is the liquidus temperature; x is the carbon equivalent, the carbon equivalent range is [3.28, 4.19], R 2 Indicates the goodness of fit.

[0059] The relationship curve between the carbon equivalent of the liquid end material and the Ac3 temperature point is expressed by the following formula:

[0060] u=4.1284x 2 +60.805x+634.98, R 2 =0.9953

[0061] Where: u is the Ac3 temperature point; x is the carbon equivalent, 3.28≤x≤4.18; R 2 represents the goodness of fit;

[0062] Step 3, using the melting point temperature and Ac3 phase transition point temperature of the liquid end material obtained in step 2, determine the initial forging temperature and the final forging temperature of the liquid end material;

[0063] See also Figure 5 and Figure 6 As shown, the initial forging temperature of the fluid end material is expressed by the following formula:

[0064] T 始 =T 熔 -T 常

[0065] Among them, T 常 Calculated by the following formula:

[0066] T 常 =28.274x 2 -158.32x+365.92, R 2 =0.9933

[0067] Where, T 始 is the initial forging temperature, T 熔 is the melting point temperature, T 常 is a constant, T 常 The range is [150, 200], x is the carbon equivalent, the carbon equivalent range is [3.28, 4.19], R 2 Indicates the goodness of fit.

[0068] The final forging temperature of the fluid end material is expressed by the following formula:

[0069] v 终 =Ac3+K

[0070] The K value is calculated by the following formula:

[0071] K = 3.6217x 2 -65.376x+225.32, R 2 =0.9992

[0072] Where, T 终is the final forging temperature, Ac3 is the austenite phase transformation temperature, K is a constant, K range is [15, 50], x is the carbon equivalent, the carbon equivalent range is [3.28, 4.19], R 2 Indicates the goodness of fit.

[0073] Step 4: According to step 3, the initial forging temperature and the final forging temperature of the liquid end material are obtained, and the forging process of the liquid end material is optimized.

[0074] Preferably, the mass percentages of the components in the liquid end material of the present invention are: C≤0.07%, Si≤1.0%, Mn≤1.00%, P≤0.040%, S≤0.030%, Cr: 14.00-15.50%, Ni: 3.50-5.50%, Mo≤0.50%, Cu: 2.50-4.50%, and the rest is Fe.

[0075] The hydraulic end forging optimization process method of the present invention can effectively improve the plasticity and forgeability of the material by optimizing the forging process of the hydraulic end, thereby ensuring the mechanical properties such as strength and toughness of the hydraulic end forging, and has potential application prospects and practical value in the field of steel metallurgical industry.

[0076] Embodiment 1:

[0077] See also Figure 1 and Figure 2 As shown, forging process and steps:

[0078] 1. Select the material, 15-5PH precipitation hardened stainless steel;

[0079] 2. Preheating: The material of the hydraulic end is selected as a multi-faceted steel ingot, and the tooling and tools are preheated to 300°C before forging; the material is preheated at 860°C before entering the furnace;

[0080] 3. Upsetting: The material is heated to 1180℃, kept at temperature for 5 hours, with a heating coefficient of 0.3min / mm. After the material is kept at temperature for the set time, it is immediately taken out of the furnace and upset on the free forging hammer while controlling the temperature. The deformation is 38%; it is upset along the length of the ingot, and the forging upsetting ratio is 1:2.2;

[0081] 4. Drawing: Heat the material in the furnace, draw it out of the furnace, draw it axially, and then draw the flat square section of the material after upsetting, with a drawing ratio of 1.8:1;

[0082] 4. Use the FM forging method with upper flat anvil and lower platform. After drawing 10 times according to the process size, lightly chamfer about 25mm, chop and remove the forging defects at both ends to obtain the step shaft forging blank, and finally trim it.

[0083] Embodiment 2:

[0084] See also Figure 3-6As shown, the carbon equivalent-liquidus curve, carbon equivalent-melting point curve and carbon equivalent-Ac3 temperature point of the hydraulic end material are:

[0085] The carbon equivalent range is [3.28, 4.19], and the liquidus curve fitting function of the hydraulic end material is

[0086] y=-49.763x+1639.7,R 2 =0.9979

[0087] Where: y is the liquidus temperature, °C; x is the carbon equivalent, %; R 2 is the fitting correlation coefficient, indicating the goodness of fit;

[0088] The carbon equivalent range is [3.28, 4.19], and the melting point curve fitting function of the hydraulic end material is

[0089] z = -54.164x + 1599.8, R 2 =0.9848

[0090] Where: z is the melting point temperature, °C; x is the carbon equivalent, %; R 2 is the fitting correlation coefficient, indicating the goodness of fit;

[0091] The carbon equivalent range is [3.28, 4.19], and the Ac3 temperature point curve fitting function of the hydraulic end material is:

[0092] u=4.1284x 2 +60.805x+634.98, R 2 =0.9953

[0093] Where: u is the Ac3 temperature point; x is the carbon equivalent, %, 3.28≤x≤4.18; R 2 represents the goodness of fit;

[0094] The relationship between different carbon equivalents and melting points and liquidus points is shown in Table 1.

[0095] See also Figure 5 and Figure 6 As shown, the initial forging temperature of the fluid end material is expressed by the following formula:

[0096] T 始 =T 熔 -T 常

[0097] Among them, T 常 Calculated by the following formula:

[0098] T 常 =28.274x 2 -158.32x+365.92, R 2=0.9933

[0099] Where, T 始 is the initial forging temperature, T 熔 is the melting point temperature, T 常 is a constant, T 常 The range is [150, 200], x is the carbon equivalent, the carbon equivalent range is [3.28, 4.19], R 2 represents the goodness of fit;

[0100] The final forging temperature of the fluid end material is expressed by the following formula:

[0101] T 终 =Ac3+K

[0102] The K value is calculated by the following formula:

[0103] K = 3.6217x 2 -65.376x+225.32, R 2 =0.9992

[0104] Where, T 终 is the final forging temperature, Ac3 is the austenite phase transformation temperature, K is a constant, K range is [15, 50], x is the carbon equivalent, the carbon equivalent range is [3.28, 4.19], R 2 Indicates the degree of fit.

[0105] Example 3: Establishing a temperature-density curve:

[0106] See also Figure 7 As shown, based on the material composition, the temperature-density curve is established by high temperature volume measurement test

[0107] The heating temperature is [20, 1200], and the density curve fitting function of the hydraulic end material is:

[0108] δ=-5E -08 t 2 -0.0003t+7.866, R 2 =1

[0109] Where: δ material density, g / cm 3 ; t is temperature, ℃, %; R 2 is the fitting correlation coefficient, indicating the goodness of fit;

[0110] Table 1 Carbon equivalent, melting point, liquidus point data table

[0111]

[0112] According to Table 1, the general initial forging temperature range of the chemical composition range of the hydraulic end material is 1170-1270°C, and the general final forging temperature range is 923-995°C.

[0113] According to the characteristics of the above-mentioned liquid end material, the forging process of the liquid end material is optimized as follows:

[0114] The forging preheating temperature of the hydraulic end material is 850℃±50℃, the heating coefficient is 0.2~0.3min / mm, the forging heating temperature is 1170~1270℃, the heating coefficient is 0.3~0.4min / mm, and after keeping warm for the set time, it is immediately taken out of the furnace and upset on the free forging hammer, while controlling the temperature, the deformation is 30%~40%, so that the material is close to the forming size, and the upsetting deformation of each step is 1:2~2.5 for the upsetting ratio and 1.5~2:1 for the elongation ratio. Preferably, the forging preheating temperature of the hydraulic end material is 860℃, and the heating coefficient is 0.2min / mm.

[0115] See also Figure 8 As shown, it has been verified by experiments that the internal structure of the hydraulic end material after forging can obtain a dense structure without defects such as holes and looseness, and the grain size range of the forged material is 6.0 to 7.5.

[0116] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any technician familiar with the profession, without departing from the scope of the technical solution of the present invention, according to the technical essence of the present invention, any simple modification, equivalent replacement and improvement made to the above embodiment still falls within the protection scope of the technical solution of the present invention.

Claims

1. A method for optimizing the forging process of a hydraulic end, characterized in that: The following steps are involved: Step 1: The temperature-density curve of the hydraulic end material is established by a high-temperature volume measurement test for hydraulic end materials with different carbon equivalents, and the equilibrium phase diagram is established by a thermodynamic equilibrium test; Step 2: Using the temperature-density curve and equilibrium phase diagram of the liquid end material, establish the carbon equivalent and liquidus curve, the carbon equivalent and melting point curve, and the carbon equivalent and Ac3 temperature point curve of the liquid end material to obtain the melting point temperature and Ac3 phase transition point temperature of the liquid end material; Step 2 The melting point curve of the liquid end material is expressed by the following formula: T 熔 =-54.164x+1599.8,R 2 =0.9979 Where: T 熔 is the melting point temperature; x is the carbon equivalent, the carbon equivalent range is [3.28, 4.19], R 2 represents the goodness of fit; Step 2 The relationship curve between the carbon equivalent of the liquid end material and the Ac3 temperature point is expressed by the following formula: Ac3 =4.1284x 2 +60.805x+634.98,R 2 =0.9953 Where: Ac3 is the Ac3 temperature point; x is the carbon equivalent, 3.28≤x≤4.18; R 2 represents the goodness of fit; Step 3, using the melting point temperature and Ac3 phase transition point temperature of the liquid end material obtained in step 2, determine the initial forging temperature and the final forging temperature of the liquid end material; The initial forging temperature of the fluid end material in step 3 is expressed by the following formula: , in, T 常 Calculated by the following formula: T 常 =28.274x 2 -158.32x+365.92,R 2 =0.9933 In the formula, T 始 is the initial forging temperature, T 熔 is the melting point temperature, T 常 is a constant, T 常 The range is [150, 200], x is the carbon equivalent, the carbon equivalent range is [3.28, 4.19], R 2 represents the goodness of fit; The final forging temperature of the fluid end material in step 3 is expressed by the following formula: , in, K The value is calculated by the following formula: K =3.6217x 2 -65.376x+225.32,R 2 =0.9992 In the formula, T 终 is the final forging temperature, Ac3 is the austenite transformation temperature, K is a constant, K The range is [15, 50], x is the carbon equivalent, the carbon equivalent range is [3.28, 4.19], R 2 represents the goodness of fit; Step 4: According to step 3, the initial forging temperature and the final forging temperature of the liquid end material are obtained, and the forging process of the liquid end material is optimized.

2. The method for optimizing the forging process of the hydraulic end according to claim 1, characterized in that: The mass percentages of the components in the liquid end material are: C≤0.07%, Si≤1.0%, Mn≤1.00%, P≤0.040%, S≤0.030%, Cr: 14.00-15.50%, Ni: 3.50-5.50%, Mo≤0.50%, Cu: 2.50-4.50%, and the rest is Fe.

3. The method for optimizing the forging process of the hydraulic end according to claim 1, characterized in that: Step 2 The liquidus curve of the liquid end material is expressed by the following formula: <h2 style=";text-align:left;direction:ltr">y=-49.763x+1639.7,R<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> =0.9848 Where: y is the liquidus temperature; x is the carbon equivalent, the carbon equivalent range is [3.28, 4.19], R 2 Indicates the goodness of fit.

4. The method for optimizing the forging process of the hydraulic end according to claim 1, characterized in that: The temperature-density curve of the liquid end material in step 1 is expressed by the following formula: δ=-5E-08t 2 -0.0003t+7.866,R 2 =1 Where: δ material density; t is temperature, the temperature range is [20, 1200], R 2 Indicates the goodness of fit.

5. The method for optimizing the forging process of the hydraulic end according to claim 1, characterized in that: In step 4, the hydraulic end material is forged according to the initial forging temperature and final forging temperature of the hydraulic end material obtained in step 3, specifically: the forging preheating temperature of the hydraulic end material is 850°C ± 50°C, the heating coefficient is 0.2-0.3min / mm, the forging heating temperature is 1170-1270°C, the heating coefficient is 0.3-0.4min / mm, and the heat preservation is 4-6 hours. The final forging temperature is 923-995°C, and the heat preservation is 4-6 hours. After being taken out of the furnace, it is upset on the free forging hammer, and the temperature is controlled at the same time, and the deformation is 30%-40%.

6. The method for optimizing the forging process of the hydraulic end according to claim 5, characterized in that: The deformation of upsetting and drawing in each working step is that the upsetting ratio is 1:2~2.5, and the drawing ratio is 1.5~2:1.