A high refractive index epoxy adhesive and preparation method thereof
By introducing sulfur atoms and hydrogenated bisphenol A into epoxy resin adhesives, a high refractive index polythiol curing agent is prepared, which solves the problem of low refractive index of traditional epoxy resin adhesives and achieves wide application in the optical field. And improve its weather resistance and bonding performance.
Patent Information
- Application Number
- CN202311831738.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-28
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-12-28
AI Technical Summary
The refractive index of traditional epoxy resin adhesives is not high, which limits its application in the optical field.
By introducing sulfur atoms, a high refractive index polythiol curing agent is prepared, and combined with hydrogenated bisphenol A, the refractive index of the epoxy adhesive is increased. The two-component system is cured at room temperature and is suitable for sealing and bonding of optical devices. .
It achieves a high refractive index of epoxy adhesive, reaching more than 1.58, and improves its weather resistance and bonding performance, making it suitable for the application of a variety of optical devices.
Smart Images

Figure BDA0004636529940000021 
Figure BDA0004636529940000061 
Figure FDA0004636529930000011
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of adhesives, and in particular relates to a high refractive index epoxy adhesive and a preparation method thereof. Background Art
[0002] In recent years, with the rapid development of social economy, people have increasingly higher requirements for the performance of various electronic products, of which optical devices are an important part. Resins with high refractive index are widely used in detectors, light-emitting diodes, microlens arrays and other fields, and have broad application prospects and value. Epoxy resin adhesives have excellent physical and mechanical properties, electrical insulation properties, heat resistance and bonding properties, and are widely used in aerospace, electronics, automotive machinery and other fields. However, traditional epoxy resin adhesives generally have the problem of low refractive index, and still have certain defects if they are to be used in the optical field. Summary of the invention
[0003] The present invention aims to solve the problem that the refractive index of existing epoxy adhesives is not high, and provides a method for preparing a high refractive index epoxy adhesive. The high refractive index epoxy adhesive has the characteristics of high refractive index and good weather resistance, and can be cured at room temperature, easy to operate, and can be applied to the sealing and bonding of various optical devices. In order to solve the above problems, the technical solution of the present invention is as follows:
[0004] A high refractive index epoxy adhesive, comprising two components A and B, measured by weight:
[0005] Component A: 70-90 parts of bisphenol A epoxy resin; 20-10 parts of hydrogenated bisphenol A epoxy resin; 1-2 parts of coupling agent;
[0006] Component B: 95-99 parts of polythiol; 1-5 parts of accelerator; 1-3 parts of thixotropic agent;
[0007] The mixing mass ratio of the A and B components is 100:70-90;
[0008] The structural formula of the polythiol is shown in formula (1):
[0009]
[0010] in,
[0011] Sulfur atoms have a high molar refractive index, good environmental stability, are non-toxic and harmless, and polymers containing sulfur atoms generally have excellent electrical and optical properties. The present invention introduces polysulfide elements into the epoxy adhesive to effectively improve the refractive index of the epoxy adhesive.
[0012] Furthermore, the preparation method of the polythiol comprises the following steps:
[0013] ① Add 2,3-dithio(2-mercapto)-1-propanethiol and triethylamine into a three-necked flask, add solvent toluene to dilute, and heat the system in an oil bath to 60-80°C;
[0014] ②Continuously add the difunctional epoxy diluent to the three-necked flask and react for 1 to 3 hours after the addition is completed;
[0015] ③Continuously add diethyl sulfide dropwise into the three-necked flask and react for 1 to 3 hours after the addition is completed;
[0016] ④ The obtained solution was evaporated at 40°C and negative pressure of -0.1MPa to remove toluene, thereby obtaining a polythiol curing agent;
[0017] The molar ratio of the 2,3-dithio(2-mercapto)-1-propanethiol, the difunctional epoxy diluent, diethyl sulfide and triethylamine is 100:(10-20):(5-10):(0.2-0.5).
[0018] Furthermore, the difunctional epoxy diluent is one or a combination of two or more of 1,4-butanediol glycidyl ether, polypropylene glycol glycidyl ether, neopentyl glycol diglycidyl ether or 1,6-hexanediol diglycidyl ether.
[0019] Furthermore, the coupling agent is one or a combination of γ-glycidyloxypropyltrimethoxysilane or 3-glycidyloxypropyltriethoxysilane.
[0020] Furthermore, the accelerator is one or a combination of 2,4,6-tris(dimethylaminomethyl)phenol or N,N-dimethylbenzylamine.
[0021] Furthermore, the thixotropic agent is hydrophobic fumed silica.
[0022] The second object of the present invention is to provide a method for preparing the above-mentioned high refractive index epoxy adhesive, the preparation steps of which are:
[0023] Preparation of component A: add bisphenol A epoxy resin, hydrogenated bisphenol A epoxy resin and coupling agent into a planetary mixer according to a proportion, mix them evenly under vacuum conditions, and then pack them;
[0024] Preparation of component B: Add polythiol, accelerator and thixotropic agent into a planetary mixer according to the proportion, mix evenly under vacuum conditions, and then package.
[0025] When using the high refractive index epoxy adhesive, components A and B are mixed in a mass ratio of 100:70-90.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] The invention prepares a polythiol curing agent with high sulfur content by introducing sulfur atoms, thereby improving the refractive index of the epoxy adhesive, which can reach above 1.58; and the polythiol curing agent works together with hydrogenated bisphenol A in the system, so that the adhesive has excellent weather resistance; the high refractive index epoxy adhesive system of the invention can be cured at room temperature, is easy to operate, and is convenient for construction operation, and has broad application prospects in the sealing and bonding of optical devices. DETAILED DESCRIPTION
[0028] The principles and features of the present invention are described below in conjunction with examples. The examples are only used to explain the present invention and are not used to limit the scope of the present invention.
[0029] Embodiment 1:
[0030] A preparation method of a high refractive index epoxy adhesive, the preparation steps of which are as follows:
[0031] (1) Synthesis of polythiol: ① Weigh 130 g of 2,3-dithio(2-mercapto)-1-propanethiol and 0.5 g of triethylamine into a three-necked flask, add 500 ml of solvent toluene to dilute, and heat the system to 80°C in an oil bath; ② 10 g of 1,4-butanediol glycidyl ether is continuously added dropwise into the three-necked flask, and the reaction is continued for 3 h after the addition is completed; ③ 3.5 g of diethyl sulfide is continuously added dropwise into the three-necked flask, and the reaction is continued for 3 h after the addition is completed; ④ The obtained solution is evaporated at 40°C and negative pressure of -0.1 MPa to remove toluene, thereby obtaining a polythiol curing agent.
[0032] (2) Preparation of component A: 75 g of bisphenol A epoxy resin NPEL-128, 25 g of hydrogenated bisphenol A epoxy resin ADEKA EP-4080E, and 1 g of γ-glycidyloxypropyltrimethoxysilane were added to a high-speed planetary agitator. The stirring speed was 400 r / min and the mixture was discharged after stirring for 2 h while maintaining a vacuum degree of not less than -0.08 MPa.
[0033] (3) Preparation method of component B: 95 g of polythiol, 5 g of 2,4,6-tris(dimethylaminomethyl)phenol and 2 g of hydrophobic fumed silica were added to a high-speed planetary agitator. The stirring speed was 400 r / min and the mixture was discharged after stirring for 2 h while maintaining a vacuum degree of not less than -0.08 MPa.
[0034] When using, components A and B need to be mixed evenly, with the mixing ratio being 100:70 by mass.
[0035] Embodiment 2:
[0036] A preparation method of a high refractive index epoxy adhesive, the preparation steps of which are as follows:
[0037] (1) Synthesis method of polythiol: ① Weigh 130g of 2,3-dithio(2-mercapto)-1-propanethiol and 0.5g of triethylamine into a three-necked flask, add 500ml of solvent toluene to dilute, and heat the system to 80°C in an oil bath; ② 20g of 1,4-butanediol glycidyl ether is continuously added dropwise into the three-necked flask, and the reaction is continued for 3h after the addition is completed; ③ 3.5g of diethyl sulfide is continuously added dropwise into the three-necked flask, and the reaction is continued for 3h after the addition is completed; ④ The obtained solution is evaporated to remove toluene at 40°C and negative pressure of -0.1MPa to obtain a polythiol curing agent.
[0038] (2) Preparation method of component A: 75 g of bisphenol A epoxy resin NPEL-128, 25 g of hydrogenated bisphenol A epoxy resin ADEKAEP-4080E, and 1 g of γ-glycidyloxypropyltrimethoxysilane are added to a high-speed planetary agitator. The stirring speed is 400 r / min and the mixture is discharged after stirring for 2 hours while maintaining a vacuum degree of not less than -0.08 MPa.
[0039] (3) Preparation method of component B: 95 g of polythiol, 5 g of 2,4,6-tris(dimethylaminomethyl)phenol and 2 g of hydrophobic fumed silica were added to a high-speed planetary agitator. The stirring speed was 400 r / min and the mixture was discharged after stirring for 2 h while maintaining a vacuum degree of not less than -0.08 MPa.
[0040] When using, components A and B need to be mixed evenly, with the mixing ratio being 100:70 by mass.
[0041] Embodiment 3:
[0042] A high refractive index epoxy adhesive is prepared by the same method as in Example 2 and will not be described in detail herein.
[0043] When using, components A and B need to be mixed evenly, with the mixing ratio being 100:80 by mass.
[0044] Comparative Example 1:
[0045] A preparation method of epoxy adhesive, the preparation steps are as follows:
[0046] (1) Synthesis method of polythiol: ① Weigh 195g of trimethylolpropane tri-3-mercaptopropionate and 0.5g of triethylamine into a three-necked flask, add 500ml of solvent toluene to dilute, and heat the system to 60-80°C by oil bath heating; ② 10g of 1,4-butanediol glycidyl ether is continuously added dropwise into the three-necked flask, and the reaction is continued for 3h after the addition is completed; ③ 3.5g of diethyl sulfide is continuously added dropwise into the three-necked flask, and the reaction is continued for 3h after the addition is completed; ④ The obtained solution is evaporated at 40°C and negative pressure of -0.1MPa to remove toluene, thereby obtaining a polythiol curing agent.
[0047] (2) Preparation method of component A: 75 g of bisphenol A epoxy resin NPEL-128, 25 g of hydrogenated bisphenol A epoxy resin ADEKAEP-4080E, and 1 g of γ-glycidyloxypropyltrimethoxysilane are added to a high-speed planetary agitator. The stirring speed is 400 r / min and the mixture is discharged after stirring for 2 hours while maintaining a vacuum degree of not less than -0.08 MPa.
[0048] (3) Preparation method of component B: 95 g of polythiol, 5 g of 2,4,6-tris(dimethylaminomethyl)phenol and 2 g of hydrophobic fumed silica were added to a high-speed planetary agitator. The stirring speed was 400 r / min and the mixture was discharged after stirring for 2 h while maintaining a vacuum degree of not less than -0.08 MPa.
[0049] When using, components A and B need to be mixed evenly, with the mixing ratio being 100:80 by mass.
[0050] Comparative Example 2:
[0051] A preparation method of epoxy adhesive, the preparation steps are as follows:
[0052] (1) Preparation method of component A: 75 g of bisphenol A epoxy resin NPEL-128, 25 g of hydrogenated bisphenol A epoxy resin ADEKAEP-4080E, and 1 g of γ-glycidyloxypropyltrimethoxysilane are added to a high-speed planetary agitator. The stirring speed is 400 r / min and the mixture is stirred for 2 h while maintaining a vacuum degree of not less than -0.08 MPa. The mixture is then discharged.
[0053] (2) Preparation method of component B: 95g of Corning Capcure 3800 polythiol, 5g of 2,4,6-tris(dimethylaminomethyl)phenol, and 1g of hydrophobic fumed silica were added to a high-speed planetary agitator. The stirring speed was 400r / min and the material was discharged after stirring for 2h while maintaining the vacuum degree not less than -0.08Mpa.
[0054] When using, components A and B need to be mixed evenly, with the mixing ratio being 100:100 by mass.
[0055] Test: The epoxy adhesives obtained in Examples 1-3 and Comparative Examples 1-2 were cured at 25°C and 50% RH for 24 hours, and then samples were made. The refractive index test required the sample to be made into a 30mm*8mm*5mm thick rectangular specimen and tested with an Abbe refractometer; the yellowing test was performed after the curing was completed, and the specimen was placed in an oven at 80°C for 100 hours, and the yellowing of the sample was observed; the tensile shear strength was tested for mechanical properties according to the standard (GB / T2792-2014); the test results are shown in Table 1:
[0056] Table 1 Performance test data results of embodiments and comparative examples
[0057]
[0058] From the test results, it can be seen that in Examples 1-3, by adjusting the ratio of the polythiol in the synthesis method and adjusting the mixing ratio of the A and B components, the refractive index can be adjusted and can reach above 1.58. Compared with Comparative Examples 1-2, the polythiol synthesized by the present invention is more stable under high-temperature epoxy because of the selection of thiol with a polysulfide structure and the thiol itself having no ester bond. It has better yellowing resistance when combined with hydrogenated bisphenol A epoxy resin, and the thiol has excellent bonding effect on transparent glass substrates.
[0059] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A high refractive index epoxy adhesive, characterized in that: It includes two components, A and B, calculated by weight. Component A: 70-90 parts of bisphenol A epoxy resin; 20-10 parts of hydrogenated bisphenol A epoxy resin; 1-2 parts of coupling agent; Component B: 95-99 parts of polythiol; 1-5 parts of accelerator; 1-3 parts of thixotropic agent; The mass ratio of the A and B components is 100:70-90; The structural formula of the polythiol is shown in formula (1): in, 2. The high refractive index epoxy adhesive according to claim 1, characterized in that: The preparation method of the polythiol comprises the following steps: ① Add 2,3-dithio(2-mercapto)-1-propanethiol and triethylamine into a three-necked flask, add solvent toluene to dilute, and heat the system in an oil bath to 60-80°C; ②Continuously add the difunctional epoxy diluent to the three-necked flask and react for 1 to 3 hours after the addition is completed; ③Continuously add diethyl sulfide dropwise into the three-necked flask and react for 1 to 3 hours after the addition is completed; ④ The obtained solution was evaporated at 40°C and negative pressure of -0.1MPa to remove toluene, thereby obtaining a polythiol curing agent; The molar ratio of the 2,3-dithio(2-mercapto)-1-propanethiol, the difunctional epoxy diluent, diethyl sulfide and triethylamine is 100:(10-20):(5-10):(0.2-0.5).
3. The high refractive index epoxy adhesive according to claim 2, characterized in that: The difunctional epoxy diluent is one or a combination of two or more of 1,4-butanediol glycidyl ether, polypropylene glycol glycidyl ether, neopentyl glycol diglycidyl ether or 1,6-hexanediol diglycidyl ether.
4. The high refractive index epoxy adhesive according to claim 1, characterized in that: The coupling agent is one or a combination of γ-glycidyloxypropyltrimethoxysilane and 3-glycidyloxypropyltriethoxysilane.
5. The high refractive index epoxy adhesive according to claim 1, characterized in that: The accelerator is one or a combination of 2,4,6-tris(dimethylaminomethyl)phenol or N,N-dimethylbenzylamine.
6. The high refractive index epoxy adhesive according to claim 1, characterized in that: The thixotropic agent is hydrophobic fumed silica.
7. A method for preparing the high refractive index epoxy adhesive according to any one of claims 1 to 6, characterized in that: The preparation steps are: Preparation of component A: Add bisphenol A epoxy resin, hydrogenated bisphenol A epoxy resin and coupling agent into a planetary mixer according to a proportion, mix them evenly under vacuum conditions, and then pack them; Preparation of component B: Add polythiol, accelerator and thixotropic agent into a planetary mixer according to the proportion, mix evenly under vacuum conditions, and then package.
Citation Information
Patent Citations
Low-stress transparent epoxy resin adhesive capable of curing fast at room temperature
CN104479607A
Modified polymercaptan and preparation method and application thereof
CN110790930A