Solar cell and method for manufacturing the same

By using aluminum-doped zinc oxide materials instead of traditional aluminum oxide materials, the passivation layer of solar cells is prepared by atomic layer deposition method, which solves the problems of laser damage and high-temperature sintering, and improves the conductivity and transmittance of the cells. Reduced production costs and conform to the trend of low-temperature preparation.

CN117810273BActive Publication Date: 2024-12-03TRINA SOLAR CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202311862844.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-29
Publication Date
2024-12-03
Estimated Expiration
2043-12-29

AI Technical Summary

Technical Problem

Traditional aluminum oxide materials are used in the preparation process of solar cell passivation layers, and laser grooves or high-temperature sintering is required, resulting in serious damage to the silicon wafer, increasing the cost of battery manufacturing and not meeting the needs of low-temperature cost reduction.

Method used

Aluminum-doped zinc oxide material is used to prepare a passivation layer by atomic layer deposition method to avoid laser damage, improve conductivity and transmittance, reduce production costs, and conform to the trend of low-temperature preparation.

Benefits of technology

It effectively avoids damage to silicon wafers by laser, improves the conductivity and transmittance of solar cells, reduces production costs, and conforms to the industry trend of low-temperature preparation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117810273B_ABST
    Figure CN117810273B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of preparation of a passivation layer of a solar cell, and provides a solar cell and a preparation method thereof, wherein the solar cell comprises: a substrate; a first dielectric film, stacked on one side of the substrate; at least one first thin film, stacked on the side of the first dielectric film away from the substrate, the material of the first thin film being at least zinc oxide; at least one second thin film, stacked on the side of the first dielectric film away from the substrate, the second thin film comprising a main material and a doping material, the main material being at least zinc oxide, the doping material being at least aluminum, and the doping material being used to improve the conductivity and transmittance of the passivation layer; a second dielectric film, stacked on the side of the first dielectric film away from the substrate, and the first thin film and the second thin film being located between the first dielectric film and the second dielectric film. The present invention uses aluminum-doped zinc oxide to prepare a passivation layer, thereby avoiding damage to a silicon wafer caused by a laser, improving the conductivity and transmittance of the battery, and reducing production costs.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of preparation of a passivation layer of a solar cell, and in particular to a solar cell and a preparation method thereof. Background Art

[0002] As the whole society pays more and more attention to environmental issues, solar cells, as a device that can directly convert solar energy into electrical energy, are getting more and more attention. Solar cells are a type of photoelectric semiconductor sheet that uses sunlight to generate electricity directly. They are devices that directly convert light energy into electrical energy through the photoelectric effect or photochemical effect.

[0003] The passivation layer in solar cells is usually located on the surface or interface of solar cells. Its main function is to improve the performance of the cell, reduce the recombination of electron-hole pairs, and improve the efficiency of charge transfer. Before printing metal paste on the passivation layer of traditional aluminum oxide materials, a laser needs to be used to make grooves in the printing area so that the metal paste can contact and conduct with the underlying doped layer, or a burn-through metal paste can be used to burn through the passivation layer of the aluminum oxide material through a high-temperature sintering process, and then contact and conduct with the underlying doped layer. Both methods cause great damage to the silicon wafer, affecting the performance of the cell. In addition, the price of laser is relatively high, which increases the cost of battery manufacturing and is not in line with the current development of low-temperature cost reduction routes.

[0004] It should be noted that the information disclosed in the above background technology section is only used to enhance the understanding of the background of the present invention, and therefore may include information that does not constitute the prior art known to ordinary technicians in the field. Summary of the invention

[0005] In view of this, the present invention provides a perovskite solar cell and a preparation method thereof, so as to at least solve the above-mentioned technical problems.

[0006] One aspect of the present invention provides a solar cell, comprising:

[0007] substrate;

[0008] A first dielectric film is stacked on one side of the substrate;

[0009] At least one first film, stacked on a side of the first dielectric film away from the substrate, wherein the material of the first film is at least zinc oxide;

[0010] at least one second film, stacked on a side of the first dielectric film away from the substrate, the second film comprising a main material and a doping material, the main material is at least zinc oxide, the doping material is at least aluminum, and the doping material is used to improve the conductivity and transmittance of the passivation layer; and

[0011] The second dielectric film is stacked on a side of the first dielectric film away from the substrate, and the first thin film and the second thin film are located between the first dielectric film and the second dielectric film.

[0012] In some embodiments, the doping material of the second film is at least a combination of one or more of aluminum, gallium, indium, titanium, and fluorine.

[0013] In some embodiments, both the first thin film and the second thin film are prepared by an atomic layer deposition method.

[0014] In some embodiments, the thickness of the first thin film is 0.2-100 nm, and the thickness of the second thin film is 0.1-50 nm.

[0015] In some embodiments, the aluminum content in the first film and the second film is 0.5% to 50%.

[0016] In some embodiments, the first thin films and the second thin films are alternately stacked between the first dielectric film and the second dielectric film.

[0017] In some embodiments, the first dielectric film and the second dielectric film are both made of SiO2, Si3N4, SiO x N y or AlO x One or more compositions, with a thickness of 0.1 to 1000 nm.

[0018] In some embodiments, the thickness of the first dielectric film is 0.2-100 nm, and the thickness of the second dielectric film is 0.1-200 nm.

[0019] In some embodiments, the first dielectric film and the second dielectric film are deposited by one or more methods selected from the group consisting of low-pressure vapor deposition, atmospheric pressure vapor deposition, plasma-enhanced chemical vapor deposition, atomic layer deposition, and magnetron sputtering.

[0020] In some embodiments, the substrate is a single crystal silicon wafer.

[0021] Another aspect of the present invention provides a method for preparing a solar cell, which is used to prepare the above-mentioned solar cell, comprising the following steps:

[0022] providing a substrate;

[0023] preparing a first dielectric film on one side of the substrate;

[0024] Preparing at least one first thin film on a side of the first dielectric film away from the substrate, wherein the material of the first thin film is at least zinc oxide;

[0025] preparing at least one second film on a side of the first dielectric film away from the substrate, the second film comprising a main material and a doping material, the main material being at least zinc oxide, the doping material being at least aluminum, and the doping material being used to improve the conductivity and transmittance of the passivation layer; and

[0026] A second dielectric film is formed on a side of the first dielectric film facing away from the substrate, and the first thin film and the second thin film are located between the first dielectric film and the second dielectric film.

[0027] In some embodiments, the step of preparing at least one first thin film on a side of the first dielectric film facing away from the substrate comprises:

[0028] Purge the gas residue in the atomic layer deposition chamber with nitrogen;

[0029] introducing a zinc-containing compound and controlling the deposition temperature within a preset temperature range to prepare the first thin film; and

[0030] When the thickness of the first film reaches a preset thickness range, the deposition is stopped.

[0031] In some embodiments, the step of preparing at least one second thin film on a side of the first dielectric film facing away from the substrate comprises:

[0032] Purge the gas residue in the atomic layer deposition chamber with nitrogen;

[0033] introducing an aluminum-containing compound and controlling the deposition temperature within a preset temperature range to prepare the second thin film; and

[0034] When the thickness of the second film reaches a preset thickness range, the deposition is stopped.

[0035] The beneficial effects of the present invention compared with the prior art include at least:

[0036] The solar cell and preparation method thereof of the present invention, by using aluminum-doped zinc oxide material instead of traditional aluminum oxide material to prepare the passivation layer, can avoid laser damage to silicon wafers, improve the conductivity and transmittance of the battery, reduce production costs, and comply with the industry trend of low-temperature preparation.

[0037] It is to be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] The accompanying drawings herein are incorporated into and constitute a part of the specification, illustrate embodiments consistent with the present invention, and together with the specification are used to explain the principles of the present invention. Obviously, the accompanying drawings described below are only some embodiments of the present invention, and for those of ordinary skill in the art, other accompanying drawings can be obtained based on these accompanying drawings without creative work.

[0039] Figure 1 A schematic diagram showing a hierarchical structure of a solar cell of the present invention;

[0040] Figure 2 Another schematic diagram of the hierarchical structure of the solar cell of the present invention is shown;

[0041] Figure 3 A flow chart showing a method for preparing a solar cell according to the present invention.

[0042] Reference numerals:

[0043] 10. Solar Cells

[0044] 11 Substrate

[0045] 12. First dielectric film

[0046] 13 First Film

[0047] 14 Second Film

[0048] 15. Second dielectric film DETAILED DESCRIPTION

[0049] In order to make the above-mentioned objects, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are described in detail below with reference to the accompanying drawings.

[0050] In the following description, many specific details are set forth to facilitate a full understanding of the present application, but the present application may also be implemented in other ways different from those described herein, and therefore the present application is not limited to the specific embodiments disclosed below.

[0051] As shown in this application and claims, unless the context clearly indicates an exception, the words "a", "an", "an" and / or "the" do not refer to the singular and may also include the plural. Generally speaking, the terms "include" and "comprise" only indicate the inclusion of the steps and elements that have been clearly identified, and these steps and elements do not constitute an exclusive list. The method or device may also include other steps or elements.

[0052] In addition, it should be noted that the use of words such as "first" and "second" to define components is only for the convenience of distinguishing the corresponding components. If not otherwise stated, the above words have no special meaning and cannot be understood as limiting the scope of protection of this application. In addition, although the terms used in this application are selected from well-known and commonly used terms, some terms mentioned in the specification of this application may be selected by the applicant at his or her discretion, and their detailed meanings are explained in the relevant parts of the description of this article. In addition, it is required to understand this application not only by the actual terms used, but also by the meaning implied by each term.

[0053] Flowcharts are used in the present application to illustrate the operations performed by the system according to the embodiments of the present application. It should be understood that the preceding or following operations are not necessarily performed accurately in order. On the contrary, various steps may be processed in reverse order or simultaneously. At the same time, other operations may be added to these processes, or one or more operations may be removed from these processes.

[0054] The inventor of this case has provided a solution to the problems existing in the prior art through careful and in-depth research. Figure 1 A schematic diagram showing a hierarchical structure of a solar cell of the present invention;

[0055] Figure 3 Flow chart showing the method for preparing a solar cell of the present invention. Figure 1 and 3 As shown, the present invention discloses a solar cell and a method for preparing the same, wherein the solar cell comprises: a substrate 11, a first dielectric film 12, at least one first thin film 13, at least one second thin film 14 and a second dielectric film 15. The first dielectric film 12 is stacked on one side of the substrate 11. The first thin film 13 is stacked on the side of the first dielectric film 12 away from the substrate 11, and the material of the first thin film 13 is at least zinc oxide. The second thin film 14 is stacked on the side of the first dielectric film 12 away from the substrate 11, and the second thin film 14 comprises a main material and a doping material, the main material is at least zinc oxide, and the doping material is at least aluminum, and the doping material is used to improve the conductivity and transmittance of the passivation layer. The second dielectric film 15 is stacked on the side of the first dielectric film 12 away from the substrate 11, and the first thin film 13 and the second thin film 14 are located between the first dielectric film 12 and the second dielectric film 15. The solar cell and preparation method thereof of the present invention, by using aluminum-doped zinc oxide material instead of traditional aluminum oxide material to prepare the passivation layer, can avoid laser damage to silicon wafers, improve the conductivity and transmittance of the battery, reduce production costs, and comply with the industry trend of low-temperature preparation.

[0056] The solar cell and the method for preparing the same according to the present invention are described below with reference to the accompanying drawings and through specific embodiments.

[0057] One aspect of the present invention provides a solar cell, such as Figure 1 As shown, the hierarchical structure of the solar cell 10 is, from bottom to top, a substrate 11 , a first dielectric film 12 , at least one first thin film 13 , at least one second thin film 14 and a second dielectric film 15 .

[0058] In some embodiments, the substrate 11 is a single crystal silicon wafer. The single crystal silicon wafer has a high crystal quality, which helps to improve the performance of the solar cell 10. The substrate 11 can also be selected from a polycrystalline silicon wafer, a non-silicon material, a transparent substrate or an organic material. The choice of the substrate 11 depends on the design, performance requirements and application scenarios of the solar cell 10. Different types of substrate materials have their own characteristics and advantages, so materials suitable for specific purposes will be selected in the manufacture of the solar cell 10.

[0059] The dielectric film of the passivation layer of the solar cell 10 is usually a thin film material used to improve the performance of the cell, reduce the recombination of electron-hole pairs, and improve the efficiency of the cell. These films are usually made of insulating or semiconductor materials. In some embodiments, the first dielectric film 12 and the second dielectric film 15 are both made of SiO2, Si3N4, SiO x N y or AlO x One or more of the compositions, the thickness of each of them is 0.1 to 1000 nm. In some preferred embodiments, the thickness of the first dielectric film 12 is 0.2 to 100 nm, and the thickness of the second dielectric film 15 is 0.1 to 200 nm. In addition, the first dielectric film 12 and the second dielectric film 15 are deposited and prepared by one or more methods of low pressure vapor deposition (LPCVD), atmospheric pressure vapor deposition (APCVD), plasma enhanced chemical vapor deposition (PECVD), atomic layer deposition (ALD) or magnetron sputtering, but not limited thereto. Different methods have different advantages and limitations, and the specific selection may depend on the process control, cost, production efficiency and performance requirements of the solar cell 10.

[0060] In some embodiments, the solar cell 10 includes at least one first film 13 and at least one second film 14. Preferably, the transparent conductive film includes a plurality of first films 13 and a plurality of second films 14. The first films 13 and the second films 14 may be arranged from bottom to top in any order. Preferably, a plurality of first films 13 and a plurality of second films 14 are alternately stacked between the first dielectric film 12 and the second dielectric film 15. Figure 2 Another schematic diagram of the hierarchical structure of the solar cell of the present invention is shown. In some preferred embodiments, Figure 2As shown, the transparent conductive film includes three layers of first films 13 and two layers of second films 14. In addition, the hierarchical structure of the solar cell 10 is, from bottom to top, a substrate 11, a first dielectric film 12, a first film 13, a second film 14, a first film 13, a second film 14, a first film 13, and a second dielectric film 15.

[0061] In some embodiments, the material of the first film 13 may be zinc oxide. Preferably, the first film 13 is a zinc oxide film, which is prepared by an atomic layer deposition (ALD) method, with a deposition temperature of 100 to 500° C. and a thickness of 0.2 to 100 nm. Optionally, the zinc oxide film is prepared by a zinc-containing compound, which may include one or more combinations of zinc halides, zinc alkyl compounds, zinc alkoxy compounds, and zinc-containing inorganic salts. Specifically, the zinc oxide film may be prepared by diethyl zinc.

[0062] In some embodiments, the second film 14 comprises a main material and a doping material, the main material may be zinc oxide, the doping material may be aluminum, and the doping material is used to improve the conductivity and transmittance of the passivation layer. The doping material of the second film 14 may also be a combination of one or more of aluminum, gallium, indium, titanium, and fluorine. Preferably, the second film 14 may be aluminum-doped zinc oxide (AZO), that is, the main material is zinc oxide and the doping material is aluminum. Optionally, aluminum-doped zinc oxide is prepared by an aluminum-containing compound, and the aluminum-containing compound may include one or more combinations of aluminum halides, aluminum alkyl compounds, aluminum alkoxy compounds, and aluminum-containing inorganic salts. In addition, the second film 14 can be prepared by an atomic layer deposition (ALD) method, with a deposition temperature of 100 to 500°C and a thickness of 0.1 to 50 nm.

[0063] In some embodiments, the Al content in the first film 13 and the second film 14 is 0.5% to 50%, that is, no matter how many layers there are in the solar cell 10, the aluminum content in the first film 13 and the second film 14 is guaranteed to be within the above range, so as to at least improve the conversion efficiency of the solar cell.

[0064] In a specific embodiment of the solar cell 10 of the present invention, reference Figure 2 As shown, the hierarchical structure of the passivation layer in the solar cell 10 from bottom to top is:

[0065] The first dielectric film 12 is made of SiO2 and is deposited by LPCVD with a thickness of 0.2-100 nm.

[0066] The second first film 13 is made of ZnO and is deposited by ALD with a thickness of 0.2-100 nm.

[0067] The third second film 14 is made of aluminum-doped zinc oxide (AZO) and is deposited by ALD with a thickness of 0.1 to 50 nm.

[0068] The fourth first film 13 is made of ZnO and is deposited by ALD with a thickness of 0.2-100 nm.

[0069] The fifth second film 14 is made of aluminum-doped zinc oxide (AZO) and is deposited by ALD with a thickness of 0.1 to 50 nm.

[0070] The sixth first film 13 is made of ZnO and is deposited by ALD with a thickness of 0.2-100 nm.

[0071] The seventh second dielectric film 15 is made of SiO2 and is deposited by LPCVD, with a thickness of 0.2-100 nm.

[0072] The solar cell 10 of the present invention uses aluminum-doped zinc oxide material instead of traditional aluminum oxide material to prepare the passivation layer, which can avoid laser damage to silicon wafers, improve the conductivity and transmittance of the battery, reduce production costs, and comply with the industry trend of low-temperature preparation.

[0073] Another aspect of the present invention provides a method for preparing a solar cell, which is used to prepare the above-mentioned solar cell 10, such as Figure 3 As shown, the following steps are included:

[0074] S110, providing a substrate 11;

[0075] S120, preparing a first dielectric film 12 on one side of the substrate 11;

[0076] S130, preparing at least one first thin film 13 on a side of the first dielectric film 12 facing away from the substrate 11, wherein the material of the first thin film 13 is at least zinc oxide;

[0077] S140, preparing at least one second film 14 on the side of the first dielectric film 12 facing away from the substrate 11, the second film 14 comprising a main material and a doping material, the main material is at least zinc oxide, the doping material is at least aluminum, and the doping material is used to improve the conductivity and transmittance of the passivation layer; and

[0078] S150 , preparing a second dielectric film 15 on a side of the first dielectric film 12 facing away from the substrate 11 , and the first thin film 13 and the second thin film 14 are located between the first dielectric film 12 and the second dielectric film 15 .

[0079] It is worth noting that S110 to S150 are merely step numbers, which are used to facilitate reference and avoid text duplication, rather than to limit the order of implementation of the steps of the method. In other embodiments, the above steps of the method can also be written in an interchangeable order, and are not limited thereto. The subsequent step numbers in the present invention all have the same meaning, and the repeated parts will not be repeated.

[0080] In the first embodiment of the method for preparing a solar cell of the present invention, the specific steps of the method for preparing a solar cell are as follows:

[0081] Step S110: providing a substrate 11, including:

[0082] A substrate 11 made of a single crystal silicon wafer is provided and cleaned by an RCA standard cleaning method.

[0083] S120, preparing a first dielectric film 12 on one side of the substrate 11;

[0084] Choose SiO2, Si3N4, SiO x N y or AlO x The first dielectric film 12 is deposited at a low temperature using one or more materials of the composition described above using an LPCVD method. Preferably, the deposition temperature is 350-1000° C., and the thickness of the first dielectric film 12 is 0.2-100 nm.

[0085] Step S130: preparing at least one first thin film 13 on the side of the first dielectric film 12 facing away from the substrate 11, specifically comprising the following steps:

[0086] S131, placing the sample in step S120 in an atomic layer deposition (ALD) chamber, and then vacuuming;

[0087] S132, introducing a zinc-containing compound and controlling the deposition temperature within a preset temperature range to prepare a first film 13 made of zinc oxide (ZnO), wherein the zinc-containing compound includes one or more combinations of zinc halides, zinc alkyl compounds, zinc alkoxy compounds, and zinc-containing inorganic salts, and the preset temperature range is 100-500° C.; and

[0088] S133 , when the thickness of the first film 13 reaches a preset thickness range, the deposition is stopped, wherein the preset thickness range is 0.2 to 100 nm.

[0089] Step S140: preparing at least one second film 14 on the side of the first dielectric film 12 facing away from the substrate 11, specifically comprising the following steps:

[0090] S131, purging gas residue in the ALD chamber with nitrogen;

[0091] S132, introducing an aluminum-containing compound and controlling the deposition temperature within a preset temperature range to prepare a second film 14 made of aluminum-doped zinc oxide (AZO), wherein the aluminum-containing compound includes one or more combinations of aluminum halides, aluminum alkyl compounds, aluminum alkoxy compounds, and aluminum-containing inorganic salts, and the preset temperature range is 100-500° C.; and

[0092] S133 , when the thickness of the second film 14 reaches a preset thickness range, stop the deposition, wherein the preset thickness range is 0.1 to 50 nm.

[0093] Afterwards, the above steps S130, S140 and S130 are repeated in sequence to continue preparing the first film 13, the second film 14 and the first film 13 to form a structure in which three layers of the first film 13 and two layers of the second film 14 are alternately stacked. In the subsequent step of preparing the first film 13, it is not necessary to evacuate the ALD chamber, but it is necessary to purge the gas residue in the ALD chamber with nitrogen.

[0094] Step S150: preparing a second dielectric film 15 on the side of the first dielectric film 12 facing away from the substrate 11, and the first thin film 13 and the second thin film 14 are located between the first dielectric film 12 and the second dielectric film 15, specifically comprising the following steps:

[0095] After the first film 13 and the second film 14 are prepared, the second dielectric film 15 is deposited on the sample by ALD or PECVD, with a deposition temperature of 100 to 500° C. and a thickness of 0.1 to 200 nm.

[0096] In addition, the method for preparing a solar cell of the present invention further comprises the following steps:

[0097] S160, placing the sample of step S150 on a heating table, an annealing table, a chain sintering furnace or a track sintering furnace, and sintering at high temperature. Preferably, the sintering temperature is 100-1000°C.

[0098] In the second embodiment of the method for preparing a solar cell of the present invention, the specific steps of the method for preparing a solar cell are as follows:

[0099] S210, selecting a single crystal silicon wafer as the substrate 11, pre-polishing it with a sodium hydroxide alkaline solution, and cleaning it with an RCA standard cleaning method;

[0100] S220, using an LPCVD method, at a temperature of 500° C. and a pressure of 0.3 torr, depositing a first dielectric film 12, preferably, the thickness of the first dielectric film 12 is 5 nm;

[0101] S231, placing the sample in an ALD chamber, evacuating the chamber, introducing diethyl zinc, and depositing a first film 13 made of zinc oxide. Preferably, the source flow rate is 200 sccm (standard cubic centimeter per minute), the deposition temperature is 400° C., and the thickness is 3 nm.

[0102] S232, after purging the residual gas in the ALD chamber of step S231 with nitrogen, trimethylaluminum is introduced to deposit a second film 14 made of aluminum-doped zinc oxide. Preferably, the source flow rate is 300 sccm, the deposition temperature is 500° C., and the thickness is 1 nm;

[0103] S233, after purging the residual gas in the ALD chamber of step S232 with nitrogen, diethyl zinc is introduced to deposit a first film 13 made of zinc oxide. Preferably, the source flow rate is 200 sccm, the deposition temperature is 400° C., and the thickness is 7 nm;

[0104] S234, after purging the residual gas in the ALD chamber of step S233 with nitrogen, trimethylaluminum is introduced to deposit a second film 14 made of aluminum-doped zinc oxide. Preferably, the source flow rate is 300 sccm, the deposition temperature is 500° C., and the thickness is 1 nm;

[0105] S235, after purging the residual gas in the ALD chamber of step S234 with nitrogen, diethyl zinc is introduced to deposit a first film 13 made of zinc oxide. Preferably, the source flow rate is 200 sccm, the deposition temperature is 400° C., and the thickness is 3 nm;

[0106] S236, after purging the residual gas in the ALD chamber of step S235 with nitrogen, trimethylaluminum is introduced to deposit a second film 14 made of aluminum-doped zinc oxide. Preferably, the source flow rate is 300 sccm, the deposition temperature is 500° C., and the thickness is 60 nm;

[0107] S240, depositing a second dielectric film 15 on the sample of step S236 by LPCVD method at a temperature of 500° C. and a pressure of 0.3 torr. Preferably, the thickness of the second dielectric film 15 is 5 nm;

[0108] S250, placing the sample in step S240 on a heating table, and annealing at 200°C for 10 minutes.

[0109] In the third embodiment of the method for preparing a solar cell of the present invention, the specific steps of the method for preparing a solar cell are as follows:

[0110] S310, selecting a single crystal silicon wafer as the substrate 11, pre-polishing it with a sodium hydroxide alkaline solution, and cleaning it with an RCA standard cleaning method;

[0111] S320, using an LPCVD method, at a temperature of 500° C. and a pressure of 0.3 torr, depositing a first dielectric film 12, preferably, the thickness of the first dielectric film 12 is 5 nm;

[0112] S331, placing the sample in an ALD chamber, evacuating the chamber, introducing diethyl zinc, and depositing a first film 13 made of zinc oxide. Preferably, the source flow rate is 200 sccm, the deposition temperature is 400° C., and the thickness is 3 nm.

[0113] S332, after purging the residual gas in the ALD chamber of step S331 with nitrogen, trimethylaluminum is introduced to deposit a second film 14 made of aluminum-doped zinc oxide. Preferably, the source flow rate is 300 sccm, the deposition temperature is 500° C., and the thickness is 1 nm;

[0114] S333, after purging the residual gas in the ALD chamber of step S332 with nitrogen, diethyl zinc is introduced to deposit a first film 13 made of zinc oxide. Preferably, the source flow rate is 200 sccm, the deposition temperature is 400° C., and the thickness is 7 nm;

[0115] S334, after purging the residual gas in the ALD chamber of step S333 with nitrogen, trimethylaluminum is introduced to deposit a second film 14 made of aluminum-doped zinc oxide. Preferably, the source flow rate is 300 sccm, the deposition temperature is 500° C., and the thickness is 1 nm;

[0116] S335, after purging the residual gas in the ALD chamber of step S334 with nitrogen, diethyl zinc is introduced to deposit a first film 13 made of zinc oxide. Preferably, the source flow rate is 200 sccm, the deposition temperature is 400° C., and the thickness is 3 nm;

[0117] S340, placing the sample in step S335 in a PECVD chamber, and introducing ammonia and silane to deposit a second dielectric film 15, preferably, the deposition temperature is 550° C., and the thickness is 80 nm;

[0118] S350, placing the sample of step S240 on a heating table, and annealing at 200°C for 10 minutes.

[0119] In the fourth embodiment of the method for preparing a solar cell of the present invention, the specific steps of the method for preparing a solar cell are as follows:

[0120] S410, selecting a single crystal silicon wafer as the substrate 11, pre-polishing it with a sodium hydroxide alkaline solution, and cleaning it with an RCA standard cleaning method;

[0121] S420, using an LPCVD method, at a temperature of 500° C. and a pressure of 0.3 torr, depositing a first dielectric film 12, preferably, the thickness of the first dielectric film 12 is 5 nm;

[0122] S431, placing the sample in an ALD chamber, evacuating the chamber, introducing diethyl zinc, and depositing a first film 13 made of zinc oxide. Preferably, the source flow rate is 200 sccm, the deposition temperature is 400° C., and the thickness is 3 nm.

[0123] S432, after purging the residual gas in the ALD chamber of step S431 with nitrogen, trimethylaluminum is introduced to deposit a second film 14 made of aluminum-doped zinc oxide. Preferably, the source flow rate is 300 sccm, the deposition temperature is 500° C., and the thickness is 1 nm;

[0124] S433, after purging the residual gas in the ALD chamber of step S432 with nitrogen, diethyl zinc is introduced to deposit a first film 13 made of zinc oxide. Preferably, the source flow rate is 200 sccm, the deposition temperature is 400° C., and the thickness is 7 nm;

[0125] S434, after purging the residual gas in the ALD chamber of step S433 with nitrogen, trimethylaluminum is introduced to deposit a second film 14 made of aluminum-doped zinc oxide. Preferably, the source flow rate is 300 sccm, the deposition temperature is 500° C., and the thickness is 1 nm;

[0126] S435, repeating the process of step S433 and step S434 10 times;

[0127] S436, after purging the residual gas in the ALD chamber of step S435 with nitrogen, diethyl zinc is introduced to deposit a first film 13 made of zinc oxide. Preferably, the source flow rate is 200 sccm, the deposition temperature is 400° C., and the thickness is 3 nm;

[0128] S440, after purging the residual gas in the ALD chamber of step S436 with nitrogen, trimethylaluminum is introduced to deposit a second dielectric film 15, preferably, the source flow rate is 300 sccm, the deposition temperature is 500° C., and the thickness is 100 nm;

[0129] S450, placing the sample in step S440 on a heating table, and annealing at 200°C for 10 minutes.

[0130] The method for preparing a solar cell of the present invention uses aluminum-doped zinc oxide material instead of traditional aluminum oxide material to prepare a passivation layer, which can avoid laser damage to silicon wafers, improve the conductivity and transmittance of the battery, reduce production costs, and comply with the industry trend of low-temperature preparation.

[0131] In summary, the solar cell and its preparation method of the present invention, by using aluminum-doped zinc oxide material instead of traditional aluminum oxide material to prepare the passivation layer, can avoid laser damage to silicon wafers, improve the conductivity and transmittance of the battery, reduce production costs, and comply with the industry trend of low-temperature preparation.

[0132] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as falling within the protection scope of the present invention.

Claims

1. A solar cell, characterized in that: include: substrate; A first dielectric film is stacked on one side of the substrate; At least two first thin films are stacked and arranged on a side of the first dielectric film away from the substrate, and the material of the first thin films is zinc oxide; At least two layers of second thin films are stacked on a side of the first dielectric film away from the substrate, the second thin films comprising a main material and a doping material, the main material is at least zinc oxide, the doping material is at least aluminum, and the doping material is used to improve the conductivity and transmittance of the passivation layer; as well as A second dielectric film is stacked on a side of the first dielectric film away from the substrate, and the first film and the second film are located between the first dielectric film and the second dielectric film; Wherein, the thickness of the first film is 0.2-100 nm, and the thickness of the second film is 0.1-50 nm; The aluminum content in the first film and the second film is 0.5% to 50%; The first thin films and the second thin films are alternately stacked and arranged between the first dielectric film and the second dielectric film.

2. The solar cell according to claim 1, characterized in that The doping material of the second film is at least one or a combination of aluminum, gallium, indium, titanium, and fluorine.

3. The solar cell according to claim 1, characterized in that The first thin film and the second thin film are both prepared by an atomic layer deposition method.

4. The solar cell according to claim 1, characterized in that The first dielectric film and the second dielectric film are both made of SiO2, Si3N4, SiO x N y or AlO x One or more compositions, with a thickness of 0.1 to 1000 nm.

5. The solar cell according to claim 4, characterized in that: The thickness of the first dielectric film is 0.2-100 nm, and the thickness of the second dielectric film is 0.1-200 nm.

6. The solar cell according to claim 4, characterized in that: The first dielectric film and the second dielectric film are deposited and prepared by one or more methods selected from the group consisting of low-pressure vapor deposition, atmospheric-pressure vapor deposition, plasma-enhanced chemical vapor deposition, atomic layer deposition, and magnetron sputtering.

7. The solar cell according to claim 1, characterized in that The substrate is a single crystal silicon wafer.

8. A method for preparing a solar cell, for preparing the solar cell according to claim 1, characterized in that: include: providing a substrate; preparing a first dielectric film on one side of the substrate; At least two first thin films are prepared on a side of the first dielectric film away from the substrate, wherein the material of the first thin films is zinc oxide; At least two layers of second thin films are prepared on the side of the first dielectric film away from the substrate, the second thin films contain a main material and a doping material, the main material is at least zinc oxide, the doping material is at least aluminum, and the doping material is used to improve the conductivity and transmittance of the passivation layer; wherein the thickness of the first thin film is 0.2-100nm, the thickness of the second thin film is 0.1-50nm; the aluminum content in the first thin film and the second thin film is 0.5%-50%; the first thin film and the second thin film are alternately stacked between the first dielectric film and the second dielectric film; and A second dielectric film is formed on a side of the first dielectric film facing away from the substrate, and the first thin film and the second thin film are located between the first dielectric film and the second dielectric film.

9. The method for preparing a solar cell according to claim 8, characterized in that: The step of preparing at least one first thin film on a side of the first dielectric film facing away from the substrate comprises: Purge the gas residue in the atomic layer deposition chamber with nitrogen; introducing a zinc-containing compound and controlling the deposition temperature within a preset temperature range to prepare the first thin film; and When the thickness of the first film reaches a preset thickness range, the deposition is stopped.

10. The method for preparing a solar cell according to claim 8, characterized in that: The step of preparing at least one second thin film on a side of the first dielectric film facing away from the substrate comprises: Purge the gas residue in the atomic layer deposition chamber with nitrogen; introducing an aluminum-containing compound and controlling the deposition temperature within a preset temperature range to prepare the second thin film; and When the thickness of the second film reaches a preset thickness range, the deposition is stopped.

Citation Information

Patent Citations

  • Solar cell and preparation method thereof

    CN114005888A