A method for fabricating a flip-chip LED and the LED chip itself.

By using screen printing technology and specific mixed pastes, the electrode structure of flip-chip LEDs was optimized, solving the problems of metal waste and brightness improvement, achieving better conductivity and heat dissipation performance, and reducing power consumption.

CN117766660BActive Publication Date: 2026-11-17JIANGXI ZHAO CHI SEMICON CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311804066.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-26
Publication Date
2026-11-17
Estimated Expiration
2043-12-26

AI Technical Summary

Technical Problem

Flip-chip LEDs suffer from significant metal waste during the evaporation process, and their brightness needs further improvement. Existing structures also suffer from issues with the work function matching between the metal and gallium nitride, resulting in poor heat dissipation and current expansion.

Method used

The first and second electrode layers were prepared using a screen printing process, employing a mixed paste containing Ni, Au, Ag, Al, Pd, and Pt, combined with a reflective layer consisting of a SiO2 layer and a Ti3O5 layer, to optimize work function matching and current spread.

Benefits of technology

Reduce metal waste, improve conductivity and reflectivity, reduce power consumption, increase chip brightness, and save costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117766660B_ABST
    Figure CN117766660B_ABST
Patent Text Reader

Abstract

This invention relates to the field of semiconductor device technology, and more particularly to a method for fabricating a flip-chip LED and the LED chip itself. The chip fabrication method includes: providing a substrate; depositing an epitaxial layer on the substrate, the epitaxial layer comprising, from bottom to top, an N-type GaN layer, a quantum well light-emitting layer, and a P-type GaN layer; etching the epitaxial layer to expose the N-type GaN layer and form an N-type conductive step; depositing a current blocking layer on the P-type GaN layer; depositing a current spreading layer on the current blocking layer to form an initial chip; screen printing a first mixed paste on the initial chip to form a first electrode layer; depositing a reflective layer on the first electrode layer to form an intermediate chip; and screen printing a second mixed paste on the intermediate chip to form a second electrode layer. In this invention, the first and second electrode layers are fabricated using screen printing technology, improving the chip electrode structure and optimizing the work function matching, thereby enhancing the chip's brightness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of semiconductor device technology, and in particular to a method for fabricating a flip-chip LED and the LED chip itself. Background Technology

[0002] Currently, in LED chips, conventional LED chips are prone to poor heat dissipation and localized current accumulation. In contrast, flip-chip LED chips extract light from the sapphire substrate, while the mirror layer is integrated with the electrode layer. The advantage of this design is that the electrodes are typically made of highly thermally conductive metals, resulting in strong heat dissipation. The light-emitting surface is not obstructed by the electrodes, allowing for maximum electrode enlargement and better current distribution. Due to their advantages such as good heat dissipation, low voltage, high brightness, and high reliability, flip-chip LEDs are highly popular in high-power and outdoor lighting applications, and their application is becoming increasingly mature.

[0003] When the metal electrode film is formed in all directions during the evaporation process of flip-chip LEDs, the metal is easily wasted due to the evaporation of metal in all directions. There is also a work function matching problem between the metal and N-type gallium nitride and P-type gallium nitride. Moreover, the brightness of existing flip-chip LEDs needs to be further improved to meet user needs. Summary of the Invention

[0004] To address the aforementioned technical problems, this invention provides a method for fabricating a flip-chip LED and the LED chip itself.

[0005] This invention adopts the following technical solution: a method for fabricating a flip-chip LED, the method comprising:

[0006] Provide a substrate;

[0007] An epitaxial layer is deposited on the substrate, the epitaxial layer comprising, from bottom to top, an N-type GaN layer, a quantum well light-emitting layer, and a P-type GaN layer;

[0008] The epitaxial layer is etched to expose the N-type GaN layer and form N-type conductive steps;

[0009] A current blocking layer is deposited on the P-type GaN layer;

[0010] A current spreading layer is deposited on the current blocking layer to form an initial chip;

[0011] A first mixed paste is printed on the initial chip using a screen printing process to form a first electrode layer; wherein the first mixed paste comprises Ni, Au, Ag, Al, Pd and Pt;

[0012] A reflective layer is deposited on the first electrode layer to form an intermediate chip;

[0013] A second mixed paste is printed on the intermediate chip using a screen printing process to form a second electrode layer. The second electrode layer corresponds to and is connected to the first electrode layer, thereby obtaining a flip-chip LED chip. The second mixed paste contains Au, Al, Pt and Sn.

[0014] The present invention discloses a method for fabricating a flip-chip LED. By employing screen printing to prepare the first and second electrode layers, the waste of raw materials generated during the metal evaporation process can be effectively reduced, saving costs. Furthermore, the work functions of Ni, Au, Pd, and Pt in the first mixed paste are relatively close to those of gallium nitride, enabling good ohmic contact. Specifically, the work function of Pd is well-connected with the work functions of the current spreading layer and the N-type GaN layer, while the work function of Pt is relatively close to that of the P-type GaN layer. This combination achieves high reflectivity and good ohmic contact, further enhancing conductivity. While Ag and Al have slightly lower work functions, they significantly improve reflectivity, and Pd can suppress the electromigration of Ag. Additionally, the second mixed paste exhibits good conductivity, high reflectivity, and strong thermal conductivity, while also enabling better die bonding. This effectively improves the electrode structure of the flip-chip LED and optimizes the matching of work functions, reducing power consumption and increasing brightness.

[0015] Furthermore, the weight fractions of Ni, Au, Ag, Al, Pd, and Pt in the first mixed slurry range from 5wt% to 10wt%, 5wt% to 20wt%, 10wt% to 25wt%, 10wt% to 40wt%, 15wt% to 20wt%, and 15wt% to 30wt%, respectively.

[0016] Furthermore, the weight fractions of Au, Al, Pt, and Sn in the second mixed slurry range from 15wt% to 30wt%, 20wt% to 40wt%, 20wt% to 25wt%, and 20wt% to 40wt%, respectively.

[0017] Furthermore, the step of printing a first mixed paste onto the initial chip using a screen printing process to form a first electrode layer includes:

[0018] Photoresist is coated on the N-type conductive step and the current spreading layer. A first P-type exposure plate is used to expose the photoresist on the current spreading layer in a first P-type manner, and a first N-type exposure plate is used to expose the photoresist on the N-type conductive step in a first N-type manner. The photoresist is then developed to generate a first P-type electrode hole and a first N-type electrode hole.

[0019] The initial chip is placed on a screen printing machine. A first screen printing screen adapted to the first P-type electrode hole and the first N-type electrode hole is used to assemble the first mixed paste on the first screen printing screen. The screen printing machine is then turned on to perform the screen printing process to form the first electrode layer.

[0020] The first electrode layer includes a first P-type electrode layer corresponding to the first P-type electrode hole and a first N-type electrode layer corresponding to the first N-type electrode hole.

[0021] Furthermore, the energy of the first P-type exposure is 250 kJ / cm². 2 -350kJ / cm 2 The energy of the first N-type exposure is 450 kJ / cm. 2 -550kJ / cm 2 The thickness of the first P-type electrode layer is 3.5μm-4.5μm, and the thickness of the first N-type electrode layer is 5μm-6μm.

[0022] Furthermore, the reflective layer is composed of SiO2 layers and Ti3O5 layers stacked alternately in a periodic manner. The number of alternating stacking periods of the reflective layer is 10 to 20, and the thickness of the SiO2 layer in each alternating stacking period is greater than the thickness of the Ti3O5 layer.

[0023] Furthermore, the step of printing a second mixed paste onto the intermediate chip using a screen printing process to form a second electrode layer includes:

[0024] Photoresist is coated on the reflective layer, and the photoresist on the reflective layer is exposed a second time using a second exposure plate and then developed to generate a second P-type electrode hole and a second N-type electrode hole.

[0025] The intermediate chip is placed on a screen printing machine. A second screen printing screen adapted to the second P-type electrode hole and the second N-type electrode hole is used to assemble the second mixed paste on the second screen printing screen. The screen printing machine is then turned on to perform the screen printing process to form the second electrode layer.

[0026] The second electrode layer includes a second P-type electrode layer corresponding to the second P-type electrode hole and a second N-type electrode layer corresponding to the second N-type electrode hole.

[0027] Furthermore, the energy of the second exposure is 250 kJ / cm². 2 -350kJ / cm 2 The thickness of both the second P-type electrode layer and the second N-type electrode layer is 3.6μm-4μm.

[0028] Furthermore, the current blocking layer has a thickness between The SiO2 layer.

[0029] The present invention also proposes a flip-chip LED, which is prepared according to the flip-chip LED preparation method described in any one of the above claims. Attached Figure Description

[0030] To more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0031] Figure 1 This is a flowchart of the method for preparing the flip-chip LED of the present invention;

[0032] Figure 2 for Figure 1 A schematic diagram of the structure corresponding to step S6, where photoresist is coated on the N-type conductive step and current spreading layer.

[0033] Figure 3 for Figure 1 In step S6, a first P-type exposure plate is used to perform first P-type exposure on the photoresist on the current spreading layer. (Corresponding structural schematic diagram)

[0034] Figure 4 for Figure 1 In step S6, a first N-type exposure plate is used to perform first N-type exposure and development on the photoresist on the N-type conductive step. (Corresponding structural schematic diagram)

[0035] Figure 5 for Figure 1 A schematic diagram of the structure corresponding to the screen printing process performed in step S6;

[0036] Figure 6 for Figure 1 A schematic diagram of the structure corresponding to the formation of the first electrode layer in step S6;

[0037] Figure 7 for Figure 1 A schematic diagram of the corresponding structure in step S7;

[0038] Figure 8 for Figure 1 A schematic diagram of the structure corresponding to step S8, where photoresist is coated on the reflective layer;

[0039] Figure 9 for Figure 1In step S8, a second exposure plate is used to perform a second exposure and development on the photoresist on the reflective layer. (Corresponding structural schematic diagram)

[0040] Figure 10 for Figure 1 In step S8, a screen printing process is performed to form the corresponding structural diagram of the second electrode layer;

[0041] Figure 11 This is a schematic diagram of the structure of the first P-type exposure plate of the present invention;

[0042] Figure 12 This is a schematic diagram of the structure of the first N-type exposure plate of the present invention;

[0043] Figure 13 This is a schematic diagram of the structure of the second exposed version of the present invention.

[0044] Explanation of reference numerals in the attached figures:

[0045] 10. Substrate; 11. Epitaxial layer; 111. N-type GaN layer; 112. Quantum well light-emitting layer; 113. P-type GaN layer; 12. Current blocking layer; 13. Current spreading layer; 14. First electrode layer; 141. First P-type electrode layer; 142. First N-type electrode layer; 143. First P-type electrode hole; 144. First N-type electrode hole; 15. Reflective layer; 16. Second electrode layer; 161. Second P-type electrode layer; 162. Second N-type electrode layer; 163. Second P-type electrode hole; 164. Second N-type electrode hole; 17. First P-type exposure plate; 18. First N-type exposure plate; 19. Second exposure plate. Detailed Implementation

[0046] Embodiments of the present invention are described in detail below, examples of which are illustrated in the accompanying drawings, wherein the same or similar reference numerals denote the same or similar elements or elements having the same or similar functions throughout. The embodiments described below with reference to the accompanying drawings are exemplary and intended to explain embodiments of the present invention, and should not be construed as limiting the present invention.

[0047] In the description of the embodiments of the present invention, it should be understood that the terms "length", "width", "upper", "lower", "front", "rear", "left", "right", "vertical", "horizontal", "top", "bottom", "inner", "outer", etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are only for the convenience of describing the embodiments of the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on the present invention.

[0048] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of that feature. In the description of embodiments of the present invention, "a plurality of" means two or more, unless otherwise explicitly specified.

[0049] In the embodiments of the present invention, unless otherwise explicitly specified and limited, the terms "installation," "connection," "linking," "fixing," etc., should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral part; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; they can refer to the internal communication of two components or the interaction between two components. Those skilled in the art can understand the specific meaning of the above terms in the embodiments of the present invention according to the specific circumstances.

[0050] Example 1

[0051] Reference Figures 1 to 13 According to the first embodiment of the present invention, a method for fabricating a flip-chip LED includes:

[0052] S1: Provide a substrate 10; in this embodiment, the substrate 10 is a 650μm sapphire substrate 10.

[0053] S2: An epitaxial layer 11 is deposited on the substrate 10. The epitaxial layer 11 includes an N-type GaN layer 111, a quantum well light-emitting layer 112, and a P-type GaN layer 113 from bottom to top. In this embodiment, the thickness of the N-type GaN layer 111 is 5 μm, the thickness of the quantum well light-emitting layer 112 is 40 nm, and the thickness of the P-type GaN layer 113 is 300 nm.

[0054] S3: Etch the epitaxial layer 11 to expose the N-type GaN layer 111 and form an N-type conductive step.

[0055] S4: Deposit a current blocking layer 12 on the P-type GaN layer 113;

[0056] Furthermore, the current blocking layer 12 has a thickness between The SiO2 layer; the current blocking layer 12 enables a more uniform current density distribution in the chip, increases current spreading performance, and reduces current accumulation; in this embodiment, the thickness of the current blocking layer 12 is... In practical implementation, its thickness can also be Not limited to this.

[0057] S5: Deposit a current spreading layer 13 on the current blocking layer 12 to form an initial chip;

[0058] Furthermore, the current spreading layer 13 has a thickness between The ITO thin film; in this embodiment, the thickness of the current spreading layer 13 is... In practical implementation, its thickness can also be Not limited to this.

[0059] S6: A first mixed paste is printed on the initial chip using a screen printing process to form a first electrode layer 14; wherein the first mixed paste contains Ni, Au, Ag, Al, Pd and Pt;

[0060] Furthermore, the weight fractions of Ni, Au, Ag, Al, Pd, and Pt in the first mixed slurry range from 5wt%-15wt%, 10wt%-25wt%, 10wt%-25wt%, 10wt%-40wt%, 10wt%-20wt%, and 10wt%-20wt%, respectively. In this embodiment, the weight fractions of Ni, Au, Ag, Al, Pd, and Pt in the first mixed slurry are 10wt%, 20wt%, 20wt%, 20wt%, 15wt%, and 15wt%, respectively, in order to better achieve ohmic contact. The work functions of the metals Ni, Au, Pt, and Pd are 5.15 eV, 5... The work functions of metals such as 0.1eV, 5.65eV, and 5.12eV are relatively close to those of gallium nitride (GaN) (7.5eV), enabling good ohmic contact. Pd has a work function of 5.12eV, which aligns well with the work functions of ITO (5.0eV) and n-GaN (4.5eV). Furthermore, Pt's work function of 5.65eV is relatively close to that of p-GaN (7.5eV). Combining these elements results in high reflectivity, good ohmic contact, and enhanced conductivity. Ag and Al have work functions of 4.26eV and 4.28eV, respectively. While their work functions are slightly lower, they significantly improve reflectivity. Additionally, Pd can suppress the electromigration of silver.

[0061] Furthermore, the step of printing a first mixed paste on the initial chip using a screen printing process to form the first electrode layer 14 includes:

[0062] Photoresist is coated on the N-type conductive step and the current spreading layer 13. The photoresist on the current spreading layer 13 is exposed to the first P-type using the first P-type exposure plate 17, and the photoresist on the N-type conductive step is exposed to the first N-type using the first N-type exposure plate 18. Then, development is performed to generate the first P-type electrode hole 143 and the first N-type electrode hole 144.

[0063] The initial chip is placed on a screen printing machine. A first screen printing screen adapted to the first P-type electrode hole 143 and the first N-type electrode hole 144 is used. The first mixed paste is assembled on the first screen printing screen. The screen printing machine is turned on to perform the screen printing process to form the first electrode layer 14.

[0064] The first electrode layer 14 includes a first P-type electrode layer 141 corresponding to the first P-type electrode hole 143 and a first N-type electrode layer 142 corresponding to the first N-type electrode hole 144.

[0065] Furthermore, the energy of the first P-type exposure was 250 kJ / cm². 2 -350kJ / cm 2 The energy of the first N-type exposure was 450 kJ / cm. 2 -550kJ / cm 2 The thickness of the first P-type electrode layer 141 is 3.5μm-4.5μm, and the thickness of the first N-type electrode layer 142 is 5μm-6μm.

[0066] By adjusting the energy of the first P-type exposure and the energy of the first N-type exposure, and then controlling the depth of the first P-type electrode hole 143 and the first N-type electrode hole 144, the thicknesses of the first P-type electrode layer 141 and the first N-type electrode layer 142 are made inconsistent. In this embodiment, the energy of the first P-type exposure is 300 kJ / cm². 2 The energy of the first N-type exposure was 500 kJ / cm². 2 The thickness of the first P-type electrode layer 141 is 4 μm, and the thickness of the first N-type electrode layer 142 is 5.5 μm. In specific implementation, the energy of the first P-type exposure can be 250 kJ / cm². 2 270kJ / cm 2 330kJ / cm 2 350kJ / cm 2 The energy of the first N-type exposure can be 450 kJ / cm. 2 480kJ / cm 2 510kJ / cm 2 550kJ / cm 2 The thickness of the first P-type electrode layer 141 can be 3.5μm, 3.6μm, 3.9μm, 4.4μm, or 4.5μm, and the thickness of the first N-type electrode layer 142 can be 5μm, 5.2μm, 5.6μm, 5.8μm, or 6μm; it is not limited to these.

[0067] S7: Deposit a reflective layer 15 on the first electrode layer 14 to form an intermediate chip;

[0068] Furthermore, the reflective layer 15 is composed of periodically alternating SiO2 layers and Ti3O5 layers, with 10-20 alternating stacking cycles. The thickness of the SiO2 layer in each alternating stacking cycle is greater than the thickness of the Ti3O5 layer. In this embodiment, the reflective layer 15 has 17 alternating stacking cycles, and the periodic film thicknesses of the SiO2 and Ti3O5 layers are as follows:

[0069]

[0070]

[0071] S8: A second mixed paste is printed on the intermediate chip using a screen printing process to form a second electrode layer 16. The second electrode layer 16 corresponds to and is connected to the first electrode layer 14, thereby obtaining a flip-chip LED chip. The second mixed paste contains Au, Al, Pt and Sn.

[0072] Furthermore, the weight fractions of Au, Al, Pt, and Sn in the second mixed slurry range from 20wt%-35wt%, 15wt%-25wt%, 10wt%-25wt%, and 20wt%-40wt%, respectively. In this embodiment, the weight fractions of Au, Al, Pt, and Sn in the second mixed slurry are 30wt%, 20wt%, 20wt%, and 30wt%, respectively, which have good conductivity, high reflectivity, strong thermal conductivity, and can better perform crystal bonding. Using screen printing technology, the conductive slurry containing metal is imprinted through the screen mesh to form an electrode layer, thereby forming a good ohmic contact with the chip and reducing losses in the current collection and extraction process.

[0073] Furthermore, the step of printing a second mixed paste on the intermediate chip using a screen printing process to form the second electrode layer 16 includes:

[0074] Photoresist is coated on the reflective layer 15, and the photoresist on the reflective layer 15 is exposed a second time using the second exposure plate 19; and development is performed to generate the second P-type electrode hole 163 and the second N-type electrode hole 164.

[0075] The intermediate chip is placed on the screen printing machine. A second screen printing screen adapted to the second P-type electrode hole 163 and the second N-type electrode hole 164 is used. The second mixed paste is assembled on the second screen printing screen. The screen printing machine is turned on to perform the screen printing process to form the second electrode layer 16.

[0076] The second electrode layer 16 includes a second P-type electrode layer 161 corresponding to the second P-type electrode hole 163 and a second N-type electrode layer 162 corresponding to the second N-type electrode hole 164.

[0077] Furthermore, the energy of the second exposure is 250 kJ / cm². 2 -350kJ / cm 2 The thicknesses of the second P-type electrode layer 161 and the second N-type electrode layer 162 are both 3.6 μm to 4.2 μm; in this embodiment, the energy of the second exposure is 300 kJ / cm². 2 The thickness of both the second P-type electrode layer 161 and the second N-type electrode layer 162 is 3.8 μm; in specific implementations, the energy of the second exposure can be 250 kJ / cm². 2 280kJ / cm 2 320kJ / cm 2 350kJ / cm 2 The thickness of the second P-type electrode layer 161 and the second N-type electrode layer 162 can be 3.6μm, 3.7μm, 3.9μm, or 4μm, and is not limited thereto.

[0078] The method for fabricating a flip-chip LED according to an embodiment of the present invention, by using screen printing to prepare the first electrode layer 14 and the second electrode layer 16, can effectively reduce the waste of raw materials generated during the metal evaporation process and save costs. Moreover, the work functions of Ni, Au, Pd and Pt in the first mixed paste are relatively close to those of gallium nitride, which can achieve good ohmic contact. Specifically, the work function of Pd is well connected with the work function of the current spreading layer 13 and the work function of the N-type GaN layer 111, while the work function of Pt is relatively close to that of the P-type GaN layer 113. The combination of these factors can achieve high reflectivity and good ohmic contact, and better increase conductivity. The work functions of Ag and Al are slightly lower, but they have a better effect on improving reflectivity, while Pd can suppress the electromigration of Ag. In addition, the second mixed paste has good conductivity, high reflectivity, strong thermal conductivity, and can better perform die bonding, thereby effectively improving the electrode structure of the flip-chip LED and optimizing the matching of work functions, reducing the power consumption of the flip-chip LED and improving the brightness of the flip-chip LED.

[0079] The chip prepared using the flip-chip LED preparation method of this embodiment has a brightness of 223mW as measured by a testing instrument.

[0080] Example 2

[0081] It is worth noting that, in this embodiment, a method for fabricating a flip-chip LED can also be summarized as follows: In the epitaxial workshop, metal-organic chemical vapor deposition (MOCVD) technology is used. Different raw materials are carried to the reaction chamber by hydrogen and chemically reacted at high temperature. A 5μm thick N-type GaN layer 111, a 40nm thick quantum well light-emitting layer 112 (MQW), and a 300nm thick P-type GaN layer 113 are deposited on a 650μm thick sapphire substrate 10. After that, the wafer is sent to the chip manufacturing workshop, where the wafer undergoes CBL process A, MSA and TCL combined process B, and ISO process C. The three processes include three yellow light operations (i.e., homogenization, exposure, and development under yellow light conditions to prevent the influence of ultraviolet light on the photoresist). Then, PD1 electrode printing (printing of the first electrode layer 14), DBR-35L deposition, and PD2 electrode printing (printing of the second electrode layer 16) processes are performed.

[0082] The CBL process A specifically includes the following steps: first, organic cleaning of the epitaxially prepared wafer to remove impurities and oil, etc., followed by deposition of a thickness of [thickness value missing] using plasma chemical vapor deposition. Silicon dioxide is used as a current blocking layer 12. With the current blocking layer 12, the current density distribution is more uniform, which can increase current spreading performance and reduce current accumulation. Then, a layer of HMDS tackifier is coated at a temperature of 80℃-100℃ to increase the adhesion between the silicon dioxide and the photoresist. At a temperature of 100℃-110℃ and a rotation speed of 3800r / s-4000r / s, a uniform layer of photoresist with a thickness of 2.2μm-2.8μm is spin-coated onto the wafer. The photoresist is then exposed using an exposure machine manufactured by Shanghai Microelectronics at 220kJ / cm². 2 -280kJ / cm 2 Exposure is performed under the specified exposure dose conditions. This exposure range allows for better selection of the photoresist on the mask. Then, the exposed photoresist area is dissolved with a chemical developer. The wafer is developed at a temperature of 120℃-140℃ for about 42 seconds. Finally, it is sent to the wet process workshop, where silicon dioxide is etched at room temperature using BOE solution and then immersed in a photoresist remover at a temperature of 80℃-90℃ for 1200 seconds. After removing the photoresist, the required semi-finished chip I is obtained.

[0083] The combined MSA and TCL process B specifically includes: firstly, cleaning the semi-finished chip I with hydrochloric acid solution, and then depositing a layer of thickness [missing information] on the cleaned wafer using a magnetron sputtering machine. The ITO thin film is used to improve current spreading performance, and then it is annealed for 9 minutes in a nitrogen atmosphere at a temperature of 500℃-600℃. The purpose of annealing is to alloy the wafer, improve the ohmic contact with p-GaN, and subsequently the ohmic contact with the first electrode layer 14. Next, the wafer is coated with photoresist with a thickness of 2.8μm-3.2μm under yellow light conditions, with a temperature range of 80℃-110℃ and a rotation speed of 2650r / s-2800r / s. The photoresist is heated to 180kJ / cm². 2 -220kJ / cm 2 The wafer is exposed under the specified exposure conditions, then developed at 110℃-130℃ for 32 seconds, and sent to the wet processing room for etching of the ITO film at 35℃-50℃ for 480 seconds. The ITO transparent conductive film is patterned using an ITO etching solution to form periodically distributed circular and hexagonal patterns. The wafer is then baked in an oven at 65℃-80℃ for 40 minutes, and finally subjected to ICP etching for 450 seconds. ICP etching is used to expose N-GaN for forming N-type ohmic contact electrodes. Finally, the photoresist is removed using a photoresist remover at 80℃-90℃ for 1300 seconds, yielding the desired semi-finished chip II.

[0084] The steps of ISO process C include: cleaning the obtained semi-finished chip II with an organic cleaning solvent, coating a layer of photoresist with a thickness of 11μm-12μm at a temperature of 110℃-130℃ and a rotation speed of 1250r / s-1350r / s, and applying 1350kJ / cm² to the photoresist-coated wafer. 2 -1450kJ / cm 2 The chip is exposed to a certain exposure dose and developed at a temperature of 100℃-120℃ for 115 seconds. It is then sent to an ICP etching machine for etching for 1165 seconds. The purpose of this ICP etching technology is to form channels for chip isolation, which facilitates subsequent dicing into complete small chips. The chip is then immersed in a resist remover solution at a temperature of 80℃-90℃ for about 2400 seconds to obtain the required semi-finished chip III.

[0085] Before printing the PD1 electrode on the semi-finished chip III, the photoresist thickness for PD1 electrode printing is set to 4μm using a spin coater. PD1 electrode exposure plate 1 (first P-type exposure plate 17) is used to expose the photoresist at the P-type electrode location, with an exposure energy of 300kJ / cm². 2 Exposure is performed, followed by exposure using PD1 electrode exposure board 2 (first N-type exposure board 18), which exposes the photoresist at the N-type electrode location. The secondary exposure energy is 500 kJ / cm². 2After exposure, the photoresist on the wafer is developed at 113°C for 80 seconds to obtain the first P-type electrode hole 143 and the first N-type electrode hole 144 to be printed in the first electrode layer 14. Using screen printing technology, the wafer after exposure is placed on the screen printing machine. The PD1 screen printing screen 1 (first screen printing screen) is used. A mixed paste of PD1 metals Ni, Au, Ag, Al, Pd and Pt is loaded on the PD1 screen printing screen 1. The screen printing machine is turned on to perform the printing process of PD1 electrode (first electrode layer 14). Since the depth of the first P-type electrode hole 143 and the depth of the first N-type electrode hole 144 are different, the thickness of the first P-type electrode layer 141 in the PD1 electrode (first electrode layer 14) is 4μm and the thickness of the first N-type electrode layer 142 is 5.5μm, thus obtaining the required semi-finished chip IV.

[0086] When printing the PD1 electrode using a screen printing machine, the metal paste can be high work function metals such as Ni, Au, Pt, and Pd. The work functions of Ni, Au, Pt, and Pd are 5.15 eV, 5.1 eV, 5.65 eV, and 5.12 eV, respectively. The work functions of these metals are not much different from the work function of gallium nitride (GaN) (7.5 eV), which can achieve good ohmic contact. Among them, Pd has an work function of 5.12 eV, which connects well with the work function of ITO (5.0 eV) and n-GaN (4.5 eV). At the same time, the work function of Pt (5.65 eV) is not much different from the work function of p-GaN (7.5 eV). The combination of these can achieve high reflectivity and good ohmic contact, and better increase conductivity. Ag and Al have work functions of 4.26 eV and 4.28 eV, respectively. Although their work functions are slightly lower, they have a better effect on improving reflectivity. At the same time, Pd can suppress the electromigration of silver.

[0087] The DBR process steps for photocontrolled evaporation of 35L include: depositing a layer on the semi-finished chip IV using a PECVD machine. The silicon dioxide is deposited using the DBR-35L deposition process to form a Bragg reflector. The reflective layer 15 in this invention is composed of alternating SiO2 and Ti3O5 layers, with 17 alternating stacking periods. This forms a highly reflective mirror surface on one side of the LED flip chip, while also providing moisture isolation. In the reflective layer 15 prepared by the 35L photocontrol method in this invention, the first layer is silicon dioxide, and the periodic film thicknesses of the SiO2 and Ti3O5 layers are as follows:

[0088]

[0089] Then, a layer of tackifier HMDS is applied at 100℃, followed by a 10μm thick layer of positive adhesive at 110℃ and a rotation speed of 1750r / s-1850r / s. This adhesive is then subjected to a process involving 800kJ / cm². 2 After exposure at the specified exposure dose, the chip is developed at 120°C for 95 seconds, then baked in an oven at 140°C for 40 minutes, followed by ICP etching for 1540 seconds and resist removal at 85°C for 1200 seconds to obtain the semi-finished chip V prepared by the fifth photolithography.

[0090] On the semi-finished chip V, a 3.8 μm thick layer of PD2 photoresist is coated onto the wafer using a spin coater. The photoresist on the wafer is then exposed using PD2 electrode exposure plate 2 (second exposure plate 19) at an energy of 300 kJ / cm². 2 Expose and develop at 113℃ for 45s to obtain the second P-type electrode hole 163 and the second N-type electrode hole 164 to be printed on the PD2 electrode (second electrode layer 16); replace the screen printing screen of the screen printing machine with the PD2 electrode screen printing screen 2 (second screen printing screen), place the mixed metal paste of Au, Al, Pt and Sn corresponding to the PD2 electrode (second electrode layer 16) on the screen printing screen 2, and use screen printing technology to prepare the PD2 electrode (second electrode layer 16) with a printing thickness of 3.8μm to obtain the desired finished chip;

[0091] The PD2 electrode (second electrode layer 16) is a mixed metal paste of Au, Al, Pt and Sn, with proportions of 30wt%, 20wt%, 20wt%, and 30wt%, respectively. It has good conductivity, high reflectivity, strong thermal conductivity, and can better perform die bonding. Using screen printing technology, the conductive paste containing metals is imprinted through the mesh of the screen to form the electrode layer, thereby forming a good ohmic contact with the chip and reducing losses in the current collection and extraction process. The purpose of setting six metal pastes in the PD1 electrode is to match the work function and improve the current conduction capability, while the purpose of setting four pastes in the PD2 electrode is to save costs. The different metal settings make it more conductive in the packaging process.

[0092] Example 3

[0093] The difference between this embodiment and Embodiment 1 is that in this embodiment, the weight fractions of Ni, Au, Ag, Al, Pd, and Pt in the first mixed slurry are 5wt%, 25wt%, 10wt%, 40wt%, 10wt%, and 10wt%, respectively, and the weight fractions of Au, Al, Pt, and Sn in the second mixed slurry are 20wt%, 25wt%, 25wt%, and 30wt%, respectively. The chip brightness was tested to be 217mW, and other electrical properties were good. The specific results are shown in Table 1.

[0094] Example 4

[0095] The difference between this embodiment and Embodiment 1 is that in this embodiment, the weight fractions of Ni, Au, Ag, Al, Pd, and Pt in the first mixed slurry are 15wt%, 10wt%, 25wt%, 10wt%, 20wt%, and 20wt%, respectively, and the weight fractions of Au, Al, Pt, and Sn in the second mixed slurry are 35wt%, 15wt%, 10wt%, and 40wt%, respectively. The chip brightness was tested to be 219mW, and other electrical properties were good. The specific results are shown in Table 1.

[0096] Example 5

[0097] The difference between this embodiment and Embodiment 1 is that in this embodiment, the weight fractions of Ni, Au, Ag, Al, Pd, and Pt in the first mixed slurry are 10wt%, 15wt%, 15wt%, 30wt%, 15wt%, and 15wt%, respectively, and the weight fractions of Au, Al, Pt, and Sn in the second mixed slurry are 30wt%, 25wt%, 25wt%, and 20wt%, respectively. The chip brightness was tested to be 220mW, and other electrical properties were good. The specific results are shown in Table 1.

[0098] Comparison Example

[0099] The flip-chip LED in this comparative example uses conventional methods to deposit metal electrodes layer by layer, and the chip brightness is measured to be 215mW by testing instruments.

[0100] Table 1: Comparison of some parameters and brightness of various embodiments and control examples

[0101]

[0102] As shown in Table 1, the present invention, by employing screen printing to prepare the first electrode layer 14 and the second electrode layer 16, can effectively reduce the waste of raw materials generated during the metal evaporation process and save costs. Furthermore, the work functions of Ni, Au, Pd, and Pt in the first mixed slurry are relatively close to those of gallium nitride, enabling good ohmic contact. Specifically, the work function of Pd is well-connected with the work functions of the current spreading layer 13 and the N-type GaN layer 111, while the work function of Pt is relatively close to that of the P-type GaN layer 113. The combination of these factors achieves a high reflectivity. The better ohmic contact enhances conductivity; while Ag and Al have slightly lower work functions, they have a better effect on improving reflectivity, and Pd can suppress the electromigration of Ag; in addition, the second mixed slurry has good conductivity and high reflectivity, strong thermal conductivity, and can better perform die bonding, thereby effectively improving the electrode structure of the flip LED chip and optimizing the work function matching, reducing the power consumption of the flip LED chip, and improving the brightness of the flip LED chip; the brightness of the flip LED chip obtained by the conventional method of layer-by-layer deposition of metal to form electrodes is significantly improved compared to the control example.

[0103] Example 6

[0104] This embodiment also proposes a flip-chip LED, which is prepared by any one of the flip-chip LED preparation methods of Embodiments 1 to 5.

[0105] In the description of this specification, references to terms such as "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.

[0106] Without causing conflict, those skilled in the art can freely combine and use the above-mentioned additional technical features.

[0107] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A method for fabricating a flip-chip LED, characterized in that, The method for preparing the flip-chip LED includes: Provide a substrate; An epitaxial layer is deposited on the substrate, the epitaxial layer comprising, from bottom to top, an N-type GaN layer, a quantum well light-emitting layer, and a P-type GaN layer; The epitaxial layer is etched to expose the N-type GaN layer and form an N-type conductive step; A current blocking layer is deposited on the P-type GaN layer; A current spreading layer is deposited on the current blocking layer to form an initial chip; A first mixed paste is printed on the initial chip using a screen printing process to form a first electrode layer; wherein the first mixed paste contains Ni, Au, Ag, Al, Pd and Pt; A reflective layer is deposited on the first electrode layer to form an intermediate chip; A second mixed paste is printed on the intermediate chip using a screen printing process to form a second electrode layer. The second electrode layer corresponds vertically to and is interconnected with the first electrode layer, thereby obtaining a flip-chip LED. The second mixed paste contains Au, Al, Pt, and Sn. The weight fractions of Ni, Au, Ag, Al, Pd, and Pt in the first mixed slurry range from 5wt% to 15wt%, 10wt% to 25wt%, 10wt% to 25wt%, 10wt% to 40wt%, 10wt% to 20wt%, and 10wt% to 20wt%, respectively. The weight percentages of Au, Al, Pt, and Sn in the second mixed slurry range from 20wt% to 35wt%, 15wt% to 25wt%, 10wt% to 25wt%, and 20wt% to 40wt%, respectively.

2. The method for fabricating a flip-chip LED according to claim 1, characterized in that, The step of printing a first mixed paste onto the initial chip using a screen printing process to form a first electrode layer includes: Photoresist is coated on the N-type conductive step and the current spreading layer. A first P-type exposure plate is used to expose the photoresist on the current spreading layer in a first P-type manner, and a first N-type exposure plate is used to expose the photoresist on the N-type conductive step in a first N-type manner. The photoresist is then developed to generate a first P-type electrode hole and a first N-type electrode hole. The initial chip is placed on a screen printing machine. A first screen printing screen adapted to the first P-type electrode hole and the first N-type electrode hole is used to assemble the first mixed paste on the first screen printing screen. The screen printing machine is then turned on to perform the screen printing process to form the first electrode layer. The first electrode layer includes a first P-type electrode layer corresponding to the first P-type electrode hole and a first N-type electrode layer corresponding to the first N-type electrode hole.

3. The method for fabricating a flip-chip LED according to claim 2, characterized in that, The energy of the first P-type exposure is 250 kJ / cm. 2 -350kJ / cm 2 The energy of the first N-type exposure is 450 kJ / cm. 2 -550kJ / cm 2 The thickness of the first P-type electrode layer is 3.5μm-4.5μm, and the thickness of the first N-type electrode layer is 5μm-6μm.

4. The method for fabricating a flip-chip LED according to claim 1, characterized in that, The reflective layer is composed of alternating SiO2 and Ti3O5 layers, with 10-20 alternating stacking cycles, and the thickness of the SiO2 layer in each alternating stacking cycle is greater than the thickness of the Ti3O5 layer.

5. The method for fabricating a flip-chip LED according to claim 1, characterized in that, The step of printing a second mixed paste onto the intermediate chip using a screen printing process to form a second electrode layer includes: Photoresist is coated on the reflective layer, and the photoresist on the reflective layer is exposed a second time using a second exposure plate and then developed to generate a second P-type electrode hole and a second N-type electrode hole. The intermediate chip is placed on a screen printing machine. A second screen printing screen adapted to the second P-type electrode hole and the second N-type electrode hole is used to assemble the second mixed paste on the second screen printing screen. The screen printing machine is then turned on to perform the screen printing process to form the second electrode layer. The second electrode layer includes a second P-type electrode layer corresponding to the second P-type electrode hole and a second N-type electrode layer corresponding to the second N-type electrode hole.

6. The method for fabricating a flip-chip LED according to claim 5, characterized in that, The energy of the second exposure is 250 kJ / cm. 2 -350kJ / cm 2 The thickness of both the second P-type electrode layer and the second N-type electrode layer is 3.6μm-4μm.

7. The method for fabricating a flip-chip LED according to claim 1, characterized in that, The current blocking layer is a SiO2 layer with a thickness between 1800 Å and 2200 Å.

8. A flip-chip LED, characterized in that, The flip-chip LED is prepared according to any one of claims 1-7.

Citation Information

Patent Citations

  • III-group nitride semiconductor light-emitting device adopting nanoimprint technology

    CN102005514A

  • Iii nitride-based compound semiconductor light-emitting element

    JP2001313420A