Gold and silver electroplating solution, electroplating method and product for preparing wear-resistant and oxidation-resistant coating
By using the complex and synergistic effect of hydantoin and silver ions in the gold and silver alloy plating solution, combined with alkaline operation, the problems of hydrogen cyanide poisoning and plating solution instability in the existing technology are solved, and high stability is achieved The durability and wear resistance ensure the low contact resistance and long-term performance of the coating.
Patent Information
- Application Number
- CN202410066606.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2024-01-10
- Filing Date
- 2024-01-17
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-01-17
AI Technical Summary
Existing gold and silver alloy plating solutions are operated under acidic conditions, and there is a risk of producing highly toxic hydrogen cyanide gas, and additional free cyanide ions need to be added to stabilize silver ions, resulting in instability of the plating solution and affecting the wear resistance and contact resistance of the coating. resistance.
Use cyanide-containing gold and silver electroplating solution, containing gold ions 1~30g/L, silver ions 5~200mg/L, pyrophosphate 10~120g/L and hydantoin or its derivatives, hydantoin and silver ions The molar ratio is above 2, the pH of the plating solution is 8~10, avoid adding additional free cyanide ions, improve stability through the complexation and synergy of hydantoin and silver ions, and operate under alkaline conditions.
It achieves high stability and wear resistance of the plating solution, reduces the risk of cyanide poisoning, keeps the contact resistance of the coating at a low level, and the oxidation resistance of silver is significantly higher than that of nickel or cobalt, extending the service life of the coating.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electroplating, and relates to a gold-silver electroplating solution, an electroplating method and a product for preparing a wear-resistant and oxidation-resistant coating. Background Art
[0002] Connectors or lead frame products require electroplating of hard gold to ensure the wear resistance of the coating. Generally, nickel or cobalt and gold are co-deposited. The nickel or cobalt content in the coating is 0.3~0.6wt%, and the hardness is about 160~180HV.
[0003] CN102131962A discloses a hard gold plating solution suitable for electronic components such as connectors, which contains a soluble gold salt or gold complex, a conductive salt, and a chelating agent. The soluble gold salt uses potassium cyanide as gold, cobalt sulfate as a hardener, and citric acid as a conductive salt. The pH of the plating solution is operated at 4.4, and the plating solution temperature is 60°C. As mentioned above, cobalt and gold are co-deposited during the electroplating process. Cobalt is a base metal. After long-term use, the surface will oxidize, and the contact resistance of the coating will increase, affecting the contact resistance of the coating. In addition, the operating conditions of the plating solution are acidic. As we all know, cyanide may produce highly toxic hydrogen cyanide gas under acidic conditions, which is very unfavorable for safe operation.
[0004] KR101392627B1 discloses a hard gold plating solution suitable for connectors and other electronic components, gold cyanide, organic acid conductive salt, chelating agent, iron ions (ferrous citrate, ferric citrate, ferric glycolate, ferric lactate, EDTA-ferric, ferric fumarate) and at least any one of boric acid and borate, the pH of the plating solution is operated at 3.5, and the plating temperature is 50°C. As mentioned above, iron and gold are co-deposited during the electroplating process. Iron, like cobalt, is a base metal. After long-term use, the surface will oxidize and affect the contact resistance of the coating. In addition, the operating conditions of the plating solution are also acidic. Cyanide may produce highly toxic hydrogen cyanide gas under acidic conditions, which is very unfavorable for safe operation.
[0005] GB1461474A discloses that the hardness of the gold coating is improved by co-depositing cadmium, tin, antimony or cobalt in the electroplating process using a cyanide plating solution, thereby improving the wear resistance of the coating. After electroplating, all samples were baked in an oven at 200°C, and the contact resistance of the coating was tested. It was found that all contact resistances increased after 24 hours.
[0006] Nickel or cobalt are base metals. After long-term use, the surface will oxidize, and the contact resistance of the coating will increase, affecting the contact resistance of the coating. The contact resistance parameter is crucial for connectors. In order to prevent the contact resistance of the gold coating from increasing, precious metals can be co-deposited. The resulting alloy coating is not easily oxidized when heated in the air. Among all precious metals, silver is a relatively cheap metal. Compared with nickel or cobalt, silver is a precious metal with higher oxidation resistance than nickel or cobalt. Therefore, after long-term use, the contact resistance of the coating co-deposited with gold and silver will be lower than that of gold-nickel or gold-cobalt alloy.
[0007] TWI495766B discloses the use of potassium gold cyanide and potassium silver cyanide electroplating solutions to prepare gold-silver alloys. The pH of the plating solution is 12, and the plating solution also contains a large amount of free cyanide ions, such as 50 g / L of potassium cyanide. This is because silver ions need the protection of cyanide ions to prevent them from decomposing. For semiconductor manufacturing, photoresists are used to define circuits. High pH or free cyanide ions will swell the photoresist, resulting in a decrease in circuit manufacturing accuracy.
[0008] CN101225536B discloses an electroplating solution for preparing gold-silver alloy, the electroplating solution is composed of potassium cyanide gold with a gold content of 1-30 g / L, potassium cyanide silver with a silver content of 1-200 ppm, potassium pyrophosphate of 30-100 g / L, boric acid of 20-50 g / L, and ethylenediamine or its derivatives (ethylenediaminetetraacetic acid, diethylenetriamine, triethylenetetramine, tetraethylenepentamine or pentaethylenehexamine) of 0.05-150 g / L. The technical solution uses boric acid as a pH buffer, and adjusts the concentration of the pH buffer, electrolyte components, etc. to make the pH value of the electroplating solution between 6.0 and 9.0; by adding ethylenediamine or its derivatives as additives, the current density range in which a good electroplating film can be formed is expanded. The technical solution needs to add a pH buffer, and the pH value of the electroplating solution is between 6.0 and 9.0. When it is in the acidic range, there is a risk of generating highly toxic hydrogen cyanide gas.
[0009] Gold-silver alloy electroplating solutions are divided into two categories: those containing cyanide and those not containing cyanide. Since the complex constants of gold ions, silver ions and cyanide ions are high, they are more stable than those not containing cyanide. However, silver ions are photosensitive substances. In addition to the cyanide part of potassium silver cyanide, the existing technology needs to introduce free cyanide ions into the plating solution to ensure that the silver ions will not decompose in the presence of light. Therefore, it is difficult for the industry to develop cyanide-containing gold-silver alloy electroplating technology, without adding additional cyanide ions to the plating solution, while ensuring the high stability of the plating solution. Summary of the invention
[0010] The primary purpose of the present invention is to provide a gold-silver electroplating solution for preparing a wear-resistant and anti-oxidation coating, the plating solution has extremely high stability, no additional free cyanide ions need to be added to the plating solution, and the plating solution is operated under alkaline conditions to reduce the risk of cyanide poisoning in the production process. The gold-silver alloy coating obtained by the electroplating solution has excellent wear-resistant properties. Since silver is a precious metal, its oxidation resistance is significantly higher than that of nickel or cobalt. After long-term use, the contact resistance of the coating remains at a low level, which can solve the technical problem of surface oxidation and increased contact resistance of the coating after long-term use of gold-nickel or gold-cobalt alloys. This purpose of the present invention is achieved by the following specific technical solutions.
[0011] The invention discloses a gold-silver electroplating solution for preparing a wear-resistant and anti-oxidation coating, wherein the gold-silver electroplating solution comprises a water-soluble cyanide-containing gold salt with a gold ion content of 1 to 30 g / L, a water-soluble cyanide-containing silver salt with a silver ion content of 5 to 200 mg / L, 10 to 120 g / L of pyrophosphate, hydantoin or its derivatives, wherein the molar ratio of hydantoin or its derivatives to silver ions is greater than 2, and the solvent is water.
[0012] The inventors have found through extensive research that in the gold and silver electroplating solution, hydantoin or its derivatives, on the one hand, act as silver ion stabilizers, complex with silver ions to prevent silver ion photoreduction, and improve the stability of the electroplating solution; in order to ensure coordination and complexation with silver ions, the molar ratio of hydantoin or its derivatives to silver ions must be above 2. On the other hand, in addition to the complexation with silver ions, hydantoin or its derivatives may have a synergistic effect with silver ions to achieve the effect of a crystallization regulator. A separate silver or gold plating solution requires the addition of a crystallization regulator, but in the present invention, a very smooth coating can be obtained without the use of a crystallization regulator.
[0013] Furthermore, the pH of the gold-silver electroplating solution is 8 to 10. The pH value can be adjusted by conventional acid or alkali in the art. Within this pH value range, the obtained gold-silver electroplating solution has good stability and can obtain a gold-silver electroplated layer with excellent performance. When the pH of the plating solution is lower than 8, the complexing ability of hydantoin or its derivatives and silver ions will decrease, and the stability of the plating solution will decrease. When the pH of the plating solution is higher than 10, the coating will become dark.
[0014] Furthermore, the water-soluble cyanide-containing gold salt is preferably potassium cyanide gold (also known as potassium gold cyanide, CAS number: 13967-50-5); the water-soluble cyanide-containing silver salt is preferably potassium silver cyanide (also known as potassium silver cyanide, CAS number: 506-61-6). The concentration of gold ions is 1-30 g / L. When it is less than 1 g / L, the coating is easily burned during electroplating. When it exceeds 30 g / L, the cost is affected due to the effect of carryover. The concentration of silver ions is 5-200 mg / L. According to different scene requirements, the ratio of gold and silver in the coating can be adjusted by adjusting the concentration of silver ions in the plating solution.
[0015] Furthermore, the hydantoin derivative is 5, 5-dimethylhydantoin (CAS No.: 77-71-4), 1,3-dihydroxymethyl-5, 5-dimethylhydantoin (CAS No.: 6440-58-0) or 1-aminohydantoin (CAS No.: 957509-31-8), preferably 5, 5-dimethylhydantoin.
[0016] The pyrophosphate as a conductive salt can be sodium pyrophosphate, potassium pyrophosphate or ammonium pyrophosphate, preferably potassium pyrophosphate, and its concentration range is 10-120 g / L. Pyrophosphate can improve the conductivity of the plating solution, but too high a concentration will lead to a high viscosity of the plating solution, which will affect the electroplating uniformity of the coating.
[0017] Another object of the present invention is to provide an electroplating method using the above electroplating solution, wherein the electroplating operation temperature is 20-60°C and the electroplating current density is 10-100A / dm 2 (ASD).
[0018] The operating temperature of electroplating is between 20 and 60°C. Below 20°C, the temperature is not easy to control and the uniformity of electroplating deteriorates. Above 60°C, the roughness of the coating tends to increase. At the same time, the volatilization of the electroplating solution causes the concentration of components in the plating solution to change, making it difficult to maintain the electroplating solution.
[0019] The current density of electroplating is 10~100A / dm 2 Within this range, a good plating layer can be formed by properly adjusting the pH, temperature, and gold ion or silver ion concentration of the plating solution.
[0020] Another object of the present invention is to provide a gold-silver alloy coating obtained by the above-mentioned gold-silver electroplating solution, wherein the silver content of the gold-silver alloy coating is 0.2-2.0wt%. A further object of the present invention is to provide a gold-silver alloy coating obtained by the above-mentioned electroplating method, wherein the silver content of the gold-silver alloy coating is 0.2-2.0wt%.
[0021] Furthermore, the thickness of the gold-silver alloy plating layer is 0.05-1.0 μm.
[0022] Furthermore, the hardness of the gold-silver alloy coating is 160-200 HV, and the contact resistance is 15-25 mΩ (milliohms).
[0023] An electrical device having an electrical contact, on which the gold-silver alloy plating layer is provided.
[0024] Furthermore, the electrical device is a connector or a lead frame.
[0025] The present invention has the following beneficial technical effects: the gold-silver electroplating solution provided by the present invention has extremely high stability, and no additional free cyanide ions need to be added to the plating solution; the plating solution is operated under alkaline conditions to reduce the risk of cyanide poisoning in the production process; and a very smooth plating layer can be obtained without using a crystallization regulator. The gold-silver alloy plating layer obtained by the gold-silver electroplating solution of the present invention has excellent wear resistance and oxidation resistance significantly higher than that of nickel or cobalt. After long-term use, the contact resistance of the plating layer remains at a low level, thereby improving the performance of electrical equipment such as connectors or lead frames after long-term use. DETAILED DESCRIPTION
[0026] The technical solution of the present invention is described clearly and completely below. Obviously, the described implementation is only a part of the implementation of the present invention, not all of the implementation. Based on the implementation of the present invention, all other implementations obtained by ordinary technicians in this field without creative work are within the protection scope of the present invention.
[0027] Prepare the electroplated gold-silver alloy coating sample:
[0028] S1 used a brass sample (20 mm × 30 mm) with a thickness of 0.3 mm, electrolytically degreased, then immersed in a 10% sulfuric acid aqueous solution for 1 minute for activation, and then thoroughly washed with deionized water.
[0029] S2 nickel-plated the sample. The nickel plating solution contained nickel sulfamate with a nickel content of 80 g / L, 3.5 g / L chloride ions, 40 g / L boric acid, and appropriate amounts of brightener and wetting agent. The pH of the plating solution was 4.0 and the temperature was 55°C. The current density was 5 ASD, the electroplating time was 3 min, and the thickness of the nickel coating was 3 μm.
[0030] Then the gold-silver alloy was electroplated according to the following example. Example 1
[0031] First, add 600mL of deionized water to a 1L beaker, then add 60g of potassium pyrophosphate and 1g of hydantoin to fully dissolve, then add 15g of potassium cyanide gold with gold ion content and 0.1g of potassium cyanide silver with silver ion content, the molar ratio of hydantoin to anion is 10.8, adjust the pH of the plating solution to 9, add deionized water to make the volume of the plating solution 1000mL. The plating solution is stable after 24 hours.
[0032] The prepared sample was placed in the electroplating solution, the electroplating temperature was set to 50°C, the current density was 50ASD, and the thickness of the coating was 0.5μm. The coating was light golden yellow with uniform color and a silver content of 1.0wt%. Example 2
[0033] Compared with Example 1, the difference is that the gold ion concentration of 15g / L is changed to 30g / L, the silver ion concentration of 0.1g / L is changed to 0.2g / L, the molar ratio of hydantoin to anion is 5.4, the plating solution pH is changed to 10, the current density of 50ASD is changed to 100ASD, the thickness of the coating is 1.0μm, and other conditions are the same. The plating solution is stable after being placed for 24h; the coating is light golden yellow, uniform in color, and has a silver content of 1.3wt%. Example 3
[0034] Compared with Example 1, the difference is that the gold ion concentration of 15g / L is changed to 1g / L, the silver ion concentration of 0.1g / L is changed to 0.05g / L, the molar ratio of hydantoin to anion is 21.6, the potassium pyrophosphate concentration of 60g / L is changed to 10g / L, the current density of 50ASD is changed to 10ASD, the thickness of the coating is 0.05μm, and other conditions are the same. The plating solution is stable after being placed for 24h; the coating is light golden yellow, uniform in color, and has a silver content of 0.8wt%. Example 4
[0035] Compared with Example 1, the difference is that the potassium pyrophosphate concentration of 60g / L is changed to 120g / L, the silver ion concentration of 0.1g / L is changed to 0.2g / L, hydantoin 1g / L is changed to 5, 5-dimethylhydantoin 0.048g / L, the molar ratio of 5, 5-dimethylhydantoin to anion is 2, the plating solution pH is changed to 8, the thickness of the coating is 0.05μm, and other conditions are the same. The plating solution is stable after being placed for 24h; the coating is light golden yellow, uniform in color, and has a silver content of 1.5wt%.
[0036] Comparative Example 1
[0037] Compared with Example 1, the difference is that 1g / L hydantoin is changed to 0g / L (i.e. no hydantoin is added). The coating is light golden yellow with uniform color; but after the plating solution is left for 24 hours, a metal film is formed on the surface of the plating solution, which comes from the light reduction of silver.
[0038] From Examples 1-4, it can be concluded that, since hydantoin or its derivatives are added to the plating solution, no silver film is formed on the surface of the plating solution after the plating solution is placed for 24 hours, that is, the stability problem of the plating solution is solved. On the contrary, it can be seen from Comparative Example 1 that when hydantoin is not added, although the appearance of the electroplated coating meets the requirements, the silver ions in the plating solution will decompose after long-term placement. Example 5
[0039] Contact resistance test: The contact resistance was tested using the coatings prepared in Examples 1-4. The results are shown in Table 1. The loading load was 10 g, and the test conditions were that the sample was untreated and oxidized at 280° C. for 5 min in an atmospheric environment.
[0040] Table 1 Test results of coating contact resistance, unit: mΩ
[0041]
[0042] The results show that there is no significant change in the contact resistance of the sample after high-temperature oxidation and that of the untreated sample, which is attributed to the good anti-oxidation ability of silver itself.
[0043] Test of coating hardness: The plating solution of Example 1-4 was also used, the electroplating temperature was set to 40°C, the current density was set to 50ASD, and the coating thickness was controlled at 10μm. The hardness of the coating was tested using a hardness tester (Mitutoyo, HM-200). The test results of the hardness of the coating are shown in Table 2.
[0044] Table 2 Coating hardness test results, unit HV
[0045]
[0046] The above results show that the gold-silver alloy coating obtained by the present invention has a hardness equivalent to that of a connector made of a gold-nickel alloy or a gold-cobalt alloy, indicating that the gold-silver coating has good wear resistance.
[0047] Although the embodiments of the present invention have been shown and described above, it is understood that the above embodiments are exemplary and cannot be understood as limiting the present invention. A person skilled in the art may change, modify, replace and modify the above embodiments within the scope of the present invention without departing from the principles and purpose of the present invention. The protection scope of the present invention is defined by the claims and their equivalent technical solutions.
Claims
1. A gold and silver electroplating solution for preparing a wear-resistant and anti-oxidation coating, characterized in that: The gold-silver electroplating solution is composed of the following components: a water-soluble cyanide-containing gold salt with a gold ion content of 1 to 30 g / L, a water-soluble cyanide-containing silver salt with a silver ion content of 5 to 200 mg / L, 10 to 120 g / L of pyrophosphate, hydantoin or its derivatives, the molar ratio of hydantoin or its derivatives to silver ions being greater than 2, water as a solvent, and an acid or base for adjusting the pH value; the gold-silver electroplating solution does not use a crystallization regulator, and the pH value of the gold-silver electroplating solution is 8 to 10.
2. The gold-silver electroplating solution according to claim 1, characterized in that: The water-soluble cyanide-containing gold salt is potassium aurous cyanide, and the water-soluble cyanide-containing silver salt is potassium silver cyanide.
3. The gold-silver electroplating solution according to claim 1, characterized in that: The hydantoin derivative is 5,5-dimethylhydantoin, 1,3-dihydroxymethyl-5,5-dimethylhydantoin or 1-aminohydantoin.
4. The gold-silver electroplating solution according to claim 3, characterized in that: The derivative of hydantoin is 5,5-dimethylhydantoin.
5. The gold-silver electroplating solution according to claim 1, characterized in that: The pyrophosphate is sodium pyrophosphate, potassium pyrophosphate or ammonium pyrophosphate.
6. The gold-silver electroplating solution according to claim 5, characterized in that: The pyrophosphate is potassium pyrophosphate.
7. An electroplating method, characterized in that: The gold and silver electroplating solution according to any one of claims 1 to 6 is used for electroplating, the operating temperature of the electroplating is 20-60° C., and the current density of the electroplating is 10-100 A / dm 2 .
8. A gold-silver alloy plating layer, characterized in that: Obtained from the gold-silver electroplating solution according to any one of claims 1 to 6, the silver content in the gold-silver alloy plating layer is 0.2-2.0wt%.
9. A gold-silver alloy plating layer, characterized in that: Obtained by the electroplating method according to claim 7, the silver content in the gold-silver alloy plating layer is 0.2-2.0wt%.
10. The gold-silver alloy plating layer according to claim 8 or 9, characterized in that: The thickness of the gold-silver alloy plating layer is 0.05-1.0 μm.
11. The gold-silver alloy plating layer according to claim 8 or 9, characterized in that: The hardness of the gold-silver alloy plating layer is 160-200 HV, and the contact resistance is 15-25 mΩ.
12. An electrical device having an electrical contact, characterized in that: The electrical contact has a gold-silver alloy plating layer as claimed in any one of claims 8 to 11.
13. The electrical device according to claim 12, characterized in that: The electrical device is a connector or a lead frame.
Citation Information
Patent Citations
Gold-silver alloy electroplating solution
CN101225536B
Hard gold plating solution
CN102131962A
Electrical connectors and a method of preparing stable electro platings
GB1461474A
Electrolytic hard gold plating solution, plating method, and method for manufacturing gold-iron alloy coating
KR101392627B1
Gold-silver alloy electroplating solution
CN101225536A