A laminated fluorine film for use in flexible copper-clad laminates and its preparation method
By adding spherical silicon to the laminated structure of fiberglass cloth and polytetrafluoroethylene layer, the problems of insufficient thermal expansion coefficient and tensile strength of polytetrafluoroethylene film are solved, and a low-loss, high-strength laminated fluorofilm is prepared, which is suitable for high-frequency flexible copper clad laminate.
Patent Information
- Application Number
- CN202211170140.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-22
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2042-09-22
AI Technical Summary
When polytetrafluoroethylene (PTFE) film is used in flexible copper-clad laminates, it suffers from insufficient thermal expansion coefficient and tensile strength, which fails to meet the requirements of high frequency and low loss.
A laminated structure of fiberglass cloth and polytetrafluoroethylene layer containing spherical silicon is adopted, and the thickness ratio is controlled at 1:3 to 9. The low loss characteristics of spherical silicon and the support of fiberglass cloth are used to improve tensile strength and reduce the coefficient of thermal expansion.
A multilayer fluorine film with low thermal expansion coefficient and high tensile strength was prepared to meet the requirements of thinness and flexibility of flexible copper clad laminates and reduce transmission loss.
Abstract
Description
Technical Field
[0001] This invention relates to the field of copper clad laminate technology, and more specifically to a laminated fluorine film that can be used in flexible copper clad laminates and its preparation method. Background Technology
[0002] With the rapid development and widespread adoption of 5G communication systems, the communication frequency bands for mobile communication devices such as mobile phones and tablets are constantly increasing, expanding from the original 800MHz to 3G to 5G and millimeter wave bands (28G, 40G). In addition, automotive communication is also developing rapidly, and the increase in the number of communication channels has placed higher demands on the low-loss of high-frequency flexible printed circuit boards in the high-frequency and even microwave fields.
[0003] Flexible copper clad laminates (FCCLs), used as substrates for high-frequency, low-loss flexible printed circuit boards (FPCBs), require not only the general performance characteristics (peel strength, electrical properties, etc.) of FCCLs, but also a stable dielectric constant (Dk) and an extremely low dielectric loss tangent (Df). Polytetrafluoroethylene (PTFE) has a symmetrical structure and provides excellent electrical properties. Its dielectric constant (1MHz) is as low as 2.1, and its dielectric loss tangent is around 10°. -4 At the horizontal level, among all resins, PTFE has the lowest dielectric constant (Dk) and dielectric loss tangent (Df), making it an ideal low-loss electrical performance dielectric material.
[0004] Although polytetrafluoroethylene (PTFE) possesses excellent dielectric constant (Dk) and loss tangent (Df), pure PTFE exhibits a very high coefficient of thermal expansion (CTE), reaching 150–200; furthermore, its tensile strength is only 20–30 MPa. Therefore, pure PTFE films cannot be directly applied to FCCLs, requiring design optimization to improve their CTE and tensile strength.
[0005] Designing a polytetrafluoroethylene (PTFE) dielectric material for flexible copper-clad laminates to address the shortcomings of PTFE's coefficient of thermal expansion and tensile strength, while simultaneously ensuring good flexibility, has become a pressing technical challenge in this field. Summary of the Invention
[0006] In view of this, the present invention provides a laminated fluoropolymer film that can be used in flexible copper clad laminates, comprising: fiberglass cloth and polytetrafluoroethylene layers disposed in contact on both sides of the fiberglass cloth;
[0007] The pores of the polytetrafluoroethylene layer and the fiberglass cloth contain spherical silicon.
[0008] The spherical silicon has a Dk of 3.5 or less and a Df of 0.001 or less;
[0009] The thickness ratio of the fiberglass cloth to the polytetrafluoroethylene layer is 1:3 to 9.
[0010] This invention employs a laminated structure of fiberglass cloth and a polytetrafluoroethylene (PTFE) layer containing spherical silica. By controlling the thickness ratio of the fiberglass cloth to the PTFE layer containing spherical silica to be 1:3–9, the tensile strength of the laminated fluoropolymer film can be significantly improved, increasing the material's flexibility. Simultaneously, by incorporating a low-loss spherical silica PTFE layer, the coefficient of thermal expansion (CTE) of the laminated fluoropolymer film can be substantially reduced, thus producing a laminated fluoropolymer film with a low coefficient of thermal expansion and high tensile strength. Furthermore, the low-loss spherical silica incorporated in this invention can fully utilize the low-loss characteristics of PTFE within the aforementioned thickness ratio range, thereby enhancing the overall performance of the laminated fluoropolymer film.
[0011] In a preferred embodiment of the present invention, the thickness ratio of the fiberglass cloth to the polytetrafluoroethylene layer is 1:3 to 5.
[0012] In a preferred embodiment of the present invention, the weight ratio of spherical silicon to polytetrafluoroethylene in the polytetrafluoroethylene layer is 0.4 to 2.5:1, more preferably 1 to 1.5:1.
[0013] In a preferred embodiment of the present invention, the thickness of the laminated fluorine film is 50 to 150 micrometers.
[0014] When the thickness of the laminated fluorine film is controlled within the above range, the performance requirements of thinness and flexibility of flexible copper clad laminate can be well met.
[0015] In a preferred embodiment of the present invention, the pore size of the fiberglass cloth is 50 to 200 micrometers.
[0016] By controlling the void size of the fiberglass cloth, spherical silicon can be filled and pass through the voids, further reducing the CTE of the laminated fluoropolymer film and improving its tensile strength. The voids are formed by the intersection of adjacent warp and weft threads in the same plane.
[0017] In a preferred embodiment of the present invention, the thickness of the fiberglass cloth is 10 to 20 micrometers.
[0018] In a preferred embodiment of the present invention, the fiberglass cloth has a wire diameter of 10 to 20 micrometers.
[0019] In a preferred embodiment of the present invention, the warp and weft density ratio of the fiberglass cloth is 0.5 to 1.5:1.
[0020] In a preferred embodiment of the present invention, the particle size of the spherical silicon is 0.5 to 20 micrometers, and more preferably 0.5 to 10 micrometers.
[0021] When selecting the particle size of the aforementioned spherical silicon, the spherical silicon can be better doped and filled into the voids of the fiberglass cloth, which is beneficial to further improve the performance of the multilayer fluorine film.
[0022] Furthermore, the present invention also provides a method for preparing a multilayer fluorine membrane in any of the above embodiments, comprising: coating a polytetrafluoroethylene solution containing spherical silicon onto a fiberglass cloth, and then curing and sintering it.
[0023] In a preferred embodiment of the present invention, the curing temperature is 130–170°C.
[0024] In a preferred embodiment of the present invention, the sintering temperature is 340–380°C.
[0025] As a preferred embodiment of the present invention, the method for preparing the multilayer fluorine film includes:
[0026] (1) Select spherical silicon with a particle size of 0.5 to 20 micrometers; the spherical silicon has a Dk of less than 3.5 and a Df of less than 0.001; then mix the spherical silicon with a polytetrafluoroethylene solution to obtain a blended solution; wherein the weight ratio of spherical silicon to polytetrafluoroethylene is 0.4 to 2.5:1.
[0027] (2) Design the fiberglass cloth, and control the thickness of the fiberglass cloth to be 10-20 micrometers, the wire diameter to be 10-20 micrometers, the warp and weft density ratio to be 0.5-1.5:1, and the gap size of the fiberglass cloth to be 50-200 micrometers;
[0028] (3) Coat the blending solution onto the surface of the fiberglass cloth, and control the overall thickness to be 50 to 150 micrometers; control the thickness ratio of the fiberglass cloth to the polytetrafluoroethylene layer to be 1:3 to 9.
[0029] (4) The glass fibers coated with the blend solution are cured at 130-170°C and then sintered at 340-380°C.
[0030] Preferably, curing takes 3–8 minutes;
[0031] Preferably, sintering takes 5 to 15 minutes.
[0032] During the coating process, it is important to coat the blended solution evenly on the surface of the fiberglass cloth to further enhance the performance of the laminated fluorofilm.
[0033] Furthermore, the present invention also provides a flexible copper-clad laminate containing a multilayer fluorine film as described in any of the above embodiments or containing a multilayer fluorine film prepared in any of the above embodiments.
[0034] In a preferred embodiment of the present invention, the flexible copper-clad laminate includes: the laminated fluorine film and copper foil disposed in contact with both sides of the laminated fluorine film.
[0035] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0036] The laminated fluoropolymer film provided by this invention has a low coefficient of thermal expansion and high tensile strength, overcoming the problems of poor CTE performance and structural strength of polytetrafluoroethylene film. At the same time, it solves the problems of dimensional stability and MIT (flexibility) in the trial production of the back-end FPC of fluorine FCCL, and reduces transmission loss while meeting the reliability requirements of FCCL process. Detailed Implementation
[0037] The following examples are used to illustrate the present invention, but are not intended to limit the scope of the invention.
[0038] Unless otherwise specified, all methods used in the examples were conventional or performed according to techniques or conditions described in the literature in this field, or in accordance with the product instructions. Reagents and instruments used without specified manufacturers were all conventional products that could be purchased from legitimate channels.
[0039] Example 1
[0040] This embodiment provides a multilayer fluorine film that can be used in flexible copper-clad laminates, and the specific preparation method is as follows:
[0041] (1) Select low-loss spherical silicon with a particle size D50 of 4 micrometers; the Dk of the low-loss spherical silicon is 3.5 and the Df is 0.001; mix the spherical silicon with PTFE solution to prepare a blend solution; the weight ratio of spherical silicon to PTFE is 55:45;
[0042] (2) Design the fiberglass cloth, and control the thickness of the fiberglass cloth to be 17 micrometers, the wire diameter to be 15 micrometers, the warp and weft density ratio to be 0.8:1 and the gap size of the fiberglass cloth to be 100 micrometers;
[0043] (3) The blending solution is uniformly coated on the surface of the fiberglass cloth, and the overall thickness is controlled to be 100 micrometers; the thickness ratio of the fiberglass cloth to the polytetrafluoroethylene layer is controlled to be 1:5.
[0044] (4) The glass fiber coated with the blend solution was cured at 160°C for 8 min and then sintered at 360°C for 20 min.
[0045] Tests showed that the thickness ratio of the fiberglass cloth to the polytetrafluoroethylene layer in the obtained laminated fluorofilm was 1:5; the weight ratio of spherical silicon to PTFE was 55:45.
[0046] This embodiment also provides a flexible copper-clad laminate, which is specifically prepared by bonding copper foil to both sides of the above-prepared laminated fluorine film.
[0047] Example 2
[0048] This embodiment provides a multilayer fluorine film that can be used in flexible copper-clad laminates, and the specific preparation method is as follows:
[0049] (1) Select low-loss spherical silicon with a particle size D50 of 4 micrometers; the Dk of the low-loss spherical silicon is 3.5 and the Df is 0.001; mix the spherical silicon with PTFE solution to prepare a blend solution; the weight ratio of spherical silicon to PTFE is 62:38;
[0050] (2) Design the fiberglass cloth, and control the thickness of the fiberglass cloth to be 17 micrometers, the wire diameter to be 15 micrometers, the warp and weft density ratio to be 1:1 and the gap size of the fiberglass cloth to be 100 micrometers.
[0051] (3) The blending solution is uniformly coated on the surface of the fiberglass cloth, and the overall thickness is controlled to be 100 micrometers; the thickness ratio of the fiberglass cloth to the polytetrafluoroethylene layer is controlled to be 1:5.
[0052] (4) The glass fibers coated with the blend solution were cured at 150°C for 15 min and then sintered at 360°C for 30 min.
[0053] Tests showed that the thickness ratio of the fiberglass cloth to the polytetrafluoroethylene layer in the obtained laminated fluorofilm was 1:5; the weight ratio of spherical silicon to PTFE was 62:38.
[0054] This embodiment also provides a flexible copper-clad laminate, which is specifically prepared by bonding copper foil to both sides of the above-prepared laminated fluorine film.
[0055] Example 3
[0056] This embodiment provides a multilayer fluorine film that can be used in flexible copper-clad laminates. The only difference in the preparation method compared to Embodiment 1 is that:
[0057] In step (3), the thickness ratio of the fiberglass cloth to the polytetrafluoroethylene layer is controlled to be 1:3.
[0058] Tests showed that the thickness ratio of the fiberglass cloth to the polytetrafluoroethylene layer in the obtained laminated fluorofilm was 1:3; and the weight ratio of spherical silicon to PTFE was 55:45.
[0059] This embodiment also provides a flexible copper-clad laminate, which is specifically prepared by bonding copper foil to both sides of the above-prepared laminated fluorine film.
[0060] Example 4
[0061] This embodiment provides a multilayer fluorine film that can be used in flexible copper-clad laminates. The only difference in the preparation method compared to Embodiment 1 is that:
[0062] In step (3), the thickness ratio of the fiberglass cloth and the polytetrafluoroethylene layer is controlled to be 1:9.
[0063] Tests showed that the thickness ratio of the fiberglass cloth to the polytetrafluoroethylene layer in the obtained laminated fluorofilm was 1:9; and the weight ratio of spherical silicon to PTFE was 55:45.
[0064] This embodiment also provides a flexible copper-clad laminate, which is specifically prepared by bonding copper foil to both sides of the above-prepared laminated fluorine film.
[0065] Comparative Example 1
[0066] This comparative example provides a laminated fluorine membrane. The only difference between this preparation method and Example 1 is that in step (3), the thickness ratio of the fiberglass cloth and the polytetrafluoroethylene layer is controlled to be 1:2.
[0067] Tests showed that the thickness ratio of the fiberglass cloth to the polytetrafluoroethylene layer in the obtained laminated fluorofilm was 1:2; the weight ratio of spherical silicon to PTFE was 55:45.
[0068] Comparative Example 2
[0069] This comparative example provides a laminated fluorine membrane, the only difference from Example 1 being that it does not contain fiberglass cloth.
[0070] Test case
[0071] The coefficient of thermal expansion, tensile strength, and MIT (flexural strength) of the laminated fluorine films prepared in the above embodiments and comparative examples were tested. Specifically:
[0072] Test equipment for coefficient of thermal expansion (CTE): NETZSCH TMA 402 F3.
[0073] The test method is as described in IPC-TM-650 2.4.41;
[0074] Tensile strength testing equipment: Shimadzu AGX-V,
[0075] The test method is based on IPC-TM-650 2.4.24;
[0076] The MIT (flexibility) test method is based on JIS C 6471.
[0077] The coefficient of thermal expansion (CTE), tensile strength, and MIT (flexural strength) of the laminated fluoropolymer films prepared in the examples and comparative examples are shown in Table 1.
[0078] Table 1 Performance Test Results
[0079] project Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Coefficient of thermal expansion (CTE) 13.3 10.7 12.5 18.2 8.6 50 Tensile strength (MPa) 50 50 53 48 100 8.5 MIT (Flexibility) 300 300 280 350 25 200
[0080] Therefore, the laminated fluorine film for flexible copper-clad laminates prepared by the present invention has a low coefficient of thermal expansion, high tensile strength, and high flexibility.
[0081] Although the present invention has been described in detail above with general descriptions and specific embodiments, modifications or improvements can be made to it, which will be obvious to those skilled in the art. Therefore, all such modifications or improvements made without departing from the spirit of the present invention fall within the scope of protection claimed by the present invention.
Claims
1. A laminated fluorine film which is used for a flexible copper-clad plate, characterized by, The thickness of the laminated fluorine film is 50~150 micrometers; Includes: fiberglass cloth and polytetrafluoroethylene layers disposed in contact on both sides of the fiberglass cloth; The pores of the polytetrafluoroethylene layer and the fiberglass cloth contain spherical silicon. The spherical silicon has a Dk of less than 3.5 and a Df of less than 0.001; the particle size of the spherical silicon is 0.5 to 10 micrometers. The thickness of the fiberglass cloth is 10-20 micrometers; the porosity of the fiberglass cloth is 50-200 micrometers. The thickness ratio of the fiberglass cloth to the polytetrafluoroethylene layer is 1:3~5; the weight ratio of spherical silicon to polytetrafluoroethylene in the polytetrafluoroethylene layer is 1~1.5:
1.
2. The laminated fluorine membrane according to claim 1, characterized in that, The fiberglass cloth has a diameter of 10-20 micrometers; and / or the warp-to-weft density ratio of the fiberglass cloth is 0.5-1.5:
1.
3. The method for preparing the multilayer fluorine film according to claim 1 or 2, characterized in that, include: A polytetrafluoroethylene solution containing spherical silica is coated onto fiberglass cloth, which is then cured and sintered.
4. The preparation method according to claim 3, characterized in that, The curing temperature is 130~170℃.
5. The preparation method according to claim 4, characterized in that, The sintering temperature is 340~380℃.
6. A flexible copper-clad laminate, characterized in that, It contains the laminated fluorine membrane as described in claim 1 or 2, or the laminated fluorine membrane prepared by any one of claims 3 to 5.
7. The flexible copper-clad laminate according to claim 6, characterized in that, The flexible copper-clad laminate includes: the laminated fluorine film and copper foil disposed in contact on both sides of the laminated fluorine film.
Citation Information
Patent Citations
Preparation method of microwave copper-clad plate for reducing Z-axis thermal expansion coefficient
CN106113802A