A foam double-sided tape and its preparation process

By treating the surface corona and modifying the foam surface, combined with specific adhesive formulas, the problem of insufficient bonding strength and impact resistance of traditional PU foam tape is solved, and a foam double-sided tape with excellent performance is prepared. It is suitable for use in the in the precision electronics industry.

CN117777875BActive Publication Date: 2024-11-08ENPING TAIBEITE NEW MATERIAL CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202311825411.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-28
Publication Date
2024-11-08
Estimated Expiration
2043-12-28

AI Technical Summary

Technical Problem

The use of traditional PU foam tape in certain fields is limited, especially the low bonding strength of the surface glue and insufficient impact resistance, which is difficult to meet the needs of the precision electronics industry.

Method used

By corona treatment on the surface of the foam, and carbonization and refining with modified PET powder, sodium lignin sulfonate, zinc oxide and other materials, metallocene polyethylene and high-pressure polyethylene are added to form a closed-cell structure and then sprinkle Nano calcium carbonate powder, combined with specific adhesive formulations, produces foam double-sided tape with excellent bonding strength and impact resistance.

Benefits of technology

The tensile strength, peel strength and impact resistance of foam double-sided tape have been significantly improved, making it more suitable for use in fields such as precision electronics industry.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004635070060000111
    Figure BDA0004635070060000111
  • Figure BDA0004635070060000121
    Figure BDA0004635070060000121
Patent Text Reader

Abstract

The invention discloses a foam double-sided tape and a preparation process thereof, belonging to the technical field of tape preparation. The preparation of the foam double-sided tape comprises the following steps: S1, corona treatment of the foam surface; S2, applying adhesive on a double-sided release film to fit the foam lower surface; S3, applying adhesive on the release film to fit the foam upper surface, peeling off the release film at the same time, and rolling up and maturing; S4, slitting into specified widths according to production specifications to obtain the foam double-sided tape; and obtaining a foam double-sided tape with excellent bonding strength and impact resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of adhesive tape preparation, and in particular relates to a foam double-sided adhesive tape and a preparation process thereof. Background Art

[0002] Foam tape is an adhesive material with foam as the base material. It is made by applying pressure-sensitive adhesive on one or both sides of the foam and then covering it with a release film. This material has excellent sealing, compression deformation resistance and long-lasting resilience, and is widely used in various scenarios to ensure that accessories are protected from shock for a long time. Foam tape has many advantages. First, it can be used for bonding substrates such as curved surfaces, rough surfaces and smooth surfaces. The bonding performance is stable and will not drop significantly over time. Secondly, it has a slow rebound characteristic, and the deformation slowly recovers over time, and has good impact resistance. In addition, foam tape also has a lower density, which can save costs. In terms of substrates, foam tapes are mostly made of EVA, XPE, IXPE, PVC, PEF, EPDF, PU, ​​etc. However, with the development of science and technology and industry, the requirements for the use of tapes in production and manufacturing and daily life are getting higher and higher, and the use of traditional foam tapes with PU foam as the base material is restricted in certain specific fields. For example, the surface adhesive has low bonding strength and poor impact resistance, making it unsuitable for use in some precision electronics industries and other fields. Summary of the invention

[0003] The invention discloses a foam double-sided tape and a preparation process thereof, belonging to the technical field of tape preparation. The preparation of the foam double-sided tape comprises the following steps: S1, corona treatment of the foam surface; S2, applying adhesive on a double-sided release film to bond with the lower surface of the foam; S3, applying adhesive on the release film to bond with the upper surface of the foam, peeling off the release film at the same time, and rolling up and maturing; S4, slitting into strips of specified width according to production specifications to obtain the foam double-sided tape.

[0004] The technical problem to be solved by the present invention is to prepare a foam double-sided tape with excellent bonding strength and impact resistance.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A foam double-sided tape and a preparation process thereof, wherein the preparation of the foam double-sided tape comprises the following steps:

[0007] S1. Perform corona treatment on the foam surface;

[0008] S2, applying adhesive on the double-sided release film to fit it to the lower surface of the foam;

[0009] S3, applying adhesive on the release film to fit it to the upper surface of the foam, peeling off the release film, and rolling it up for maturation;

[0010] S4. Slice the tape into strips of specified width according to production specifications to obtain the foam double-sided tape.

[0011] As a preferred technical solution of the present invention, the preparation of the foam comprises the following steps:

[0012] S11, taking modified PET powder, sodium lignin sulfonate and zinc oxide, mixing, heating, carbonizing, acid washing and drying to obtain a carrier;

[0013] S12, mixing high-pressure polyethylene and metallocene polyethylene, drying, adding the carrier, placing in an internal mixer, sequentially adding azodicarbonamide, antioxidant 1010, zinc oxide, talcum powder, stirring, internal mixing, pressing, irradiation treatment, foaming, cooling, and obtaining material A;

[0014] S13, taking the material A and performing rolling hot pressing treatment on the surface of the material A using a heating roller to obtain a material B with a closed-cell structure;

[0015] S14, evenly sprinkle nano calcium carbonate powder on the surface of the material B, and then use a cooling roller to roll and cold press the surface of the material B sprinkled with the nano calcium carbonate powder to obtain the foam.

[0016] As a preferred technical solution of the present invention, the preparation of the adhesive comprises the following steps:

[0017] A1. Sodium lauryl sulfate, reactive emulsifier and deionized water are mixed and stirred, and acrylic acid, isooctyl acrylate, methyl methacrylate and vinylidene chloride are added and stirred to obtain material C;

[0018] A2. Deionized water, potassium persulfate, sodium dodecyl sulfate and reactive emulsifier are introduced into a reactor and stirred. 10-12% of the mass of the material C is introduced into the reactor and reacted in a nitrogen atmosphere. When a blue light phenomenon appears in the reactor, the remaining material C and potassium persulfate are added, the reaction is continued, the temperature is reduced and the pressure is released, and the material is filtered to obtain the adhesive.

[0019] As a preferred technical solution of the present invention, the preparation of the modified PET powder comprises the following steps:

[0020] Taking polyethylene terephthalate, drying it, adding silicon carbide whiskers and potassium titanate whiskers, extruding and granulating it, drying it, and grinding it to obtain the modified PET powder;

[0021] The mass ratio of the polyethylene terephthalate, the silicon carbide whisker and the potassium titanate whisker is 8-10:6-8:7-9.

[0022] As a preferred technical solution of the present invention, in step S11, the mass ratio of the modified PET powder, sodium lignin sulfonate and zinc oxide is 2-4:1-2:2-4.

[0023] As a preferred technical solution of the present invention, in step S12, the mass ratio of the high-pressure polyethylene, metallocene polyethylene, carrier, azodicarbonamide, antioxidant 1010, zinc oxide, and talc is 8-10: 1.5-1.8: 20-30: 0.5-0.6: 0.4-0.5: 0.55-0.65: 0.1-0.12.

[0024] As a preferred technical solution of the present invention, the dosage of the nano calcium carbonate powder is 2-3g / m 2 .

[0025] As a preferred technical solution of the present invention, in step A1, the mass ratio of sodium dodecyl sulfate, reactive emulsifier, deionized water, acrylic acid, isooctyl acrylate, methyl methacrylate and vinylidene chloride is 2-3:2.5-3:200:15-20:15-20:15-20:22-30.

[0026] As a preferred technical solution of the present invention, in step A2, the mass ratio of the deionized water, the potassium persulfate added for the first time, the sodium dodecyl sulfate, the reactive emulsifier, the material C, and the potassium persulfate added for the second time is 40-45:1.5-2.2:1.5-2:1.8-2.2:270-300:3-4.5.

[0027] A foam double-sided tape made using the above preparation process.

[0028] Beneficial effects of the present invention:

[0029] (1) The foam double-sided tape and its preparation process disclosed in the present invention improve the tensile toughness of the obtained carrier and the tensile strength of the foam double-sided tape by modifying PET and introducing synergistic silicon carbide whiskers and potassium titanate whiskers.

[0030] (2) The foam double-sided tape and its preparation process disclosed in the present invention enhance the peel strength of the foam double-sided tape by adding nano calcium carbonate powder as an adhesive, making the adhesive more firmly bonded.

[0031] (3) The foam double-sided tape and its preparation process disclosed in the present invention use metallocene polyethylene and high-pressure polyethylene as raw materials, attach them to a carrier, increase the nucleation points of the foaming system, and make the prepared foam have excellent impact resistance.

[0032] (4) The foam double-sided tape and its preparation process disclosed in the present invention use acrylic acid, isooctyl acrylate, methyl methacrylate, and vinylidene chloride as raw material monomers to prepare an adhesive, which has excellent adhesion and improves the bonding performance of the foam double-sided tape. DETAILED DESCRIPTION

[0033] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in combination with the embodiments.

[0034] Example 1

[0035] The preparation of a foam double-sided tape comprises the following steps:

[0036] S1. Perform corona treatment on the foam surface;

[0037] The preparation of the foam comprises the following steps:

[0038] S11, taking modified PET powder, sodium lignin sulfonate and zinc oxide, mixing, heating at 275°C for 10 minutes, carbonizing at 490°C for 8 hours, acid washing until the pH is neutral, and drying to obtain a carrier; the mass ratio of the modified PET powder, sodium lignin sulfonate and zinc oxide is 2:1:2;

[0039] S12, take high-pressure polyethylene and metallocene polyethylene, mix them at 80°C and dry for 2h, add the carrier, put them in an internal mixer, add azodicarbonamide, antioxidant 1010, zinc oxide and talcum powder in turn, stir for 0.5h, internally knead and mix at 120°C for 10min, then transfer the internally kneaded materials to a flat vulcanizer and press them at 140°C and 4MPa pressure for 2min, irradiate the pressed materials with an electron accelerator at 85kGy, foam the irradiated materials at 240°C for 2min, cool to room temperature, and obtain material A; the mass ratio of the high-pressure polyethylene, metallocene polyethylene, carrier, azodicarbonamide, antioxidant 1010, zinc oxide and talcum powder is 8:1.5:20:0.5:0.4:0.55:0.1;

[0040] S13, taking the material A and performing rolling hot pressing on the surface of the material A using a heating roller to obtain a material B with a closed-cell structure; the hot pressing temperature is 270° C.;

[0041] S14, evenly sprinkle nano calcium carbonate powder on the surface of the material B, and then use a cooling roller to perform rolling cold pressing treatment on the surface of the material B sprinkled with the nano calcium carbonate powder, the cold pressing temperature is 40° C., and the foam is obtained;

[0042] The dosage of the nano calcium carbonate powder is 2g / m 2 .

[0043] The preparation of the modified PET powder comprises the following steps:

[0044] Polyethylene terephthalate is dried at 125° C. for 4 hours, placed in a twin-screw granulator with a length-to-diameter ratio of L:D=40, silicon carbide whiskers and potassium titanate whiskers are added, extruded and granulated at 250° C., dried at 125° C. for 4 hours, and ground to obtain the modified PET powder;

[0045] The mass ratio of the polyethylene terephthalate, the silicon carbide whisker and the potassium titanate whisker is 8:6:7.

[0046] S2, applying adhesive on the double-sided release film to fit it to the lower surface of the foam;

[0047] S3, applying adhesive on the release film to fit it to the upper surface of the foam, peeling off the release film, and rolling it up for maturation;

[0048] The preparation of the adhesive comprises the following steps:

[0049] A1. Mix sodium dodecyl sulfate, reactive emulsifier and deionized water, stir for 0.5h, add acrylic acid, isooctyl acrylate, methyl methacrylate and vinylidene chloride, stir for 2h to obtain material C; the mass ratio of sodium dodecyl sulfate, reactive emulsifier, deionized water, acrylic acid, isooctyl acrylate, methyl methacrylate and vinylidene chloride is 2:2.5:200:15:15:15:22;

[0050] A2, deionized water, potassium persulfate, sodium dodecyl sulfate, and reactive emulsifier were introduced into a reactor, stirred for 0.5 h, 10% of the mass of the material C was introduced into the reactor, and reacted in a nitrogen atmosphere, and when a blue light phenomenon appeared in the reactor, the remaining material C and potassium persulfate were added, and the reaction was continued, the temperature was lowered and the pressure was released, and the material was filtered to obtain the adhesive;

[0051] The mass ratio of the deionized water, the potassium persulfate added for the first time, sodium lauryl sulfate, the reactive emulsifier, material C, and the potassium persulfate added for the second time is 40:1.5:1.5:1.8:270:3;

[0052] The pressure of the first reaction is 0.24 MPa and the temperature is 74°C;

[0053] The continued reaction refers to reacting at 0.24 MPa and 85° C. for 3 hours.

[0054] S4. Slice the tape into strips of specified width according to production specifications to obtain the foam double-sided tape.

[0055] Example 2

[0056] The preparation of a foam double-sided tape comprises the following steps:

[0057] S1. Perform corona treatment on the foam surface;

[0058] The preparation of the foam comprises the following steps:

[0059] S11, taking modified PET powder, sodium lignin sulfonate and zinc oxide, mixing, heating at 280°C for 15 minutes, carbonizing at 500°C for 9 hours, acid washing until the pH is neutral, and drying to obtain a carrier; the mass ratio of the modified PET powder, sodium lignin sulfonate and zinc oxide is 3:1.5:3;

[0060] S12, take high-pressure polyethylene and metallocene polyethylene, mix them, dry them at 85°C for 2.5h, add the carrier, put them in an internal mixer, add azodicarbonamide, antioxidant 1010, zinc oxide, and talcum powder in sequence, stir for 0.8h, internally knead and mix them at 120°C for 11min, then transfer the internally kneaded materials to a flat vulcanizer and press them at 140°C and 5MPa pressure for 2.5min, irradiate the pressed materials with an electron accelerator at 90kGy, foam the irradiated materials at 250°C for 2.5min, and cool them to room temperature to obtain material A; the mass ratio of the high-pressure polyethylene, metallocene polyethylene, carrier, azodicarbonamide, antioxidant 1010, zinc oxide, and talcum powder is 9:1.65:25:0.55:0.45:0.6:0.11;

[0061] S13, taking the material A and performing rolling hot pressing treatment on the surface of the material A using a heating roller to obtain a material B with a closed-cell structure; the hot pressing temperature is 280° C.;

[0062] S14, evenly sprinkle nano calcium carbonate powder on the surface of the material B, and then use a cooling roller to roll and cold press the surface of the material B sprinkled with the nano calcium carbonate powder, the cold pressing temperature is 50° C., to obtain the foam;

[0063] The dosage of the nano calcium carbonate powder is 2.5 g / m 2 .

[0064] The preparation of the modified PET powder comprises the following steps:

[0065] Polyethylene terephthalate is dried at 130° C. for 5 hours, placed in a twin-screw granulator with an aspect ratio of L:D=40, silicon carbide whiskers and potassium titanate whiskers are added, extruded and granulated at 255° C., dried at 130° C. for 5 hours, and ground to obtain the modified PET powder;

[0066] The mass ratio of the polyethylene terephthalate, the silicon carbide whisker and the potassium titanate whisker is 9:7:8.

[0067] S2, applying adhesive on the double-sided release film to fit it to the lower surface of the foam;

[0068] S3, applying adhesive on the release film to fit it to the upper surface of the foam, peeling off the release film, and rolling it up for maturation;

[0069] The preparation of the adhesive comprises the following steps:

[0070] A1. Mix sodium dodecyl sulfate, reactive emulsifier and deionized water, stir for 0.8h, add acrylic acid, isooctyl acrylate, methyl methacrylate and vinylidene chloride, stir for 2.5h to obtain material C; the mass ratio of sodium dodecyl sulfate, reactive emulsifier, deionized water, acrylic acid, isooctyl acrylate, methyl methacrylate and vinylidene chloride is 2.5:2.8:200:18:18:18:26;

[0071] A2, deionized water, potassium persulfate, sodium dodecyl sulfate, and reactive emulsifier were introduced into a reactor, stirred for 0.8h, 11% of the mass of the material C was introduced into the reactor, and reacted in a nitrogen atmosphere, and when a blue light phenomenon appeared in the reactor, the remaining material C and potassium persulfate were added, and the reaction was continued, the temperature was lowered and the pressure was released, and the material was filtered to obtain the adhesive;

[0072] The mass ratio of the deionized water, the potassium persulfate added for the first time, sodium lauryl sulfate, the reactive emulsifier, the material C, and the potassium persulfate added for the second time is 42:1.8:1.8:2:285:4;

[0073] The pressure of the first reaction is 0.25 MPa and the temperature is 75°C;

[0074] The continued reaction refers to reacting at 0.25 MPa and 86° C. for 4 hours.

[0075] S4. Slice the tape into strips of specified width according to production specifications to obtain the foam double-sided tape.

[0076] Example 3

[0077] The preparation of a foam double-sided tape comprises the following steps:

[0078] S1. Perform corona treatment on the foam surface;

[0079] The preparation of the foam comprises the following steps:

[0080] S11, taking modified PET powder, sodium lignin sulfonate and zinc oxide, mixing, heating at 285°C for 20 minutes, carbonizing at 510°C for 10 hours, acid washing until the pH is neutral, and drying to obtain a carrier; the mass ratio of the modified PET powder, sodium lignin sulfonate and zinc oxide is 4:2:4;

[0081] S12, take high-pressure polyethylene and metallocene polyethylene, mix them, dry them at 90°C for 3h, add the carrier, put them in an internal mixer, add azodicarbonamide, antioxidant 1010, zinc oxide, and talcum powder in sequence, stir for 1h, internally knead and mix them at 120°C for 12min, then transfer the internally kneaded and mixed materials to a flat vulcanizer and press them at 140°C and 6MPa pressure for 3min, irradiate the pressed materials with an electron accelerator at 95kGy, foam the irradiated materials at 260°C for 3min, and cool them to room temperature to obtain material A; the mass ratio of the high-pressure polyethylene, metallocene polyethylene, carrier, azodicarbonamide, antioxidant 1010, zinc oxide, and talcum powder is 10:1.8:30:0.6:0.5:0.65:0.12;

[0082] S13, taking the material A and performing rolling hot pressing treatment on the surface of the material A using a heating roller to obtain a material B with a closed-cell structure; the hot pressing temperature is 285° C.;

[0083] S14, evenly sprinkle nano calcium carbonate powder on the surface of the material B, and then use a cooling roller to perform rolling cold pressing treatment on the surface of the material B sprinkled with the nano calcium carbonate powder, the cold pressing temperature is 60° C., and the foam is obtained;

[0084] The dosage of the nano calcium carbonate powder is 3g / m 2 .

[0085] The preparation of the modified PET powder comprises the following steps:

[0086] Taking polyethylene terephthalate and drying it at 135° C. for 6 hours, placing it in a twin-screw granulator with an aspect ratio of L:D=40, adding silicon carbide whiskers and potassium titanate whiskers, extruding and granulating at 250-260° C., drying it at 135° C. for 6 hours, and grinding it to obtain the modified PET powder;

[0087] The mass ratio of the polyethylene terephthalate, the silicon carbide whisker and the potassium titanate whisker is 10:8:9.

[0088] S2, applying adhesive on the double-sided release film to fit it to the lower surface of the foam;

[0089] S3, applying adhesive on the release film to fit it to the upper surface of the foam, peeling off the release film, and rolling it up for maturation;

[0090] The preparation of the adhesive comprises the following steps:

[0091] A1. Mix sodium dodecyl sulfate, reactive emulsifier and deionized water, stir for 1 hour, add acrylic acid, isooctyl acrylate, methyl methacrylate and vinylidene chloride, stir for 3 hours to obtain material C; the mass ratio of sodium dodecyl sulfate, reactive emulsifier, deionized water, acrylic acid, isooctyl acrylate, methyl methacrylate and vinylidene chloride is 3:3:200:20:20:20:30;

[0092] A2, deionized water, potassium persulfate, sodium dodecyl sulfate, and reactive emulsifier were introduced into a reactor, stirred for 1 hour, 12% of the mass of the material C was introduced into the reactor, and reacted in a nitrogen atmosphere, and when a blue light phenomenon appeared in the reactor, the remaining material C and potassium persulfate were added, and the reaction was continued, the temperature was lowered and the pressure was released, and the material was filtered to obtain the adhesive;

[0093] The mass ratio of the deionized water, the potassium persulfate added for the first time, sodium lauryl sulfate, the reactive emulsifier, the material C, and the potassium persulfate added for the second time is 45:2.2:2:2.2:300:4.5;

[0094] The pressure of the first reaction is 0.26MPa and the temperature is 76°C;

[0095] The continued reaction refers to reacting at 0.26 MPa and 87° C. for 5 hours.

[0096] S4. Slice the tape into strips of specified width according to production specifications to obtain the foam double-sided tape.

[0097] Comparative Example 1

[0098] The difference from Example 2 is that the PET powder is not modified.

[0099] Comparative Example 2

[0100] The difference from Example 2 is that in the preparation of the modified PET powder, the mass ratio of polyethylene terephthalate, silicon carbide whiskers and potassium titanate whiskers is 9:15:0.

[0101] Comparative Example 3

[0102] The difference from Example 2 is that in the preparation of the modified PET powder, the mass ratio of polyethylene terephthalate, silicon carbide whiskers and potassium titanate whiskers is 9:0:15.

[0103] Comparative Example 4

[0104] The difference from Example 2 is that no carrier is added in the preparation of the foam.

[0105] Comparative Example 5

[0106] The difference from Example 2 is that metallocene polyethylene is not added in the preparation of the foam.

[0107] Comparative Example 6

[0108] The difference from Example 2 is that high-pressure polyethylene is not added in the preparation of the foam.

[0109] Comparative Example 7

[0110] The difference from Example 2 is that no nano calcium carbonate powder is added in the preparation of the foam.

[0111] Comparative Example 8

[0112] The difference from Example 2 is that in the preparation of the adhesive, the mass ratio of acrylic acid, isooctyl acrylate, methyl methacrylate and vinylidene chloride is 18:44:18:0.

[0113] Comparative Example 9

[0114] The difference from Example 2 is that in the preparation of the adhesive, the mass ratio of acrylic acid, isooctyl acrylate, methyl methacrylate and vinylidene chloride is 18:18:0:44.

[0115] Comparative Example 10

[0116] The difference from Example 2 is that in the preparation of the adhesive, the mass ratio of acrylic acid, isooctyl acrylate, methyl methacrylate and vinylidene chloride is 36:0:18:26.

[0117] Comparative Example 11

[0118] The difference from Example 2 is that in the preparation of the adhesive, the mass ratio of acrylic acid, isooctyl acrylate, methyl methacrylate and vinylidene chloride is 0:18:36:26.

[0119] Performance Testing

[0120] Test Example 1 Foam Double-Sided Tape Performance Test

[0121] 1) Conduct tensile properties test according to standard GB / T 7753-1987;

[0122] 2) Peel strength test according to GB / T 2792-1998;

[0123] 3) Impact resistance test according to standard NF X41-033-1996;

[0124] The foam double-sided tapes obtained in Examples 1-3 and Comparative Examples 1-11 were subjected to performance tests according to the above standards. The test results are shown in Table 1 below.

[0125] Table 1

[0126]

[0127]

[0128] Discussion and Analysis

[0129] As shown in Table 1, the foam double-sided tapes obtained in Examples 1-3 have excellent tensile toughness, peel strength and impact resistance;

[0130] In Comparative Example 1, since the PET powder was not modified, its tensile strength was significantly reduced;

[0131] In Comparative Example 2-3, due to the different ratios of silicon carbide whiskers and potassium titanate whiskers in the process of modifying PET powder, the tensile strength of the foam double-sided tape obtained in Comparative Example 2-3 is reduced;

[0132] In Comparative Example 4, since no carrier was added during the preparation of the foam, its tensile strength and impact resistance were significantly reduced;

[0133] In Comparative Example 5-6, due to the different ratios of metallocene polyethylene and high-pressure polyethylene, the impact resistance of the obtained foam double-sided tape is reduced;

[0134] Comparative Example 7 did not add nano calcium carbonate powder, resulting in reduced peel strength of the obtained foam double-sided tape;

[0135] In Comparative Examples 8-11, due to the different ratios of raw material monomers used to prepare the adhesive, the peel strength of the obtained foam double-sided tape was reduced.

[0136] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. A preparation process of a foam double-sided tape, characterized in that the preparation of the foam double-sided tape comprises the following steps: S1. Perform corona treatment on the foam surface; S2, applying adhesive on the double-sided release film to fit it to the lower surface of the foam; S3, applying adhesive on the release film to fit it to the upper surface of the foam, peeling off the release film, and rolling it up for maturation; S4, dividing into strips of specified width according to production specifications, thus obtaining the foam double-sided tape; The preparation of the foam comprises the following steps: S11, taking modified PET powder, sodium lignin sulfonate and zinc oxide, mixing, heating, carbonizing, acid washing and drying to obtain a carrier; S12, mixing high-pressure polyethylene and metallocene polyethylene, drying, adding the carrier, placing in an internal mixer, sequentially adding azodicarbonamide, antioxidant 1010, zinc oxide, talcum powder, stirring, internal mixing, pressing, irradiation treatment, foaming, cooling, and obtaining material A; S13, taking the material A and performing rolling hot pressing treatment on the surface of the material A using a heating roller to obtain a material B with a closed-cell structure; S14, evenly sprinkle nano calcium carbonate powder on the surface of the material B, and then use a cooling roller to roll and cold press the surface of the material B sprinkled with the nano calcium carbonate powder to obtain the foam; The preparation of the modified PET powder comprises the following steps: Taking polyethylene terephthalate, drying it, adding silicon carbide whiskers and potassium titanate whiskers, extruding and granulating it, drying it, and grinding it to obtain the modified PET powder; The mass ratio of polyethylene terephthalate, silicon carbide whisker and potassium titanate whisker is 8-10:6-8:7-9; In step S11, the mass ratio of the modified PET powder, sodium lignin sulfonate, and zinc oxide is 2-4:1-2:2-4; In step S12, the mass ratio of the high pressure polyethylene, metallocene polyethylene, carrier, azodicarbonamide, antioxidant 1010, zinc oxide, and talcum powder is 8-10: 1.5-1.8:20-30:0.5-0.6:0.4-0.5:0.55-0.65:0.1-0.12; The dosage of the nano calcium carbonate powder is 2-3 g / m 2 .

2. The preparation process of a foam double-sided tape according to claim 1, characterized in that: The preparation of the adhesive comprises the following steps: A1. Sodium lauryl sulfate, reactive emulsifier and deionized water are mixed and stirred, and acrylic acid, isooctyl acrylate, methyl methacrylate and vinylidene chloride are added and stirred to obtain material C; A2. Deionized water, potassium persulfate, sodium dodecyl sulfate and reactive emulsifier are introduced into a reactor and stirred. 10-12% of the mass of the material C is introduced into the reactor and reacted in a nitrogen atmosphere. When a blue light phenomenon appears in the reactor, the remaining material C and potassium persulfate are added, the reaction is continued, the temperature is reduced and the pressure is released, and the material is filtered to obtain the adhesive.

3. The preparation process of a foam double-sided tape according to claim 2, characterized in that: In step A1, the mass ratio of sodium dodecyl sulfate, reactive emulsifier, deionized water, acrylic acid, isooctyl acrylate, methyl methacrylate and vinylidene chloride is 2-3:2.5-3:200:15-20:15-20:15-20:22-30.

4. The preparation process of a foam double-sided tape according to claim 2, characterized in that: In step A2, the mass ratio of the deionized water, the potassium persulfate added for the first time, the sodium dodecyl sulfate, the reactive emulsifier, the material C, and the potassium persulfate added for the second time is 40-45:1.5-2.2:1.5-2:1.8-2.2:270-300:3-4.

5.

5. A foam double-sided tape obtained by the preparation process according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • High-strength binder composition

    CN104830241A

  • Enhanced composite foam material and preparation method thereof

    CN109401006A

  • LED lamp molding printing process

    CN109659419A

  • Modified ZnO / PET protective film with high barrier property and preparation method thereof

    CN111019305A

  • Nano-modified PET packing belt

    CN113402858A