Wear-resistant heat-insulating gloves and preparation method thereof
By combining modified silica aerogel and sepiolite aerogel and combining water-based polyurethane, hollow microbeads, aramid fiber and other materials, wear-resistant heat-insulating gloves are prepared, which solves the problem of wear resistance and insulation of traditional gloves. The problem of insufficient thermal performance is achieved, and good insulation and durability in high temperature environments are achieved.
Patent Information
- Application Number
- CN202311677749.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-08
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-12-08
AI Technical Summary
Traditional heat-insulating gloves have insufficient wear resistance and poor heat-insulating properties during use, and cannot meet the needs of the actual working environment.
Wear-resistant heat-insulating gloves are prepared by combining modified silica aerogel and sepiolite aerogel, combining water-based polyurethane, hollow microspheres and aramid fibers, and using modified surfactants and defoaming agents. Enhance its thermal insulation properties and wear resistance.
The insulation performance and wear resistance of the gloves are improved, making them more durable in high-strength and high-friction environments, making them suitable for industrial production and high-temperature operations.
Smart Images

Figure BDA0004595133450000091
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of labor protection gloves, in particular to a wear-resistant heat-insulating glove and a preparation method thereof. Background Art
[0002] With the increase of industrial production and high-temperature operation, the demand for heat-insulating gloves is also increasing. However, traditional heat-insulating gloves often have problems such as insufficient wear resistance and poor heat insulation performance during use, which cannot meet the needs of actual working environments.
[0003] In recent years, nano aerogel has attracted much attention as a new type of solid thermal insulation material. This material has low thermal conductivity and is a thermal insulation material with excellent performance. In the research of aerogel, silica aerogel has always been one of the mainstream directions. Due to its excellent thermal insulation performance and lightweight characteristics, it has been widely used in the field of thermal insulation materials. However, during the production process, silica aerogel itself has no bonding strength with the fabric, and has disadvantages such as low strength and high brittleness.
[0004] Therefore, we propose a wear-resistant heat-insulating glove and a preparation method thereof. Summary of the invention
[0005] The object of the present invention is to provide a wear-resistant heat-insulating glove and a preparation method thereof to solve the problems raised in the above background technology.
[0006] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0007] A method for preparing wear-resistant heat-insulating gloves comprises the following steps:
[0008] Step S1: mixing hydrophobic silica aerogel, surfactant and deionized water uniformly to obtain modified silica aerogel slurry; then adding sepiolite aerogel and mixing uniformly to obtain composite aerogel material;
[0009] Step S2: mixing waterborne polyurethane and deionized water evenly, adding composite aerogel slurry, hollow microspheres and aramid fibers to mix, ultrasonically dispersing for 30-50 minutes, adding surfactant, defoamer and thickener to mix evenly to obtain a rubber material;
[0010] Step S3: Put the glove blank on the hand mold, preheat at 40-50°C for 30-50min, dip into the coagulant, take out and air-dry for 30-50s, dip into the rubber obtained in step S2 1-2 times, take out; dip into the coagulant for the second time, take out and air-dry for 30-60min, dry and demould, and obtain the wear-resistant heat-insulating gloves.
[0011] In the above technical scheme, the hydrophobic silica aerogel is modified by coating the surface of the hydrophobic silica aerogel with a surfactant, the surfactant is composed of a hydrophilic group and a lipophilic group, the lipophilic group is adsorbed on the hydrophobic group on the surface of the hydrophobic silica aerogel, and the hydrophilic group extends to the aqueous solution to make its surface hydrophilic. The modified silica aerogel is compounded with sepiolite aerogel in the form of a slurry, thereby improving the compatibility of the silica aerogel and the inorganic gelling material, and enhancing the thermal insulation performance and strength of the composite material; using water-based polyurethane as a film-forming substance, and combining the composite aerogel material, hollow microspheres, aramid fibers and surfactants, defoamers, and thickeners to produce a rubber material with excellent wear resistance and thermal insulation performance.
[0012] Furthermore, in step S1, the mass ratio of the hydrophobic silica aerogel, the surfactant, and the deionized water is 1:(0.01-0.03):(8-10).
[0013] Furthermore, the preparation method of the surfactant is as follows:
[0014] Step (1): 14-bromo-1-tetradecanol and anhydrous ethanol are mixed evenly, an aqueous solution of tert-butyldimethylamine is added, the temperature is raised to 70-80° C., refluxed for 22-24 hours, and a tertiary amine compound is obtained by extraction, drying and concentration;
[0015] Step (2): uniformly mix the tertiary amine compound, triethylamine and anhydrous acetonitrile, add 2-methyl-3-phenyl-2-acryloyl chloride in an ice bath, raise the temperature to 30-40° C., react for 10-12 hours, extract, dry and concentrate to obtain an intermediate;
[0016] Step (3): the intermediate, 1,3-propane sultone and anhydrous acetonitrile are uniformly mixed, 4-methoxyphenol is added, and the mixture is refluxed at 30-40° C. for 22-24 hours under an argon atmosphere. After filtering, washing and drying, a surfactant is obtained.
[0017] In the above technical scheme, 14-bromo-1-tetradecanol reacts with tert-butyldimethylamine to generate a tertiary amine compound, the hydroxyl group in the tertiary amine compound reacts with 2-methyl-3-phenyl-2-acryloyl chloride to generate an intermediate containing a double bond, and finally reacts with 1,3-propane sultone to introduce a carbon-carbon double bond, thereby generating a surfactant having a hydrophilic group and a lipophilic group.
[0018] Furthermore, in the step (1), the mass ratio of 14-bromo-1-tetradecanol to anhydrous ethanol is 1:(20-25).
[0019] Furthermore, in the step (1), the mass of the aqueous solution of tert-butyldimethylamine is 3-4 times the mass of 14-bromo-1-tetradecanol, and its concentration is 40-50 wt%.
[0020] Furthermore, in the step (2), the mass ratio of the tertiary amine compound to triethylamine and anhydrous acetonitrile is 1:(0.4-0.6):(30-40).
[0021] Furthermore, in step (2), the mass of 2-methyl-3-phenyl-2-acryloyl chloride is 0.6-0.8 times the mass of the tertiary amine compound.
[0022] Furthermore, in the step (3), the mass ratio of the intermediate to 1,3-propane sultone and anhydrous acetonitrile is 1:(0.8-1.0):(30-40).
[0023] Furthermore, in step (3), the mass of 4-methoxyphenol is 5-7% of the mass of the intermediate.
[0024] Furthermore, in step S1, the mass of the sepiolite aerogel is 2-3 times the mass of the modified silica aerogel.
[0025] Furthermore, the preparation method of the sepiolite aerogel in step S1 is as follows:
[0026] The sepiolite is dispersed in deionized water, subjected to ultrasonic treatment for 30-50 minutes, polyvinyl alcohol solution, γ-(2,3-epoxypropoxy)propyltrimethoxysilane and polyethyleneimine are added and mixed, the mixture is heated to 70-80°C, stirred for 3-4 hours, freeze-dried, and reacted at 110-120°C for 30-50 minutes to obtain the sepiolite aerogel.
[0027] Furthermore, the mass ratio of the sepiolite to deionized water is 1:(25-30).
[0028] Furthermore, the mass of the polyvinyl alcohol is 0.5-0.7 times the mass of the sepiolite, and the concentration of the polyvinyl alcohol solution is 3-5wt%.
[0029] Furthermore, the mass of the γ-(2,3-epoxypropoxy)propyltrimethoxysilane is 0.1-0.3 times the mass of sepiolite.
[0030] Furthermore, the mass ratio of the γ-(2,3-epoxypropoxy)propyltrimethoxysilane to polyethyleneimine is 1:(1-2).
[0031] Furthermore, the rubber material in step S2 includes the following components by weight: 40-50 parts of waterborne polyurethane, 10-15 parts of deionized water, 5-15 parts of composite aerogel slurry, 5-10 parts of hollow microspheres, 10-15 parts of aramid fibers, 0.1-0.5 parts of surfactants, 0.2-0.3 parts of defoaming agents, and 0.1-0.3 parts of thickeners.
[0032] Furthermore, the model of the defoaming agent is BYK-028.
[0033] Furthermore, the thickener is a water-based acrylic thickener: model NY-935, solid content 30%, sourced from Guangdong Nuoyi Chemical Co., Ltd.
[0034] Furthermore, the viscosity of the rubber in step S2 is 1800-3000 mPa·S.
[0035] Furthermore, the coagulant in step S3 is a methanol solution of calcium chloride, and the mass fraction of calcium chloride is 2-8%.
[0036] Furthermore, the process conditions for drying in step S3 are: drying temperature 100-150° C., and drying time 5-10 min.
[0037] Compared with the prior art, the present invention has the following beneficial effects:
[0038] 1. A wear-resistant heat-insulating glove and a preparation method thereof of the present invention is to modify the hydrophobic silica aerogel by coating the surface of the hydrophobic silica aerogel with a surfactant, wherein the surfactant is composed of a hydrophilic group and a lipophilic group, the lipophilic group is adsorbed on the hydrophobic group on the surface of the hydrophobic silica aerogel, and the hydrophilic group extends toward the aqueous solution to make the surface hydrophilic, and the modified silica aerogel is composited with sepiolite aerogel in the form of slurry, thereby improving the compatibility of the silica aerogel with the inorganic gelling material and enhancing the heat-insulating performance and strength of the composite hydrogel material.
[0039] 2. A wear-resistant heat-insulating glove and a preparation method thereof of the present invention, using water-based polyurethane as a film-forming material, and combining composite aerogel materials, hollow microspheres, aramid fibers, surfactants, defoamers, and thickeners to work together to prepare a rubber compound with excellent wear resistance and heat insulation performance. Among them, water-based polyurethane is a polymer with good elasticity and wear resistance, which can increase the wear resistance of the rubber compound and make it more durable; hollow microspheres can reduce the density of the rubber compound and improve its heat insulation performance, making it excellent in heat conduction; aramid fibers have good tensile strength and wear resistance, which can increase the strength and wear resistance of the rubber compound, making it more suitable for use in high-strength and high-friction environments; at the same time, the surfactant prepared by the present invention can play a dispersing and wetting role to improve the uniformity and stability of the rubber compound. DETAILED DESCRIPTION
[0040] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0041] In this embodiment, hydrophobic silica aerogel: powder, product number 1407014, pore size 20nm, particle size 2-40μm, sourced from Forsman Technology (Beijing) Co., Ltd.; water-based polyurethane: model 1624, solid content 38%, sourced from Shenzhen Yoshida Chemical Co., Ltd.; hollow microspheres: particle size 325 mesh, sourced from Hebei Yilei Mining Co., Ltd.; aramid fiber: short-cut aramid fiber, average length 3mm, sourced from Dongguan Lanxin New Material Weaving Technology Co., Ltd.; defoamer: model BYK-028, sourced from Dongguan Haoyouduo New Materials Co., Ltd.; thickener: water-based acrylic thickener: model NY-935, solid content 30%, sourced from Guangdong Nuoyi Chemical Co., Ltd.; sepiolite: 400-800 mesh, sourced from Hebei Kexu Building Materials Co., Ltd.; glove blank: 13-gauge white nylon glove core, sourced from Linyi Xinbaidun Labor Protection Products Co., Ltd.
[0042] In the following examples and comparative examples, 1 part is equal to 10 g.
[0043] Embodiment 1: A method for preparing wear-resistant heat-insulating gloves, comprising the following process:
[0044] Step S1: 5 parts of hydrophobic silica aerogel, 0.05 parts of surfactant, and 40 parts of deionized water are mixed evenly to prepare a modified silica aerogel slurry; and 10 parts of sepiolite aerogel are added and mixed evenly to prepare a composite aerogel material;
[0045] Step S2: 40 parts of waterborne polyurethane and 10 parts of deionized water are mixed evenly, 5 parts of composite aerogel slurry, 5 parts of hollow microspheres and 10 parts of aramid fibers are added, and ultrasonic dispersion is performed for 30 minutes, and 0.1 parts of surfactant, 0.2 parts of defoamer and 0.1 parts of thickener are added and mixed evenly to obtain a rubber material;
[0046] Step S3: Put the glove blank on the hand mold, preheat at 40°C for 30 minutes, dip in 2wt% calcium chloride methanol solution, take out and air for 30 seconds, dip in the rubber obtained in step S2 once, take out; dip in 2wt% calcium chloride methanol solution for the second time, take out and air for 30 minutes, dry (drying temperature 100°C, drying time 5 minutes), demould, and obtain wear-resistant heat-insulating gloves;
[0047] The preparation method of the surfactant is as follows:
[0048] Step (1): 0.2 parts of 14-bromo-1-tetradecanol and 4 parts of anhydrous ethanol are mixed evenly, 0.6 parts of tert-butyldimethylamine aqueous solution are added, the temperature is raised to 70° C., refluxed for 22 hours, extracted, dried and concentrated to obtain a tertiary amine compound;
[0049] Step (2): 0.2 parts of a tertiary amine compound, 0.08 parts of triethylamine and 6 parts of anhydrous acetonitrile are mixed uniformly, 0.12 parts of 2-methyl-3-phenyl-2-acryloyl chloride are added under ice bath conditions, the temperature is raised to 30° C., the reaction is carried out for 10 hours, and an intermediate is obtained after extraction, drying and concentration;
[0050] Step (3): 0.2 parts of the intermediate, 0.16 parts of 1,3-propane sultone and 6 parts of anhydrous acetonitrile were mixed evenly, 0.01 parts of 4-methoxyphenol were added, and the mixture was refluxed at 30° C. for 22 hours under an argon atmosphere. After filtering, washing and drying, a surfactant was obtained;
[0051] The preparation method of sepiolite aerogel in step S1 is as follows:
[0052] 10 parts of sepiolite were dispersed in 250 parts of deionized water, and ultrasonically treated for 30 minutes. 5 parts of 3wt% polyvinyl alcohol solution, 1 part of γ-(2,3-epoxypropoxy)propyltrimethoxysilane, and 1 part of polyethyleneimine were added and mixed. The mixture was heated to 70°C and stirred for 3 hours. After freeze-drying, the mixture was reacted at 110°C for 30 minutes to obtain sepiolite aerogel.
[0053] Embodiment 2: A method for preparing wear-resistant heat-insulating gloves, comprising the following process:
[0054] Step S1: 10 parts of hydrophobic silica aerogel, 0.2 parts of surfactant, and 90 parts of deionized water are mixed evenly to prepare a modified silica aerogel slurry; and 25 parts of sepiolite aerogel are added and mixed evenly to prepare a composite aerogel material;
[0055] Step S2: 45 parts of waterborne polyurethane and 12 parts of deionized water are mixed evenly, 10 parts of composite aerogel slurry, 8 parts of hollow microspheres and 12 parts of aramid fibers are added, and ultrasonic dispersion is performed for 40 minutes, and 0.3 parts of surfactant, 0.25 parts of defoamer and 0.2 parts of thickener are added and mixed evenly to obtain a rubber material;
[0056] Step S3: putting the glove blank on the hand mold, preheating at 45° C. for 40 min, dipping in a 6wt% calcium chloride methanol solution, taking out and airing for 40 s, dipping in the rubber obtained in step S2 twice, taking out; dipping in a 6wt% calcium chloride methanol solution for the second time, taking out and airing for 50 min, drying (drying temperature 120° C., drying time 8 min), demoulding, and obtaining a wear-resistant heat-insulating glove;
[0057] The preparation method of the surfactant is as follows:
[0058] Step (1): 0.5 parts of 14-bromo-1-tetradecanol and 11 parts of anhydrous ethanol are mixed evenly, 1.8 parts of a 45 wt% aqueous solution of tert-butyldimethylamine are added, the temperature is raised to 75° C., refluxed for 23 hours, extracted, dried and concentrated to obtain a tertiary amine compound;
[0059] Step (2): 0.5 parts of a tertiary amine compound, 0.25 parts of triethylamine and 18 parts of anhydrous acetonitrile are mixed uniformly, 0.35 parts of 2-methyl-3-phenyl-2-acryloyl chloride are added under ice bath conditions, the temperature is raised to 35° C., the reaction is carried out for 11 hours, and an intermediate is obtained after extraction, drying and concentration;
[0060] Step (3): 0.5 parts of the intermediate, 0.45 parts of 1,3-propane sultone and 18 parts of anhydrous acetonitrile were mixed evenly, 0.03 parts of 4-methoxyphenol were added, and the mixture was refluxed at 35° C. for 23 hours under an argon atmosphere. After filtering, washing and drying, a surfactant was obtained;
[0061] The preparation method of sepiolite aerogel in step S1 is as follows:
[0062] 25 parts of sepiolite were dispersed in 700 parts of deionized water, ultrasonically treated for 40 minutes, 15 parts of 4wt% polyvinyl alcohol solution, 0.5 parts of γ-(2,3-epoxypropoxy)propyltrimethoxysilane, and 0.75 parts of polyethyleneimine were added and mixed, the temperature was raised to 75°C, stirred for 3.5 hours, freeze-dried, and reacted at 115°C for 40 minutes to obtain sepiolite aerogel.
[0063] Embodiment 3: A method for preparing wear-resistant heat-insulating gloves, comprising the following process:
[0064] Step S1: 15 parts of hydrophobic silica aerogel, 0.45 parts of surfactant, and 150 parts of deionized water are mixed evenly to prepare a modified silica aerogel slurry; and 45 parts of sepiolite aerogel are added and mixed evenly to prepare a composite aerogel material;
[0065] Step S2: 50 parts of waterborne polyurethane and 15 parts of deionized water are mixed evenly, 15 parts of composite aerogel slurry, 10 parts of hollow microspheres and 15 parts of aramid fibers are added, ultrasonically dispersed for 50 minutes, 0.5 parts of surfactant, 0.3 parts of defoamer and 0.3 parts of thickener are added and mixed evenly to obtain a rubber material;
[0066] Step S3: putting the glove blank on the hand mold, preheating at 50° C. for 50 min, dipping in 8wt% calcium chloride methanol solution, taking out and airing for 50 s, dipping in the rubber obtained in step S2 twice, taking out; dipping in 8wt% calcium chloride methanol solution for the second time, taking out and airing for 60 min, drying (drying temperature 150° C., drying time 10 min), demoulding, and obtaining wear-resistant heat-insulating gloves;
[0067] The preparation method of the surfactant is as follows:
[0068] Step (1): 1 part of 14-bromo-1-tetradecanol and 25 parts of anhydrous ethanol are mixed evenly, 4 parts of a 50 wt% aqueous solution of tert-butyldimethylamine are added, the temperature is raised to 80° C., refluxed for 24 hours, extracted, dried and concentrated to obtain a tertiary amine compound;
[0069] Step (2): 1 part of a tertiary amine compound, 0.6 parts of triethylamine and 40 parts of anhydrous acetonitrile are mixed evenly, 0.8 parts of 2-methyl-3-phenyl-2-acryloyl chloride are added under ice bath conditions, the temperature is raised to 40° C., the reaction is carried out for 12 hours, and an intermediate is obtained after extraction, drying and concentration;
[0070] Step (3): uniformly mix 1 part of the intermediate, 1 part of 1,3-propane sultone and 40 parts of anhydrous acetonitrile, add 0.07 parts of 4-methoxyphenol, and reflux at 40° C. for 24 hours under an argon atmosphere, filter, wash and dry to obtain a surfactant;
[0071] The preparation method of sepiolite aerogel in step S1 is as follows:
[0072] Sepiolite was dispersed in deionized water, ultrasonically treated for 50 minutes, polyvinyl alcohol solution, γ-(2,3-epoxypropoxy)propyltrimethoxysilane and polyethyleneimine were added and mixed, the mixture was heated to 80°C, stirred for 4 hours, freeze-dried, and reacted at 120°C for 50 minutes to obtain sepiolite aerogel.
[0073] Comparative Example 1: The rubber material includes the following components by weight: 40 parts of aqueous polyurethane, 10 parts of deionized water, 5 parts of composite aerogel slurry, 5 parts of hollow microspheres, 10 parts of aramid fiber, 0.1 parts of surfactant, 0.2 parts of defoaming agent, and 0.1 parts of thickener. No surfactant is added in step S2 of Comparative Example 1; other steps and processes are the same as those in Example 1.
[0074] Comparative Example 2: The rubber material includes the following components by weight: 40 parts of aqueous polyurethane, 10 parts of deionized water, 5 parts of composite aerogel slurry, 5 parts of hollow microspheres, 10 parts of aramid fiber, 0.1 parts of surfactant, 0.2 parts of defoaming agent, and 0.1 parts of thickener. In Comparative Example 2, 1 part of composite aerogel slurry is added; the other steps and processes are the same as those in Example 1.
[0075] Comparative Example 3: A method for preparing wear-resistant heat-insulating gloves, comprising the following processes:
[0076] Step S1: 10 parts of hydrophobic silica aerogel, 0.2 parts of surfactant, and 90 parts of deionized water are mixed uniformly to prepare modified silica aerogel slurry;
[0077] Step S2: 45 parts of waterborne polyurethane and 12 parts of deionized water are mixed evenly, 10 parts of modified silica aerogel slurry, 8 parts of hollow microspheres and 12 parts of aramid fibers are added, and ultrasonic dispersion is performed for 40 minutes, and 0.3 parts of surfactant, 0.25 parts of defoamer and 0.2 parts of thickener are added and mixed evenly to obtain a rubber material;
[0078] Step S3: putting the glove blank on the hand mold, preheating at 45° C. for 40 min, dipping in a 6wt% calcium chloride methanol solution, taking out and airing for 40 s, dipping in the rubber obtained in step S2 twice, taking out; dipping in a 6wt% calcium chloride methanol solution for the second time, taking out and airing for 50 min, drying (drying temperature 120° C., drying time 8 min), demoulding, and obtaining a wear-resistant heat-insulating glove;
[0079] Compared with Example 2, no sepiolite aerogel is added in step S1 of Comparative Example 3; the other steps are the same as those of Example 2.
[0080] Comparative Example 4: A method for preparing wear-resistant heat-insulating gloves, comprising the following processes:
[0081] The preparation method of the surfactant is as follows:
[0082] Step (1): 0.5 parts of 14-bromo-1-tetradecanol and 11 parts of anhydrous ethanol are mixed evenly, 1.8 parts of a 45 wt% aqueous solution of tert-butyldimethylamine are added, the temperature is raised to 75° C., refluxed for 23 hours, extracted, dried and concentrated to obtain a tertiary amine compound;
[0083] Step (2): 0.5 parts of a tertiary amine compound, 0.25 parts of triethylamine and 18 parts of anhydrous acetonitrile are mixed uniformly, 0.35 parts of 2-methyl-3-phenyl-2-acryloyl chloride are added under ice bath conditions, the temperature is raised to 35° C., the reaction is carried out for 11 hours, and an intermediate is obtained after extraction, drying and concentration;
[0084] Step (3): 0.5 parts of the intermediate, 0.25 parts of 1,3-propane sultone and 5 parts of anhydrous acetonitrile were mixed evenly, 0.03 parts of 4-methoxyphenol were added, and the mixture was refluxed at 35° C. for 23 hours under an argon atmosphere. After filtering, washing and drying, a surfactant was obtained;
[0085] Compared with Example 2, the mass ratio of the intermediate to 1,3-propane sultone and anhydrous acetonitrile in step (3) of Comparative Example 4 is 1:0.5:10; the other steps are the same as those in Example 2.
[0086] Experiment: Take the wear-resistant heat-insulating gloves obtained in Examples 1-3 and Comparative Examples 1-4, prepare samples, test their properties respectively and record the test results:
[0087] The wear resistance is measured according to GB 24541-2009 "Hand Protection Gloves against Mechanical Hazards". The experimental steps are as follows: the sample is a circle with a diameter of 38 mm and is tested using a PK-213 Martindale abrasion tester. The total mass of the loading block and the sample fixture assembly should be 600 g. The wear resistance is characterized by the number of cycles, where a cycle is a planar motion whose trajectory forms a perfect figure, including 16 cycles, i.e., the side moving wheel rotates 16 times and the inner moving wheel rotates 15 times, until the sample is worn out, and is graded: Level 3 is between 2000-8000 cycles; Level 4 is 8000 cycles and above.
[0088] The thermal conductivity of the sample was measured using a thermal constant analyzer. The sample size was 90mm×90mm×20mm. The test environment temperature was 20°C and the relative humidity was 65%. The measurement time was 1s and the heating power was 1mW. Each sample was measured 5 times and the average value was taken.
[0089] Test Results
[0090]
[0091] According to the data in the above table, we can clearly draw the following conclusions:
[0092] 1. Compared with Examples 1-3, the wear resistance and thermal insulation properties of the products obtained in Comparative Examples 1 and 2 are reduced. It can be seen that the addition of surfactants to the rubber compound in the present invention can make the filler dispersed evenly to improve the wear resistance and thermal insulation properties of the rubber compound; it shows that the performance of the rubber compound prepared by the present invention is affected by its component ratio, and by selecting the component ratio within the said range, a rubber compound with excellent wear resistance and thermal insulation properties can be prepared.
[0093] 2. Compared with Examples 1-3, the wear resistance and thermal insulation performance of the product obtained in Comparative Example 3 are both reduced, indicating that the addition of sepiolite aerogel and silica aerogel in the present invention play a synergistic role in jointly improving the thermal insulation performance and strength of the material.
[0094] 3. Compared with Examples 1-3, the wear resistance and thermal insulation properties of the product obtained in Comparative Example 4 are reduced. It can be seen that the performance of the surfactant prepared by the present invention is affected by the ratio of each reagent in its preparation process. By selecting a mass ratio within the range, the prepared surfactant has excellent performance.
[0095] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process method article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process method article or device.
[0096] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing wear-resistant heat-insulating gloves, Features: The steps include: Step S1: mixing hydrophobic silica aerogel, surfactant and deionized water uniformly to obtain modified silica aerogel slurry; then adding sepiolite aerogel and mixing uniformly to obtain composite aerogel material; Step S2: mixing waterborne polyurethane and deionized water evenly, adding composite aerogel slurry, hollow microspheres and aramid fibers to mix, ultrasonically dispersing for 30-50 minutes, adding surfactant, defoamer and thickener to mix evenly to obtain a rubber material; Step S3: Put the glove blank on the hand mold, preheat at 40-50°C for 30-50min, dip into the coagulant, take out and air dry for 30-50s, dip into the rubber obtained in step S2 1-2 times, take out; dip into the coagulant for the second time, take out and air dry for 30-60min, dry and demould, and obtain the wear-resistant heat-insulating gloves; The preparation method of the surfactant used in step S1 and step S2 is as follows: Step (1): 14-bromo-1-tetradecanol and anhydrous ethanol are mixed evenly, an aqueous solution of tert-butyldimethylamine is added, the temperature is raised to 70-80° C., refluxed for 22-24 hours, and a tertiary amine compound is obtained by extraction, drying and concentration; Step (2): uniformly mix the tertiary amine compound, triethylamine and anhydrous acetonitrile, add 2-methyl-3-phenyl-2-acryloyl chloride in an ice bath, raise the temperature to 30-40° C., react for 10-12 hours, extract, dry and concentrate to obtain an intermediate; Step (3): uniformly mixing the intermediate, 1,3-propane sultone and anhydrous acetonitrile, adding 4-methoxyphenol, and reacting under argon atmosphere at 30-40° C. for 22-24 hours, filtering, washing and drying to obtain a surfactant; In the step (3), the mass ratio of the intermediate to 1,3-propane sultone and anhydrous acetonitrile is 1:(0.8-1.0):(30-40); The thickener is a water-based acrylic thickener.
2. A method for preparing a wear-resistant heat-insulating glove according to claim 1, Features: The mass ratio of the hydrophobic silica aerogel, the surfactant and the deionized water in step S1 is 1: (0.01-0.03):(8-10)。 3. The method for preparing the wear-resistant heat-insulating gloves according to claim 1, Features: The mass of the sepiolite aerogel in step S1 is 2-3 times the mass of the modified silica aerogel.
4. The method for preparing the wear-resistant heat-insulating gloves according to claim 1, Features: The preparation method of the sepiolite aerogel in step S1 is as follows: The sepiolite is dispersed in deionized water, subjected to ultrasonic treatment for 30-50 minutes, polyvinyl alcohol solution, γ-(2,3-epoxypropoxy)propyltrimethoxysilane and polyethyleneimine are added and mixed, the mixture is heated to 70-80°C, stirred for 3-4 hours, freeze-dried, and reacted at 110-120°C for 30-50 minutes to obtain the sepiolite aerogel.
5. The method for preparing the wear-resistant heat-insulating gloves according to claim 1, Features: The rubber material in step S2 includes the following components by weight: 40-50 parts of waterborne polyurethane, 10-15 parts of deionized water, 5-15 parts of composite aerogel material, 5-10 parts of hollow microspheres, 10-15 parts of aramid fiber, 0.1-0.5 parts of surfactant, 0.2-0.3 parts of defoamer, and 0.1-0.3 parts of thickener.
6. The method for preparing the wear-resistant heat-insulating gloves according to claim 1, It is characterized in that The process conditions for drying in step S3 are: drying temperature 100-150° C., and drying time 5-10 min.
7. A wear-resistant heat-insulating glove made according to the preparation method according to any one of claims 1 to 6.
Citation Information
Patent Citations
Nanometer high temperature resistant thermal insulation and prevention coating
CN104231917A
Energy-saving thermal insulation material and preparation method thereof
CN108793932A