A flexible silicon heterojunction solar cell with high photoelectric conversion efficiency and a method for manufacturing the same
By depositing specific layers of amorphous silicon and nanocrystalline layers on the silicon base layer, and combining plasma-enhanced chemical vapor deposition and gas pretreatment technology, high-efficiency and bendable silicon heterojunction solar cells are prepared, solving the problems of traditional crystalline silicon heterojunction solar cells. Silicon solar cells achieve high-efficiency conversion and increased flexibility despite their application limitations in extreme environments.
Patent Information
- Application Number
- CN202311478687.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-08
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-11-08
AI Technical Summary
Traditional crystalline silicon solar cells have low energy conversion efficiency, high cost, and are inflexible, which limits their application in extreme environments, especially in satellites, spacecraft, and drones.
A hydrogenated amorphous silicon oxide layer, a hydrogenated amorphous silicon layer, an n-type hydrogenated nanocrystalline silicon oxide layer and a transparent conductive oxide layer are sequentially deposited on the silicon base layer, and a hydrogenated amorphous silicon oxide layer, hydrogenated amorphous silicon oxide layer, and hydrogenated amorphous silicon oxide layer are sequentially deposited on the back. The silicon layer and p-type hydrogenated nanocrystalline silicon layer are combined with non-contact laser transfer printing technology to prepare metal electrodes. The passivation layer and doped contact layer are formed through plasma enhanced chemical vapor deposition and gas pretreatment technology to improve the photoelectric conversion efficiency of the battery. and flexibility.
It achieves an improvement in photoelectric conversion efficiency in silicon heterojunction solar cells with a thickness below 130 μm, reaching 26.06% to 26.79%, and significantly improves the flexibility of the cell, making it suitable for applications requiring high weight and flexibility.
Smart Images

Figure CN117766640B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a bendable silicon heterojunction solar cell with high photoelectric conversion efficiency, and also relates to a method for preparing the silicon heterojunction solar cell. Background Art
[0002] Solar energy has attracted much attention as a renewable energy source due to the growing demand for energy and the urgent need for environmentally friendly energy. However, traditional crystalline silicon solar cells are limited by their energy conversion efficiency, cost and inflexibility, which restricts their application areas.
[0003] In order to improve the efficiency of solar cells and reduce costs, researchers have begun to focus on the potential of crystalline silicon heterojunction solar cells. This type of solar cell uses crystalline silicon (c-Si) as the substrate material and introduces amorphous silicon on its surface or interface to form a heterojunction, thereby improving the light absorption and carrier separation efficiency of the cell.
[0004] Existing c-Si solar cells account for more than 95% of the solar cell market, and their wafer thickness is usually 150 to 180 μm. This thickness makes them unsuitable for use in some extreme environments (such as satellites, spacecraft and drones), so higher requirements are placed on the weight reduction and flexibility of solar cells. Currently, reducing the thickness of c-Si wafers to be much thinner than typical c-Si solar cells and incorporating the advantages of "thin-film solar cells" into c-Si solar cells is a hot topic. However, the power conversion efficiency of thin c-Si solar cells (55 to 130 μm) has been maintained in the range of 23.27 to 24.70% for decades. Summary of the invention
[0005] Purpose of the invention: The purpose of the present invention is to provide a silicon heterojunction solar cell that is bendable (thickness less than 130 μm) and has high photoelectric conversion efficiency; another purpose of the present invention is to provide a method for preparing the above-mentioned silicon heterojunction solar cell.
[0006] Technical solution: The bendable silicon heterojunction solar cell with high photoelectric conversion efficiency described in the present invention includes a silicon base layer; a hydrogenated amorphous silicon oxygen layer, a hydrogenated amorphous silicon layer, an n-type hydrogenated nanocrystalline silicon oxygen layer and a transparent conductive oxide layer are sequentially deposited on the front side of the silicon base layer; a hydrogenated amorphous silicon oxygen layer, a hydrogenated amorphous silicon layer, a p-type hydrogenated nanocrystalline silicon layer and a transparent conductive oxide layer are sequentially deposited on the back side of the silicon base layer; and a metal electrode is printed on the transparent conductive oxide layer.
[0007] Among them, the metal electrodes silk-screened on the transparent conductive oxide layer on the front and back sides of the silicon substrate layer are all in the form of grid lines; or the metal electrodes silk-screened on the transparent conductive oxide layer on the front side of the silicon substrate layer are in the form of grid lines, and the metal electrodes on the transparent conductive oxide layer on the back side of the silicon substrate layer are metal electrodes that fully cover the entire surface.
[0008] The silicon base layer is n-type single crystal silicon, the surface adopts a texturing structure, and the thickness of the silicon base layer is less than 130 μm.
[0009] The thickness of the hydrogenated amorphous silicon oxygen layer is less than 0.5 nm, the oxygen atom content is 8-12 at.%, and the hydrogen content is 22-30 at.%; the thickness of the hydrogenated amorphous silicon layer is 4-5 nm, and the hydrogen content is 18-25 at.%.
[0010] The thickness of the n-type hydrogenated nanocrystalline silicon oxygen layer is 12-18 nm, and the volume fraction of the crystal is 40-46%; the thickness of the p-type hydrogenated nanocrystalline silicon layer is 20-25 nm, and the volume fraction of the crystal is 60-66%.
[0011] The transparent conductive oxide layer is cerium-doped indium oxide with a thickness of 70nm; the metal electrode is a silver electrode. For double-sided cells, both the front and back sides are in the form of grid lines with a width of 16 to 18μm. For single-sided cells, the front side is in the form of grid lines, and the back side of the cell is fully covered with metal electrodes, that is, the back side is covered with silver paste.
[0012] The method for preparing the above silicon heterojunction solar cell comprises the following steps:
[0013] (1) Thinning and texturing the silicon substrate layer;
[0014] (2) Continuously plasma-enhanced chemical vapor deposition of a hydrogenated amorphous silicon oxide layer and a hydrogenated amorphous silicon layer on the silicon substrate to form a passivation layer; the present invention uses an ultra-thin hydrogenated amorphous silicon oxide layer and a hydrogenated amorphous silicon layer to form a composite, which can effectively reduce the adverse effects of the passivation layer on the conductivity of the battery, and can effectively protect the integrity and flatness of the passivation layer through process control, so that it has a good passivation effect;
[0015] (3) Plasma pretreatment is performed on the passivation layer using a mixture of CO2 and H2 to achieve nanocrystal seeding on the shallow surface of the passivation layer. The use of a mixed gas for plasma pretreatment can, on the one hand, enable nanocrystal seeding on the surface of the passivation layer, and the subsequent doped contact layer can grow vertically, thereby improving the conductivity of the battery; on the other hand, it can inhibit the reverse epitaxy of the seed layer, thereby ensuring the integrity of the passivation layer and avoiding damage to the passivation effect.
[0016] (4) under the gas flow ratio of high hydrogen silane, a phosphorus-doped n-type nanocrystalline silicon oxide layer is vertically grown on the nanocrystalline seeds of the passivation layer, and the volume fraction of the crystal is 40-46% (i.e., a specific proportion of amorphous silicon is converted into nanocrystalline silicon); further increasing the gas flow ratio of hydrogen silane, a boron-doped p-type nanocrystalline silicon layer is vertically grown on the nanocrystalline seeds of the back passivation layer, and the volume fraction of the crystal is 60-66%;
[0017] (5) Depositing cerium-doped indium oxide as a transparent conductive oxide layer, and then using non-contact laser transfer printing on the transparent conductive oxide layer.
[0018] In step (2), during the continuous deposition of the hydrogenated amorphous silicon oxide layer and the hydrogenated amorphous silicon layer on the silicon substrate layer, the gas resistance in the working chamber is monitored in real time by a gas resistance sensor, and the density is set at 18 to 19 cells / cm on the surface of the sample stage. 2 The diode (as a voltage sensor, feedback the bombardment intensity of the battery surface plasma) is used to detect the bombardment voltage on the battery surface. The resistance sensor transmits the collected gas resistance value and the voltage value of each point on the battery surface detected by the diode to the intelligent terminal of the system; the intelligent terminal switches the gas and adjusts the gas flow rate by controlling the opening of different types of gas inlet valves, so that the fluctuation value of the battery surface bombardment voltage is less than ±0.5% of the initial battery surface voltage value. Even during gas switching or gas flow rate adjustment, the gas resistance in the working chamber can be maintained constant, thereby achieving low damage to the surface of the passivation layer and avoiding damage to the passivation effect.
[0019] The specific process of continuously depositing the hydrogenated amorphous silicon oxide layer and the hydrogenated amorphous silicon layer is as follows: at 190°C, silane (SiH4) and CO2 are used as raw materials to grow an ultra-thin (<0.5nm) hydrogenated amorphous silicon oxide layer with a thickness of 2 to 3 atomic layers and resistant to epitaxial growth on both sides (front and back) of the silicon substrate layer; the gas flow ratio of CO2:SiH4 is 0.1 to 0.2:1; when transitioning from the hydrogenated amorphous silicon oxide layer to the hydrogenated amorphous silicon layer deposition, CO2 is switched to H2 inlet, and the gas flow ratio of H2:SiH4 is adjusted to 18 to 20%. 20:1, so that the plasma fluctuation voltage is <±0.5%, and another non-epitaxial hydrogenated amorphous silicon layer is deposited on the hydrogenated amorphous silicon oxygen sub-monolayer; the present invention can realize the continuous deposition of hydrogenated amorphous silicon oxygen layer and hydrogenated amorphous silicon layer on the silicon substrate layer, that is, it can realize the natural interface transition from the first passivation layer to the second passivation layer, and the whole passivation process protects the fine amorphous layer from plasma damage, especially the damage of the ultra-thin hydrogenated amorphous silicon oxygen layer, thereby effectively improving its ability to prevent epitaxial growth; the surface of the passivation layer obtained by the method of the present invention is complete, such as Figure 3 As shown, the photoelectric conversion efficiency of the battery of the present invention is greatly improved.
[0020] Wherein, in step (4), a phosphorus-doped n-type nanocrystalline silicon oxide layer is vertically grown on the nanocrystalline seeds of the passivation layer (hydrogenated amorphous silicon layer) under the conditions of a H2:SiH4:PH3 gas flow ratio of 720 to 780:5:0.1 and a CO2:SiH4 gas flow ratio of 0.5±0.2; the CO2 intake is disconnected, and the gas flow ratio of hydrogen silane is further increased to a H2:SiH4:B2H6 gas flow ratio of 2500 to 2900:5:0.1, and a boron-doped p-type nanocrystalline silicon layer is vertically grown on the nanocrystalline seeds of the back passivation layer.
[0021] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: the present invention can produce silicon heterojunction solar cells with a photoelectric conversion efficiency higher than 26% at a thickness of 55 to 130 μm, and obtain photoelectric conversion efficiencies of 26.06%, 26.19%, 26.50%, 26.56% and 26.79% at thicknesses of 57, 74, 84, 106 and 125 μm, respectively; among them, the open circuit voltage of the 57 μm thick battery reaches 761 mV, which is the highest value among current c-Si solar cells; the power-to-weight ratio of the 57 μm thick battery reaches 1.9 W·g -1 , which is the highest level of c-Si solar cells; at the same time, the thinning of the battery also brings a significant improvement in flexibility, so that the battery curvature radius can reach 19.6mm (57μm), which opens up new possibilities for drones, spacecraft and other applications that require extremely high weight and flexibility. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 It is a schematic structural diagram of a double-sided silicon heterojunction solar cell of the present invention;
[0023] Figure 2 This is a schematic structural diagram of a single-sided silicon heterojunction solar cell of the present invention;
[0024] Figure 3 This is a high-resolution transmission electron microscope photograph of the cross section of the silicon heterojunction solar cell of Example 1;
[0025] Figure 4 (a) is an atomic force microscope photograph and roughness of the passivation layer obtained by conventional discontinuous plasma enhanced chemical vapor deposition; (b) is an atomic force microscope photograph and roughness of the passivation layer obtained by low-damage continuous plasma enhanced chemical vapor deposition adopted in Example 1;
[0026] Figure 5 The relationship between the main performance of the silicon heterojunction solar cell of the present invention and the thickness;
[0027] Figure 6 The invention relates to the anti-potential induced degradation performance and the anti-light-induced degradation performance of the silicon heterojunction solar cell. DETAILED DESCRIPTION
[0028] Example 1
[0029] like Figure 1 As shown, the bendable silicon heterojunction solar cell with high photoelectric conversion efficiency of the present invention includes a silicon substrate layer 1; a hydrogenated amorphous silicon oxygen layer 2, a hydrogenated amorphous silicon layer 3, an n-type hydrogenated nanocrystalline silicon oxygen layer 4 and a transparent conductive oxide layer 6 are sequentially deposited on the front side of the silicon substrate layer 1; a hydrogenated amorphous silicon oxygen layer 2, a hydrogenated amorphous silicon layer 3, a p-type hydrogenated nanocrystalline silicon layer 5 and a transparent conductive oxide layer 6 are sequentially deposited on the back side of the silicon substrate layer 1; a metal electrode 7 is printed on the transparent conductive oxide layer 6; wherein the metal electrodes 7 printed on the transparent conductive oxide layer 6 on the front and back sides of the silicon substrate layer 1 are both in the form of grid lines.
[0030] Among them, the silicon base layer 1 is n-type single crystal silicon, the surface adopts a texturing structure, and the thickness of the silicon base layer 1 is 57μm; the thickness of the hydrogenated amorphous silicon oxygen layer 2 is less than 0.5nm, wherein the oxygen atom content is 10at.%, and the hydrogen content is 26.3at.%; the thickness of the hydrogenated amorphous silicon layer 3 is 4.5nm, wherein the hydrogen content is 19.2at.%; the thickness of the n-type hydrogenated nanocrystalline silicon oxygen layer 4 is 15nm, and the volume fraction of the crystal is 43.7%; the thickness of the p-type hydrogenated nanocrystalline silicon layer 5 is 22nm, and the volume fraction of the crystal is 63.4%; the transparent conductive oxide layer 6 is cerium-doped indium oxide, and the thickness is 70nm; the metal electrode 7 is a silver electrode, and the width of the silver electrode in the form of a gate line is 18μm.
[0031] The method for preparing the above silicon heterojunction solar cell comprises the following steps:
[0032] (1) The silicon substrate layer is thinned and textured, specifically: the silicon wafer is selected as an n-type Czochralski c-Si single crystal silicon with a thickness of 150 μm and a size of M6 (166×166 mm±0.25), with a (100) orientation and a resistivity of 1 to 3 Ω·cm; the silicon wafer is immersed in a KOH solution with a mass fraction of 10% for isotropic chemical etching, and the etching time is about 1200 s to reduce the thickness of the wafer; the silicon wafer is textured in the KOH solution with an additive added to form a tetrahedral pyramid with a size of 3 to 9 μm and an exposed (111) crystal plane on the wafer surface, and then chemically etched with a HF solution with a mass fraction of 1 to 2% to remove the natural SiO on the wafer surface. x The average thickness of each group of wafers was measured by weighing method with an accuracy of ±0.5μm;
[0033] (2) continuously depositing a hydrogenated amorphous silicon oxide layer and a hydrogenated amorphous silicon layer on the silicon substrate layer to form a passivation layer, specifically: using a radio frequency enhanced plasma chemical vapor deposition (RF-PECVD) (13.56MHz) system, at 190°C, using SiH4 and CO2 as raw gas to grow an ultra-thin (<0.5nm) hydrogenated amorphous silicon oxide layer with a thickness of 2 to 3 atomic layers and capable of resisting epitaxial growth on both sides (front and back sides) of the silicon substrate layer; the gas flow ratio of CO2:SiH4 is 0.15:1; when transitioning from the hydrogenated amorphous silicon oxide layer to the hydrogenated amorphous silicon layer deposition, CO2 is switched to H2 inlet gas, and the gas flow ratio of H2:SiH4 is adjusted to 19:1, so that the plasma fluctuation voltage is <±0.5%, and another non-epitaxial hydrogenated amorphous silicon layer is deposited on the hydrogenated amorphous silicon oxide sub-monolayer;
[0034] During the continuous deposition of hydrogenated amorphous silicon oxide layer and hydrogenated amorphous silicon layer on the silicon substrate layer, the gas resistance in the working chamber is monitored in real time by a gas resistance sensor, and the density is set at 18 to 19 / cm on the battery surface. 2 The diode (voltage sensor, used to feedback the bombardment intensity (bombardment voltage) of the battery surface plasma) is used to detect the bombardment voltage on the battery surface; the resistance sensor transmits the collected gas resistance value and the bombardment voltage value of each point on the battery surface detected by the diode to the intelligent terminal of the system; the intelligent terminal switches the gas and adjusts the intake flow rate of each gas by controlling the opening of each gas intake pipe valve, so that the fluctuation value of the battery surface bombardment voltage is less than ±0.5% of the initial battery surface voltage value;
[0035] (3) Plasma pretreatment is performed on the passivation layer using a mixture of CO2 and H2 to achieve seeding of nanocrystals on the surface of the passivation layer, specifically: a doped contact layer is prepared by a self-recovering nanocrystal seeding and vertical growth induction (NSVGI) method, and the surface of the hydrogenated amorphous silicon layer is pretreated with a mixture of CO2 and H2 by a very high frequency plasma chemical vapor deposition (VHF-PECVD) method (40.68 MHz) (the flow ratio of CO2:H2 is 1:20, and the treatment time is 20 to 50 s); nanocrystal seeds are seeded and the hydrogen content in the passivation layer is retained, so that the passivation layer maintains the best passivation effect, and at the same time, the nanocrystal seeding can be limited to the surface of the passivation layer, which can, on the one hand, induce the vertical growth of the subsequent doped nanocrystal junction, and on the other hand, will not destroy the passivation effect of the passivation layer;
[0036] (4) Under the conditions of H2:SiH4:PH3 gas flow ratio of 750:5:0.1 and CO2:SiH4 gas flow ratio of 0.5±0.2, a 15 nm thick phosphorus-doped n-type nanocrystalline silicon oxide layer (n + :nc-SiO x:H), as the electron collection layer, the volume fraction of the crystal is 43.7%, and the optical band gap is optimal under this crystallinity; for the back junction, the CO2 intake is disconnected, and the gas flow ratio of hydrogen silane is further increased to 2700:5:0.1. A 22nm thick boron-doped p-type nanocrystalline silicon layer (p + :nc-Si:H), the volume fraction of the crystal is 63.4%; n + :nc-SiO x :H and p + :nc-Si:H contacts are grown in the same chamber with a substrate temperature of 170°C; optimization of the crystal volume fraction of the doped contact layer can improve the fill factor and conversion efficiency of the cell;
[0037] (5) Using an indium oxide (In2O3) target doped with 2.8 wt.% Ce, a 70 nm cerium-doped indium oxide layer was deposited on both sides on a low-damage reactive plasma deposition (RPD) sputtering tool with high-purity argon (Ar) as the sputtering gas at a substrate temperature of 100°C. During the RPD process, the ion bombardment voltage was less than 30 eV to avoid damage to the nanocrystalline junction and the passivation layer; silver grid lines with a line width of 18 μm were printed by non-contact laser transfer, and the aspect ratio was optimized to 0.7;
[0038] (6) using a thermal evaporation device to cover the front of the battery with a 80 nm thick magnesium fluoride (MgF2) layer; or using a thermal evaporation device to cover both the front and back of the battery with a 80 nm thick MgF2 layer, either of which is acceptable;
[0039] (7) The current-voltage (JV) curve test was carried out under the AM 1.5 spectrum, and the photoelectric conversion efficiency was 26.06%.
[0040] Only the etching time is adjusted, and the other process parameters remain unchanged. The preparation process of Example 1 can also be used to obtain batteries with thicknesses of 74, 84, 106, and 125 μm. The JV curve test of the batteries with thicknesses of 74, 84, 106, and 125 μm under the AM 1.5 spectrum shows that the photoelectric conversion efficiencies are 26.19%, 26.50%, 26.56%, and 26.79%, respectively.
[0041] Figure 3 This is a high-resolution transmission electron microscopy picture of the cross section of the battery, where it can be observed that there is no epitaxial growth in the passivation layer and that the nanocrystals of the doped contact layer grow vertically; Figure 4 a: non-continuous plasma is used, the passivation layer has multiple holes and high damage; Figure 4 b. Using continuous plasma, the passivation layer is complete and smooth with low damage; Figure 5The performance parameters of batteries with different thicknesses (57-125 μm) prepared by the method of the present invention are shown. It can be seen that the battery obtained by the method of the present invention has good conversion efficiency, fill factor, open circuit voltage, and short circuit current.
[0042] Figure 6 Batteries with different thicknesses (57-125 μm) prepared by the method of the present invention all have reliable weather resistance.
[0043] Example 2
[0044] like Figure 2 As shown, the bendable silicon heterojunction solar cell with high photoelectric conversion efficiency of the present invention includes a silicon substrate layer 1; a hydrogenated amorphous silicon oxygen layer 2, a hydrogenated amorphous silicon layer 3, an n-type hydrogenated nanocrystalline silicon oxygen layer 4 and a transparent conductive oxide layer 6 are sequentially deposited on the front side of the silicon substrate layer 1; a hydrogenated amorphous silicon oxygen layer 2, a hydrogenated amorphous silicon layer 3, a p-type hydrogenated nanocrystalline silicon layer 5 and a transparent conductive oxide layer 6 are sequentially deposited on the back side of the silicon substrate layer 1; a metal electrode 7 is printed on the transparent conductive oxide layer 6; wherein the metal electrode 7 printed on the transparent conductive oxide layer 6 on the front side of the silicon substrate layer 1 is in the form of a grid line, and the transparent conductive oxide layer 6 on the back side of the silicon substrate layer 1 covers the metal electrode entirely.
[0045] Among them, the silicon base layer 1 is n-type single crystal silicon, the surface adopts a texturing structure, and the thickness of the silicon base layer 1 is 57μm; the thickness of the hydrogenated amorphous silicon oxygen layer 2 is less than 0.5nm, wherein the oxygen atom content is 10at.%, and the hydrogen content is 26.3at.%; the thickness of the hydrogenated amorphous silicon layer 3 is 4.5nm, wherein the hydrogen content is 19.2at.%; the thickness of the n-type hydrogenated nanocrystalline silicon oxygen layer 4 is 15nm, and the volume fraction of the crystal is 43.7%; the thickness of the p-type hydrogenated nanocrystalline silicon layer 5 is 22nm, and the volume fraction of the crystal is 63.4%; the transparent conductive oxide layer 6 is cerium-doped indium oxide, and the thickness is 70nm; the metal electrode 7 is a silver electrode, and the width of the silver electrode in the form of a grid line on the front of the battery is 18μm, and the back of the battery is fully covered, that is, the back is fully brushed with silver paste.
[0046] The method for preparing the above silicon heterojunction solar cell comprises the following steps:
[0047] (1) The silicon substrate layer is thinned and textured, specifically: the silicon wafer is selected as an n-type Czochralski c-Si single crystal silicon with a thickness of 150 μm and a size of M6 (166×166 mm±0.25), with a (100) orientation and a resistivity of 1 to 3 Ω·cm; the silicon wafer is immersed in a KOH solution with a mass fraction of 10% for isotropic chemical etching, and the etching time is about 1200 s to reduce the thickness of the wafer; the silicon wafer is textured in the KOH solution with an additive added to form a tetrahedral pyramid with a size of 3 to 9 μm and an exposed (111) crystal plane on the wafer surface, and then chemically etched with a HF solution with a mass fraction of 1 to 2% to remove the natural SiO on the wafer surface. x The average thickness of each group of wafers was measured by weighing method with an accuracy of ±0.5μm;
[0048] (2) continuously depositing a hydrogenated amorphous silicon oxide layer and a hydrogenated amorphous silicon layer on the silicon substrate layer to form a passivation layer, specifically: using an RF-PECVD (13.56 MHz) system, at 190° C., using SiH4 and CO2 as raw gas to grow an ultra-thin (<0.5 nm) hydrogenated amorphous silicon oxide layer with a thickness of 2 to 3 atomic layers and capable of resisting epitaxial growth on both sides (front and back sides) of the silicon substrate layer; the gas flow ratio of CO2:SiH4 is 0.15:1; when transitioning from the hydrogenated amorphous silicon oxide layer to the hydrogenated amorphous silicon layer deposition, CO2 is switched to H2 inlet gas, and the gas flow ratio of H2:SiH4 is adjusted to 19:1, so that the plasma fluctuation voltage is <±0.5%, and another non-epitaxial hydrogenated amorphous silicon layer is deposited on the hydrogenated amorphous silicon oxide sub-monolayer;
[0049] During the continuous deposition of hydrogenated amorphous silicon oxide layer and hydrogenated amorphous silicon layer on the silicon substrate layer, the gas resistance in the working chamber is monitored in real time by a gas resistance sensor, and the density is set at 18 to 19 / cm on the battery surface. 2 The diode (voltage sensor, used to feedback the bombardment intensity (bombardment voltage) of the battery surface plasma) is used to detect the bombardment voltage on the battery surface; the resistance sensor transmits the collected gas resistance value and the bombardment voltage value of each point on the battery surface detected by the diode to the intelligent terminal of the system; the intelligent terminal switches the gas and adjusts the intake flow rate of each gas by controlling the opening of each gas intake pipe valve, so that the fluctuation value of the battery surface bombardment voltage is less than ±0.5% of the initial battery surface voltage value;
[0050] (3) Plasma pretreatment is performed on the passivation layer using a mixture of CO2 and H2 to achieve seeding of nanocrystals on the surface of the passivation layer, specifically: a doped contact layer is prepared by the NSVGI method, and the surface of the hydrogenated amorphous silicon layer is pretreated with a mixture of CO2 and H2 plasma by a VHF-PECVD method (40.68 MHz) (the flow ratio of CO2:H2 is 1:20, and the treatment time is 20 to 50 s); nanocrystal seeds are seeded and the hydrogen content in the passivation layer is retained, so that the passivation layer maintains the best passivation effect, and at the same time, the seeding of nanocrystals can be limited to the surface of the passivation layer, which can, on the one hand, induce the vertical growth of the subsequent doped nanocrystal junction, and on the other hand, will not destroy the passivation effect of the passivation layer;
[0051] (4) Under the conditions of H2:SiH4:PH3 gas flow ratio of 750:5:0.1 and CO2:SiH4 gas flow ratio of 0.5±0.2, a 15 nm thick phosphorus-doped n-type nanoparticle was vertically grown on the passivation layer nanocrystal seed. + :nc-SiO x :H layer, as the electron collection layer, the volume fraction of the crystal is 43.7%, and the optical band gap is optimal under this crystallinity; for the back junction, the CO2 intake is disconnected, and the gas flow ratio of hydrogen silane is further increased to 2700:5:0.1. A 22nm thick boron-doped p-type nanoparticle is vertically grown on the nanocrystal seeds of the back passivation layer. + :nc-Si:H layer, the volume fraction of the crystal is 63.4%; n + :nc-SiO x :H and p + :nc-Si:H contacts are grown in the same chamber with a substrate temperature of 170°C; optimization of the crystal volume fraction of the doped contact layer can improve the fill factor and conversion efficiency of the cell;
[0052] (5) Using an In2O3 target doped with 2.8wt.% Ce, on a low-damage RPD sputtering tool, with high-purity Ar as the sputtering gas, at a substrate temperature of 100°C, a 70nm cerium-doped indium oxide layer was deposited on both sides. During the RPD process, the ion bombardment voltage was less than 30eV to avoid damage to the nanocrystalline junction and the passivation layer; a silver grid line with a line width of 18μm was printed on the front of the battery by non-contact laser transfer, and the aspect ratio was optimized to 0.7; and silver paste was applied to the back of the battery;
[0053] (6) using a thermal evaporation device to cover the front of the battery with a MgF2 layer of 80 nm thick; or using a thermal evaporation device to cover both the front and back of the battery with a MgF2 layer of 80 nm thick, either method is acceptable;
[0054] (7) The JV curve test was carried out under the AM 1.5 spectrum, and the photoelectric conversion efficiency was 26.11%.
Claims
1. A flexible silicon heterojunction solar cell with high photoelectric conversion efficiency, Features: The invention comprises a silicon base layer (1); a hydrogenated amorphous silicon oxide layer (2), a hydrogenated amorphous silicon layer (3), an n-type hydrogenated nanocrystalline silicon oxide layer (4) and a transparent conductive oxide layer (6) are sequentially deposited on the front side of the silicon base layer (1); a hydrogenated amorphous silicon oxide layer (2), a hydrogenated amorphous silicon layer (3), a p-type hydrogenated nanocrystalline silicon layer (5) and a transparent conductive oxide layer (6) are sequentially deposited on the back side of the silicon base layer (1); and a metal electrode (7) is printed on the transparent conductive oxide layer (6).
2. The bendable silicon heterojunction solar cell with high photoelectric conversion efficiency according to claim 1, Features: The metal electrodes (7) printed by non-contact laser transfer printing on the transparent conductive oxide layer (6) on the front and back sides of the silicon substrate layer (1) are both in the form of grid lines; or the metal electrodes (7) printed by non-contact laser transfer printing on the transparent conductive oxide layer (6) on the front side of the silicon substrate layer (1) are in the form of grid lines, and the transparent conductive oxide layer (6) on the back side of the silicon substrate layer (1) is fully covered with metal electrodes.
3. The bendable silicon heterojunction solar cell with high photoelectric conversion efficiency according to claim 1, Features: The silicon base layer (1) is n-type single crystal silicon, the surface of which adopts a textured structure, and the thickness of the silicon base layer (1) is less than 130 μm.
4. The bendable silicon heterojunction solar cell with high photoelectric conversion efficiency according to claim 1, Features: The thickness of the hydrogenated amorphous silicon oxygen layer (2) is less than 0.5 nm, wherein the oxygen atom content is 8-12 at.%, and the hydrogen content is 22-30 at.%. The thickness of the hydrogenated amorphous silicon layer (3) is 4-5 nm, wherein the hydrogen content is 18-25 at.%.
5. The bendable silicon heterojunction solar cell with high photoelectric conversion efficiency according to claim 1, Features: The thickness of the n-type hydrogenated nanocrystalline silicon oxide layer (4) is 12-18 nm, and the volume fraction of the crystal is 40-46%; the thickness of the p-type hydrogenated nanocrystalline silicon layer (5) is 20-25 nm, and the volume fraction of the crystal is 60-66%.
6. The bendable silicon heterojunction solar cell with high photoelectric conversion efficiency according to claim 1, Features: The transparent conductive oxide layer (6) is cerium-doped indium oxide; the metal electrode (7) is a silver electrode, and the width of the silver electrode in the form of a grid line is 16 to 18 μm.
7. The method for preparing the silicon heterojunction solar cell according to claim 1, It is characterized in that The following steps are involved: (1) Thinning and texturing the silicon substrate layer; (2) continuously depositing a hydrogenated amorphous silicon oxide layer and a hydrogenated amorphous silicon layer on the silicon base layer to form a composite passivation layer; (3) Utilization of carbon dioxide (CO 2 ) and hydrogen (H 2 ) The mixed gas performs plasma pretreatment on the passivation layers on both sides to achieve nanocrystal seeding on the shallow surface of the passivation layer; (4) under a high hydrogen silane gas flow ratio, a phosphorus-doped n-type nanocrystalline silicon oxide layer is vertically grown on the front passivation layer seeded with nanocrystals, and the volume fraction of the crystal is 40-46%; further increasing the hydrogen silane gas flow ratio, a boron-doped p-type nanocrystalline silicon layer is vertically grown on the back passivation layer seeded with nanocrystals, and the volume fraction of the crystal is 60-66%; (5) Depositing cerium-doped indium oxide as a transparent conductive oxide layer, and then using non-contact laser transfer printing on the transparent conductive oxide layer.
8. The method for preparing a silicon heterojunction solar cell according to claim 7, It is characterized in that In step (2), during the continuous deposition of the hydrogenated amorphous silicon oxide layer and the hydrogenated amorphous silicon layer on the silicon substrate layer, the gas resistance in the working chamber is monitored in real time by a gas resistance sensor, and the density is set to 18 to 19 cells / cm on the surface of the sample stage. 2 The diode is used to detect the plasma bombardment voltage on the battery surface; the resistance sensor transmits the collected gas resistance value and the voltage value of each point on the battery surface detected by the diode to the intelligent terminal of the system; the intelligent terminal switches the gas and adjusts the gas flow rate by controlling the opening of different types of gas inlet valves, so that the fluctuation value of the battery surface bombardment voltage is less than ±0.5% of the initial battery surface voltage value.
9. The method for preparing a silicon heterojunction solar cell according to claim 8, It is characterized in that The specific process of continuously depositing hydrogenated amorphous silicon oxide layer and hydrogenated amorphous silicon layer is as follows: first, at 190-200°C, silane and CO 2 As a raw material gas, a hydrogenated amorphous silicon oxide layer with a thickness of 2 to 3 atomic layers and capable of resisting epitaxial growth is grown on both sides of the silicon substrate layer; CO 2 :SiH 4 The gas flow ratio is 0.1 to 0.2:1; when transitioning from the hydrogenated amorphous silicon oxide layer to the hydrogenated amorphous silicon layer deposition, CO 2 Switch to H 2 Intake, adjust H 2 :SiH 4 The gas flow ratio is 18 to 20:1, so that the plasma voltage fluctuation on the cell surface is <±0.5%, and another epitaxial-free hydrogenated amorphous silicon layer is deposited on the hydrogenated amorphous silicon oxygen layer.
10. The method for preparing a silicon heterojunction solar cell according to claim 7, It is characterized in that In step (4), in H 2 :SiH 4 :PH 3 The airflow ratio is 720-780:5:0.1, CO 2 :SiH 4 When the gas flow ratio is 0.5±0.2, a phosphorus-doped n-type nanocrystalline silicon oxide layer is vertically grown on the passivation layer nanocrystal seeds on the front side of the cell. When the gas flow ratio of hydrogen silane is further increased to H 2 :SiH 4 :B 2 H 6 The airflow ratio is 2500-2900:5:0.1, and a boron-doped p-type nanocrystalline silicon layer is vertically grown on the passivation layer nanocrystalline seeds on the back of the battery.
Citation Information
Patent Citations
Heterojunction solar cell and preparation method thereof
CN106098835A
Novel microcrystalline-crystalline silicon laminated heterojunction battery structure and preparation method thereof
CN114188432A
Heterojunction solar cell
CN202549860U
Silicon heterojunction solar cell and photovoltaic module with novel projecting pole
CN205920977U
Silicon Heterojunction Solar Cells
US20130180578A1