A crack-resistant solvent-free silicone-impregnated insulating resin composition and preparation method thereof

By combining modified acrylate copolymer with silicone resin, the problem of cracking of silicone resin in extreme environments is solved, the mechanical and insulation properties are improved, and it is suitable for high-temperature and high-humidity environment applications of composite materials.

CN117801522BActive Publication Date: 2024-11-01QINGYUAN BETTER NEW MATERIALS CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202311624555.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-30
Publication Date
2024-11-01
Estimated Expiration
2043-11-30

AI Technical Summary

Technical Problem

Silicone resins are prone to cracking in extreme environments, and lack mechanical properties, insulation properties and compatibility, making it difficult to meet the application needs of composite materials in high temperature and high humidity environments.

Method used

Using modified acrylic ester copolymer combined with polyaromatic or alkyl silicone resin, a solvent-resistant silicone impregnated insulating resin composition that is resistant to cracking is prepared by unsaturated acid grafting and ultrasonic heating, thereby enhancing glass fibers and acrylic acid. Ester compatibility and binding strength.

Benefits of technology

It significantly improves the mechanical properties and weather resistance of silicone resin, overcomes cracking problems in extreme environments, and improves insulation properties and interface bonding strength, and is suitable for a wide range of electrical insulation materials applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004580203310000011
    Figure BDA0004580203310000011
  • Figure BDA0004580203310000031
    Figure BDA0004580203310000031
  • Figure BDA0004580203310000041
    Figure BDA0004580203310000041
Patent Text Reader

Abstract

The present invention relates to the technical field of composite materials, and discloses a crack-resistant solvent-free silicone-impregnated insulating resin composition and a preparation method thereof. The insulating silicone resin composition comprises a silicone resin, an acrylic resin, glass fibers, and a modified acrylic ester copolymer, wherein the unsaturated acid-grafted glass fibers and polylauryl acrylate produce a synergistic effect, so that the insulation and weather resistance of the silicone resin are significantly improved. The finished product has both good insulation performance and good weather resistance, can overcome the problems of aging cracking and reduced insulation performance in extreme environments, and can be used for electrical insulation materials in harsh environments.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of composite materials, in particular to a crack-resistant solvent-free organic silicon-impregnated insulating resin composition and a preparation method thereof. Background Art

[0002] Silicone resin is a general term for a class of polymers that are formed by alternating silicon and oxygen atoms forming a skeleton, and then organic groups are linked to it. Compared with conventional organic resins, silicone resin materials have the properties of both organic and inorganic materials, and present unique physical and chemical properties, such as better thermal stability, weather resistance, insulation, etc., and are widely used in the field of electrical insulation.

[0003] However, the groups on the silicone resin can rotate freely and occupy a large space, thereby reducing the intermolecular interaction force, resulting in a low effective crosslinking density of the silicone resin and poor mechanical properties. This defect can be enhanced by compounding with other materials. The silicone resin composite material is a composite formed by combining silicone resin with other materials (such as glass fiber, carbon fiber fabric, etc.) to meet specific functions. This composite material not only has the special properties of silicone resin, but also combines the excellent properties of other materials, and can control the properties and functions of the material by adjusting the proportion and combination of each component. The working temperature of silicone resin is generally between -50℃ and 200℃, which can cover most environments, but there is still a risk of cracking and aging failure in some extreme environments. Although the composite use with other materials has broadened the application field of silicone resin, it faces problems such as mechanical properties, insulation properties, compatibility, and weather resistance that need to be improved.

[0004] In summary, there is an urgent need to develop a silicone resin-based composite material that has good insulation properties and can overcome the cracking problem in extreme environments to meet the current market needs. Summary of the invention

[0005] The purpose of the present invention is to provide a crack-resistant solvent-free silicone-impregnated insulating resin composition in view of the deficiencies of the prior art. The silicone resin composition is a composite of an acrylic ester copolymer with a specific structure and a silicone resin, and has the advantages of both, having good insulation performance and overcoming the cracking problem in extreme environments.

[0006] An object of the present invention is to provide a crack-resistant solvent-free silicone-impregnated insulating resin composition comprising the following components in parts by mass:

[0007]

[0008] Additives;

[0009] The modified acrylic ester copolymer is a polymer obtained by copolymerizing acrylic acid and glass fiber grafted with an unsaturated acid.

[0010] Furthermore, the organosilicon resin is selected from polyaromatic organosilicon resin, polyalkyl organosilicon resin, or polyaromatic-alkyl organosilicon resin.

[0011] Furthermore, the auxiliary agent is selected from one or more of a pigment, a thixotropic agent, and a defoaming agent.

[0012] Another object of the present invention is to provide a method for preparing the above-mentioned crack-resistant solvent-free silicone-impregnated insulating resin composition, which comprises the following steps:

[0013] S1. preparing modified glass fiber grafted with unsaturated acid: soaking hydroxylated glass fiber in an aqueous solution of unsaturated acid, and ultrasonically heating the glass fiber to obtain the unsaturated acid grafted glass fiber;

[0014] S2, preparing a modified acrylate copolymer: under an inert gas atmosphere, mixing unsaturated acid-grafted glass fiber and acrylate in a solvent, heating and reacting under the action of an initiator, and removing the solvent to obtain the modified acrylate copolymer;

[0015] S3. Preparing the crack-resistant solvent-free organosilicon-impregnated insulating resin composition: blending the modified acrylate copolymer with other ingredients and dispersing them to a specified fineness to obtain the crack-resistant solvent-free organosilicon-impregnated insulating resin composition.

[0016] Furthermore, the unsaturated acid is selected from one or more of oleic acid and linolenic acid.

[0017] Furthermore, the acrylic acid ester is selected from lauryl acrylate, tetradecyl acrylate, hexadecyl acrylate or octadecyl acrylate.

[0018] Furthermore, in step S1, the heating temperature is 70-80°C.

[0019] Furthermore, in step S3, the fineness is less than or equal to 80 μm.

[0020] Furthermore, in step S3, the initiator is selected from an azo initiator or a peroxide initiator.

[0021] The present invention has the following beneficial effects:

[0022] 1. The organic silicon resin composition provided by the present invention adopts organic silicon resin as a matrix and an acrylic ester copolymer containing glass fibers as a reinforcement. Part of the glass fibers are grafted with oleic acid and then free radical copolymerized with acrylic ester, so that the glass fibers and the acrylic ester part are tightly combined, so that they can be used as a compatibilizer to improve the compatibility of acrylic resin, organic silicon resin and glass fibers in the composition, so that the heat resistance and corrosion resistance of the glass fibers complement the flexibility of the acrylic ester polymer, so that the mechanical and weather resistance of the organic silicon resin are enhanced, so that the prepared organic silicon resin composition has good insulation performance and can overcome the cracking problem in extreme environments.

[0023] 2. The present invention adopts solvent-free silicone resin as the matrix. Compared with conventional solvent-containing silicone resin, it has the advantages of less pores formed by volatilization, high filling rate and small internal stress. As an electrical insulating material, it has excellent interface bonding strength and better insulation performance. DETAILED DESCRIPTION

[0024] In order to more clearly illustrate the technical solution of the present invention, the following examples are listed. Unless otherwise stated, the raw materials, reactions and post-treatment methods shown in the examples are common raw materials on the market and technical methods well known to those skilled in the art.

[0025] The words "preferred", "preferably", "more preferably", etc. in the present invention refer to embodiments of the present invention that can provide certain beneficial effects in certain circumstances. However, other embodiments may also be preferred under the same circumstances or other circumstances. In addition, the description of one or more preferred embodiments does not imply that other embodiments are not applicable, nor is it intended to exclude other embodiments from the scope of the present invention.

[0026] It should be understood that, except in any operating examples, or where otherwise indicated, all numbers indicating, for example, the amounts of ingredients used in the specification and claims should be understood to be modified in all cases by the term "about". Therefore, unless indicated to the contrary, the numerical parameters set forth in the following specification and the appended claims are approximate values ​​that vary depending on the desired properties to be obtained by the present invention.

[0027] The present invention uses the following raw materials:

[0028] Silicone resin, model SC-8-2045, purchased from Shanghai Yiyu;

[0029] Acrylic resin, model HPD671, purchased from BASF;

[0030] Glass fiber, model is 9-13μm short-cut fiber material, purchased from Taian Haoda New Materials;

[0031] The modified acrylate copolymer is self-made. It is polymerized by acrylate and glass fiber grafted with unsaturated acid.

[0032] Pigment, model is 800 mesh iron black, purchased from Jufa Technology;

[0033] Thixotropic agent, model number RHEOLATE 299, purchased from Haimingsi Fine Chemicals;

[0034] Defoaming agent, model ZHC-301, purchased from Wuxi Zhonghecheng New Materials;

[0035] The parts involved in the present invention refer to the parts by mass;

[0036] In the embodiment of the present invention, the glass fiber used for modifying the acrylic ester copolymer must be hydroxylated in advance. The treatment method is: add an excess of H2O2 aqueous solution (10wt%) to the glass fiber raw material, stir evenly, heat to 105°C, reflux for 4h, filter and dry to obtain the hydroxylated glass fiber.

[0037] Example 1

[0038] A crack-resistant solvent-free silicone-impregnated insulating resin composition comprising the following components in parts by mass:

[0039]

[0040]

[0041] The preparation method of the above-mentioned crack-resistant solvent-free silicone-impregnated insulating resin composition is as follows:

[0042] S1. Preparation of modified glass fiber grafted with unsaturated acid:

[0043] The hydroxylated glass fiber was immersed in a sufficient amount of oleic acid ethanol solution (50 wt%), ultrasonicated and heated to 70°C, and reacted for 1 hour to obtain oleic acid-grafted glass fiber;

[0044] S2. Preparation of modified acrylate copolymer:

[0045] In a reactor equipped with a condenser under nitrogen protection, oleic acid-grafted glass fiber and dodecyl acrylate (1:10, m / m) are mixed in a sufficient amount of toluene solvent, and a catalytic amount of initiator BPO is added, and the mixture is reacted at 90° C. for 1 hour, and then toluene is removed under reduced pressure to obtain the modified acrylate copolymer;

[0046] S3, preparing the crack-resistant solvent-free silicone-impregnated insulating resin composition:

[0047] The modified acrylate copolymer was blended with other ingredients according to the above mass fractions, and dispersed at a rotation speed of 1000 rpm for 1 hour until the material fineness was about 80 μm, thereby obtaining a crack-resistant solvent-free silicone-impregnated insulating resin composition.

[0048] Example 2

[0049] A crack-resistant solvent-free silicone-impregnated insulating resin composition comprising the following components in parts by mass:

[0050]

[0051] The preparation method of the above crack-resistant solvent-free silicone-impregnated insulating resin composition is the same as that of Example 1, except that the mass fraction of the above composition is changed.

[0052] Example 3

[0053] A crack-resistant solvent-free silicone-impregnated insulating resin composition comprising the following components in parts by mass:

[0054]

[0055]

[0056] The preparation method of the above crack-resistant solvent-free silicone-impregnated insulating resin composition is the same as that of Example 1, except that the mass fraction of the above composition is changed.

[0057] Comparative Example 1

[0058] The raw materials and preparation method used in Comparative Example 1 are the same as those in Example 1, with the only difference being that in S2 of Comparative Example 1, the glass fiber is physically blended with polydodecyl acrylate (1:10, m / m) and does not participate in the polymerization reaction.

[0059] The polylauryl acrylate, model number 26246-92-4, was purchased from Shanghai Zhenzhun Biotechnology.

[0060] Comparative Example 2

[0061] The raw materials and preparation method used in Comparative Example 2 are the same as those in Example 1, with the only difference being that in S3 of Comparative Example 2, no modified acrylate copolymer is added, but polylauryl acrylate in an equal mass fraction is used instead.

[0062] The polylauryl acrylate, model number 26246-92-4, was purchased from Shanghai Zhenzhun Biotechnology.

[0063] Test Case

[0064] Test method:

[0065] The composite material samples prepared in Examples 1-3 and Comparative Examples 1-2 were placed at room temperature and in an environment of 85°C / 85° humidity for 3 months, and then their performance was tested according to standards such as "GB / T 1040.5-2008 Determination of Tensile Properties of Plastics" and "GB / T31838.2-2019 Test Method for Volume Resistivity and Surface Resistivity of Solid Insulating Materials".

[0066] The test results are shown in Table 1.

[0067] Table 1 Performance test results

[0068]

[0069] According to Table 1, the mechanical properties and insulation properties of Examples 1-3 are significantly more advantageous than those of Comparative Examples 1-2. Moreover, the test results after aging at high temperature and high humidity for 3 months show that the composite silicone resin with glass fiber and acrylate copolymer added has significantly better weather resistance, and the loss of mechanical properties and insulation properties after aging is less than 5%. The test results show that the insulating silicone resin composition composed of glass fiber, acrylate copolymer, silicone resin and other materials has both good insulation properties and good weather resistance, and can overcome the problems of aging cracking and reduced insulation properties under extreme environments.

[0070] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.

[0071] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A crack-resistant solvent-free silicone-impregnated insulating resin composition, characterized in that: The crack-resistant solvent-free silicone-impregnated insulating resin composition comprises the following components in parts by mass: 30-50 parts of silicone resin Acrylic resin 10-15 parts Glass fiber 10-15 parts Modified acrylic copolymer 10-12 parts Additives; in, The modified acrylate copolymer is a polymer obtained by copolymerizing acrylate and glass fiber grafted with an unsaturated acid; The organosilicon resin is selected from polyaromatic organosilicon resin, polyalkyl organosilicon resin, or polyaromatic-alkyl organosilicon resin; The method for preparing the crack-resistant solvent-free silicone-impregnated insulating resin composition comprises the following steps: S1. preparing modified glass fiber grafted with unsaturated acid: soaking hydroxylated glass fiber in an aqueous solution of unsaturated acid, and ultrasonically heating the glass fiber to obtain the unsaturated acid grafted glass fiber; S2, preparing a modified acrylate copolymer: under an inert gas atmosphere, mixing unsaturated acid-grafted glass fiber and acrylate in a solvent, heating and reacting under the action of an initiator, and removing the solvent to obtain the modified acrylate copolymer; S3, preparing the crack-resistant solvent-free organosilicon-impregnated insulating resin composition: blending the modified acrylate copolymer with other ingredients and dispersing them to a specified fineness to obtain the crack-resistant solvent-free organosilicon-impregnated insulating resin composition; The unsaturated acid is selected from one or more of oleic acid and linolenic acid; The acrylate is selected from lauryl acrylate, tetradecyl acrylate, hexadecyl acrylate or octadecyl acrylate; The glass fibers used to modify the acrylic copolymers must be hydroxylated in advance.

2. The crack-resistant solvent-free silicone-impregnated insulating resin composition according to claim 1, characterized in that: The auxiliary agent is selected from one or more of a pigment, a thixotropic agent, and a defoaming agent.

3. The method for preparing the crack-resistant solvent-free silicone-impregnated insulating resin composition according to claim 1, characterized in that: In step S1, the heating temperature is 70-80°C.

4. The method for preparing the crack-resistant solvent-free silicone-impregnated insulating resin composition according to claim 1, characterized in that: In step S3, the fineness is less than or equal to 80 μm.

5. The method for preparing the crack-resistant solvent-free silicone-impregnated insulating resin composition according to claim 1, characterized in that: In step S3, the initiator is selected from an azo initiator or a peroxide initiator.

Citation Information

Patent Citations

  • Transformer coating and preparation method thereof

    CN109207058A

  • Super-hydrophobic super-wear-resistant anti-fog coating composition and application thereof

    CN112521851A

  • Preparation method of glass fiber reinforced polyvinyl chloride material

    CN113150330A

  • Surface treatment method of glass fiber, glass fiber surface-modified by the method, and printed circuit board using the same

    JP2014062346A