Preparation process of a highly absorbent resin and its application in soil metal adsorption

By introducing DL-cysteine ​​and histidine into polyvinyl alcohol and cross-linking it with acrylate histidine, a super absorbent resin is formed, which solves the problem of poor heavy metal adsorption performance of traditional resin in soil and achieves It has high water absorption and improved water retention performance, and shows excellent adsorption performance in the field of soil remediation.

CN117843875BActive Publication Date: 2024-10-18INST OF AGRI PROD QUALITY SAFETY & STANDARD JIANGXI ACAD OF AGRI SCI
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202311686467.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-11
Publication Date
2024-10-18
Estimated Expiration
2043-12-11

AI Technical Summary

Technical Problem

Traditional polyvinyl alcohol water-absorbent resin has poor adsorption performance of heavy metals in soil, is not environmentally friendly, and has the risk of secondary pollution.

Method used

Using polyvinyl alcohol as the matrix, introducing DL-cysteine ​​and histidine as functional monomers, cross-linking with acrylate histidine to form a super absorbent resin, containing hydrophilic amino, carboxyl, imine and other groups groups to form a three-dimensional network structure, improve water absorption and water retention properties, and form strong coordination and complexation with heavy metal ions through amino, carboxyl, mercaptoimidazole and other groups.

Benefits of technology

It significantly improves the water absorption and water retention performance of the water-absorbent resin, enhances the adsorption capacity of heavy metal ions such as Cd2+ and Pb2+, and provides a green and environmentally friendly soil remediation and water retention solution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117843875B_ABST
    Figure CN117843875B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of water-absorbent resins, and discloses a preparation process of a highly water-absorbent resin and its application in soil metal adsorption. The highly water-absorbent resin prepared by the present invention contains hydrophilic amino, carboxyl, imine and other groups, which significantly improves the water absorption rate of the water-absorbent resin; at the same time, acrylate histidine is used as a functional cross-linking agent to form a three-dimensional network structure through cross-linking, which has good water retention performance. It is very useful in the field of soil water retention and remediation. The highly water-absorbent resin contains functional groups such as amino, carboxyl, and mercaptoimidazole, which can be combined with Cd 2+ , Pb 2+ The metal ions form strong coordination complexation and electrostatic interaction, so that the super absorbent resin exhibits excellent adsorption performance; it has good application in the field of soil metal adsorption and soil remediation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of water-absorbent resins, in particular to a preparation process of a highly water-absorbent resin and its application in soil metal adsorption. Background Art

[0002] With the modernization of industry and agriculture in human society, the problem of heavy metal pollution in soil caused by human activities is becoming more and more serious. The main source of heavy metal pollution is the development and smelting of non-ferrous heavy metal deposits; such as mining, mineral processing, metallurgy, electroplating and other industries. When the soil contains a large amount of heavy metals such as cadmium, lead, and mercury, it will cause serious harm to the growth and reproduction of animals in the soil, as well as the growth of crops.

[0003] Water-absorbent resin is a polymer resin material with high water absorption performance, which is widely used in soil water-retaining agent, soil remediation agent, metal pollutant adsorption material, etc.; such as polyacrylic acid, polyacrylamide, etc.; however, these synthetic resins are not environmentally friendly, will form secondary pollution in the soil, and their functional groups are relatively single; polyvinyl alcohol is a green and environmentally friendly polymer material, and has good hydrophilicity and biodegradability; it can be used as a matrix for highly absorbent resin; amino acid compounds, such as cysteine, histidine, etc., have good biocompatibility, are non-toxic and environmentally friendly, and the development of new polyamino acid resins is a research hotspot. Summary of the invention

[0004] Technical problem solved: Provides a green and environmentally friendly highly absorbent resin, which solves the problems of low water absorption and water retention rate of traditional polyvinyl alcohol absorbent resin and poor adsorption performance for soil heavy metals.

[0005] Technical solution:

[0006] A preparation process of a highly absorbent resin comprises the following steps: adding distilled water and polyvinyl alcohol to a flask, heating to 95° C. and stirring to dissolve, cooling to 55-65° C. and adding pentylene imine cysteine ​​and acrylate histidine, stirring to dissolve, introducing nitrogen, adding azobisisobutyronitrile, stirring to react for 2-4 hours, filtering the solvent, washing the product with water, placing it in a dialysis bag, and purifying it with distilled water to obtain a highly absorbent resin;

[0007] Further, the chemical structure of pentylenimine cysteine ​​is:

[0008] The chemical structure of histidine acrylate is:

[0009] Furthermore, the masses of pentylene imine cysteine ​​and acrylate histidine are 400-800% and 15-60% of the mass of polyvinyl alcohol, respectively.

[0010] Furthermore, pentylenimine cysteine ​​is prepared according to the following process: a solvent, DL-cysteine ​​and 4-pentenal are added to a flask, reacted at 55-70° C. for 6-12 hours, cooled, concentrated to remove the solvent, washed with n-hexane, and dried to obtain pentylenimine cysteine.

[0011] Furthermore, the solvent is any one of ethanol, isopropanol and 1,4-dioxane.

[0012] Further, histidine acrylate is prepared according to the following process:

[0013] S1. Add a reaction solvent, a catalyst, benzyloxycarbonyl-DL-histidine and 2,2-bis(bromomethyl)-1,3-propanediol into a flask, stir to react, add water and ethyl acetate, extract and separate, concentrate the organic phase to obtain an intermediate.

[0014] S2. Add dichloromethane, the intermediate and triethylamine into a flask, add acryloyl chloride dropwise at -5 to 5°C, then react at room temperature for 4-10 hours, concentrate the solvent, wash the product with petroleum ether, dissolve it in ethanol, add Pd / C catalyst, pass hydrogen, react at room temperature for 12-18 hours, filter and recover the Pd / C catalyst, concentrate the filtrate, and recrystallize the product in ethyl acetate to obtain acrylate histidine.

[0015] Furthermore, in S1, the reaction solvent is ethanol or methanol; and the catalyst is sodium ethoxide or sodium methoxide.

[0016] Furthermore, the masses of the catalyst and benzyloxycarbonyl-DL-histidine in S1 are (25-30)% and (220-280)% of the mass of 2,2-bis(bromomethyl)-1,3-propanediol, respectively.

[0017] Furthermore, in S1, the reaction temperature is controlled to be 65-80°C, and the reaction time is controlled to be 2-4h.

[0018] Furthermore, the masses of triethylamine and acryloyl chloride in S2 are (25-32)% and (28-35)% of the mass of the intermediate, respectively.

[0019] Technical effect: The present invention uses DL-cysteine ​​and benzyloxycarbonyl-DL-histidine as the functional monomers to prepare pentylenimine cysteine ​​and acrylate histidine, wherein acrylate histidine contains two alkenyl groups and can replace the traditional N,N-methylenebisacrylamide crosslinking agent, and is grafted and crosslinked with polyvinyl alcohol to obtain a highly absorbent resin. The highly absorbent resin uses polyvinyl alcohol as the matrix and introduces amino acid bio-based functional monomers of cysteine ​​and histidine, which has the advantages of being non-toxic and green.

[0020] The highly water-absorbent resin prepared by the present invention contains hydrophilic amino, carboxyl, imine and other groups, which significantly improves the water absorption rate of the water-absorbent resin; at the same time, acrylate histidine is used as a functional cross-linking agent to form a three-dimensional network structure through cross-linking, and has good water retention performance. It is very suitable for the field of soil water retention and restoration.

[0021] The highly absorbent resin prepared by the present invention contains functional groups such as amino, carboxyl, and mercaptoimidazole, which can react with Cd 2+ , Pb 2+ The metal ions form strong coordination complexation and electrostatic interaction, so that the super absorbent resin exhibits excellent adsorption performance; it has good application in the field of soil metal adsorption and soil remediation. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is the reaction formula for the preparation of pentylene imine cysteine.

[0023] Figure 2 This is the reaction formula for the preparation of histidine acrylate. DETAILED DESCRIPTION

[0024] In the following description, for the purpose of illustration, in order to provide a comprehensive understanding of one or more embodiments, many specific details are set forth. However, it is apparent that these embodiments may also be implemented without these specific details. In other examples, for ease of describing one or more embodiments, known structures and devices are shown in the form of block diagrams.

[0025] Example 1

[0026] Add 50 mL of ethanol solvent, 3 g of DL-cysteine, and 2.5 g of 4-pentenal into a flask, react at 70° C. for 6 h, cool, concentrate to remove the solvent, wash with n-hexane, and dry to obtain pentylenimine cysteine.

[0027] Add 80 mL of ethanol solvent, 0.82 g of sodium ethoxide catalyst, 7.2 g of benzyloxycarbonyl-DL-histidine, and 3 g of 2,2-bis(bromomethyl)-1,3-propanediol into a flask, stir and reflux at 65°C for 4 h, add water and ethyl acetate, extract and separate, and concentrate the organic phase to obtain an intermediate.

[0028] Add 120 mL of dichloromethane, 8 g of the intermediate and 2.56 g of triethylamine into a flask, add 2.68 g of acryloyl chloride dropwise at 0°C, then react at room temperature for 10 h, concentrate the solvent, wash the product with petroleum ether, dissolve it in 100 mL of ethanol, add 1.1 g of Pd / C catalyst, pass hydrogen, react at room temperature for 12 h, filter and recover the Pd / C catalyst, concentrate the filtrate, and recrystallize the product in ethyl acetate to obtain acrylate histidine.

[0029] Add 40 mL of distilled water and 2 g of polyvinyl alcohol to a flask, heat to 95 ° C and stir to dissolve, cool to 55 ° C, add 8 g of pentylene imine cysteine ​​and 0.3 g of acrylate histidine (0.58 mmol), stir to dissolve, pass nitrogen, add 0.06 g of azobisisobutyronitrile, stir to react for 3 hours, filter the solvent, wash the product with water, put it in a dialysis bag, dialyze it with distilled water, and obtain a highly absorbent resin.

[0030] Example 2

[0031] Add 30 mL of 1,4-dioxane solvent, 3 g of DL-cysteine, and 2.1 g of 4-pentenal into a flask, react at 60° C. for 12 h, cool, concentrate to remove the solvent, wash with n-hexane, and dry to obtain pentylenimine cysteine.

[0032] Add 80 mL of ethanol solvent, 0.9 g of sodium ethoxide catalyst, 7.8 g of benzyloxycarbonyl-DL-histidine, and 3 g of 2,2-bis(bromomethyl)-1,3-propanediol into a flask, stir and reflux at 80°C for 2 h, add water and ethyl acetate, extract and separate, and concentrate the organic phase to obtain an intermediate.

[0033] Add 80 mL of dichloromethane, 8 g of the intermediate and 2 g of triethylamine into a flask, add 2.24 g of acryloyl chloride dropwise at -5 °C, then react at room temperature for 4 h, concentrate the solvent, wash the product with petroleum ether, dissolve it in 100 mL of ethanol, add 0.9 g of Pd / C catalyst, pass hydrogen, react at room temperature for 18 h, filter and recover the Pd / C catalyst, concentrate the filtrate, and recrystallize the product in ethyl acetate to obtain acrylate histidine.

[0034] Add 80 mL of distilled water and 2 g of polyvinyl alcohol to a flask, heat to 95 ° C and stir to dissolve, cool to 55 ° C, add 12 g of pentylene imine cysteine ​​and 0.8 g of acrylate histidine, stir to dissolve, pass nitrogen, add 0.068 g of azobisisobutyronitrile, stir to react for 4 hours, filter the solvent, wash the product with water, put it in a dialysis bag, and purify it with distilled water to obtain a highly absorbent resin.

[0035] Example 3

[0036] Add 40 mL of isopropanol solvent, 3 g of DL-cysteine, and 2.5 g of 4-pentenal into a flask, react at 55° C. for 12 h, cool, concentrate to remove the solvent, wash with n-hexane, and dry to obtain pentylenimine cysteine.

[0037] Add 60 mL of methanol solvent, 0.75 g of sodium methoxide catalyst, 6.6 g of benzyloxycarbonyl-DL-histidine, and 3 g of 2,2-bis(bromomethyl)-1,3-propanediol into a flask, stir and reflux at 70°C for 4 h, add water and ethyl acetate, extract and separate, and concentrate the organic phase to obtain an intermediate.

[0038] Add 120 mL of dichloromethane, 8 g of the intermediate and 2.4 g of triethylamine to a flask, add 2.8 g of acryloyl chloride dropwise at 5 °C, then react at room temperature for 6 h, concentrate the solvent, wash the product with petroleum ether, dissolve it in 100 mL of ethanol, add 0.8 g of Pd / C catalyst, pass hydrogen, react at room temperature for 18 h, filter and recover the Pd / C catalyst, concentrate the filtrate, and recrystallize the product in ethyl acetate to obtain acrylate histidine.

[0039] Add 80 mL of distilled water and 2 g of polyvinyl alcohol to a flask, heat to 95 ° C and stir to dissolve, cool to 65 ° C, add 16 g of pentylene imine cysteine ​​and 1.2 g of acrylate histidine, stir to dissolve, pass nitrogen, add azobisisobutyronitrile, stir to react for 2 hours, filter the solvent, wash the product with water, put it in a dialysis bag, dialyze with distilled water to purify it, and obtain a highly absorbent resin.

[0040] Comparative Example 1

[0041] The difference between Comparative Example 1 and Example 1 is that pentylenimine cysteine ​​is not added.

[0042] Add 40 mL of distilled water and 2 g of polyvinyl alcohol to a flask, heat to 95 ° C and stir to dissolve, cool to 55 ° C, add 0.3 g of histidine acrylate (0.58 mmol), stir to dissolve, pass nitrogen, add 0.06 g of azobisisobutyronitrile, stir to react for 3 hours, filter the solvent, wash the product with water, put it in a dialysis bag, dialyze it with distilled water to obtain a water-absorbent resin.

[0043] Comparative Example 2

[0044] The difference between Comparative Example 1 and Example 1 is that no histidine acrylate is added.

[0045] Add 40 mL of distilled water and 2 g of polyvinyl alcohol to a flask, heat to 95 ° C and stir to dissolve, cool to 55 ° C, add 8 g of pentylene imine cysteine, stir to dissolve, pass nitrogen, add 0.075 g of azobisisobutyronitrile, stir to react for 3 hours, filter the solvent, wash the product with water, put it in a dialysis bag, dialyze it with distilled water to obtain a water-absorbent resin.

[0046] Comparative Example 3

[0047] The difference of Comparative Example 3 is that an equimolar amount of N,N-methylenebisacrylamide is used as a cross-linking agent instead of histidine acrylate.

[0048] Add 40 mL of distilled water and 2 g of polyvinyl alcohol to a flask, heat to 95 ° C and stir to dissolve, cool to 55 ° C, add 8 g of pentylene imine cysteine ​​and 0.089 g of N, N-methylenebisacrylamide (0.58 mmol), stir to dissolve, pass nitrogen, add 0.075 g of azobisisobutyronitrile, stir to react for 3 hours, filter the solvent, wash the product with water, put it in a dialysis bag, dialyze it with distilled water to obtain a water-absorbent resin.

[0049] Determination of water absorption rate of water-absorbent resin: Weigh a certain mass (m) of water-absorbent resin, put it into distilled water, soak it at room temperature for 6 hours, take out the resin, wipe off the excess water, weigh it m1; calculate the water absorption rate Q. Put the resin after water absorption at room temperature for 72 hours, then wipe off the excess water, weigh it m2; calculate the water retention rate W. Water absorption rate Q = (m1-m) / m; Water retention rate W = (m2 / m1)×100%.

[0050] Table 1 Water absorption and water retention test of water-absorbent resin

[0051] Water absorption (g / g) Water retention rate (%) Example 1 794.2 84.1 Example 2 1220.1 90.2 Example 3 1014.1 90.6 Comparative Example 1 362.7 85.6 Comparative Example 2 112.4 12.9 Comparative Example 3 602.3 80.8

[0052] In Examples 1 to 3, pentylenimine cysteine ​​is used as a functional monomer, acrylate histidine is used as a functional crosslinking agent, and crosslinking polymerization is carried out with polyvinyl alcohol to obtain a highly absorbent resin, which contains hydrophilic amino, carboxyl, imine and other groups, and significantly improves the water absorption rate of the absorbent resin to 794.2-1220.1%; at the same time, acrylate histidine is used as a functional crosslinking agent, and crosslinking forms a three-dimensional network structure, which has good water retention performance. It is very well used in the field of soil water retention and remediation.

[0053] In Comparative Example 1, no pentylene imine cysteine ​​was added, and the hydrophilic carboxyl and imine contents of the water-absorbent resin were lower than those in Example 1, and the water absorption rate was lower.

[0054] In Comparative Example 2, no acrylate histidine was added, and polyvinyl alcohol and pentylene imine cysteine ​​could not be chemically cross-linked to form a three-dimensional network structure, and the water absorption rate and water retention rate were the lowest.

[0055] Comparative Example 3 uses an equimolar amount of N,N-methylenebisacrylamide as a crosslinking agent instead of histidine acrylate. N,N-methylenebisacrylamide does not contain hydrophilic amino and carboxyl groups, resulting in a lower water absorption rate of the water-absorbent resin than that of Example 1.

[0056] Soil metal ion adsorption simulation experiment: Weigh 100g natural soil, crush and dry it, mix it with 10mg cadmium nitrate or lead nitrate, add it to 300mL water, stir it thoroughly to make a simulated soil solution, remove the last clear solution, provide atomic absorption spectrophotometry, and then add Cd 2+ or Pb 2+Add 0.5g of absorbent resin, stir and adsorb, and measure the Cd content of the solution every 0.5h. 2+ or Pb 2+ The concentration C1 is used to calculate the adsorption rate A. A = (C-C1) / C×100%. C is the concentration of metal ions in the soil solution before adsorption, and C1 is the concentration of metal ions in the soil solution after adsorption.

[0057] Table 2 Water absorption rate Cd of water-absorbent resin 2+ Adsorption rate test.

[0058]

[0059]

[0060] Table 3 Water absorption rate Pb of water-absorbent resin 2+ Adsorption rate test.

[0061]

[0062] In Example 1-3, pentylenimine cysteine ​​is used as a functional monomer, acrylate histidine is used as a functional crosslinking agent, and polyvinyl alcohol is subjected to crosslinking polymerization to obtain a highly absorbent resin containing amino, carboxyl, mercaptoimidazole and other functional groups, which can be combined with Cd 2+ , Pb 2+ The metal ions form strong coordination complexation and electrostatic interaction, so that the super absorbent resin exhibits excellent adsorption performance; it has good application in the field of soil metal adsorption and soil remediation.

[0063] Comparative Example 1 did not add pentylene imine cysteine, the water-absorbing resin did not contain thiol groups, and the carboxyl content was low, which was effective for Cd 2+ , Pb 2+ The adsorption performance is the worst.

[0064] Comparative Example 2 did not add acrylate histidine, and the water-absorbing resin did not contain imidazole groups. Compared with Example 1, the amino and carboxyl groups contents were lower, and the Cd 2+ , Pb 2+ The adsorption performance is poor.

[0065] Comparative Example 3 uses an equal molar amount of N,N-methylenebisacrylamide as a crosslinking agent to replace histidine acrylate. The water-absorbing resin does not contain imidazole groups. Compared with Example 1, the amino and carboxyl groups are lower in content. 2+ , Pb 2+ The adsorption performance is poor.

Claims

1. A process for preparing a highly water-absorbent resin, characterized in that: The highly absorbent resin is prepared according to the following process: distilled water and polyvinyl alcohol are added to a flask, heated and stirred to dissolve, then pentylene imine cysteine ​​and acrylate histidine are added at 55-65° C., stirred to dissolve, nitrogen is introduced, azobisisobutyronitrile is added, stirred to react for 2-4 hours, the solvent is filtered, the product after washing is placed in a dialysis bag, and purified by dialysis with distilled water to obtain a highly absorbent resin; The chemical structure of the pentylene imine cysteine ​​is: The chemical structure of the histidine acrylate is:

2. The process for preparing a highly water-absorbent resin according to claim 1, characterized in that: The masses of the pentylene imine cysteine ​​and the acrylate histidine are 400-800% and 15-60% of the mass of the polyvinyl alcohol respectively.

3. The process for preparing a highly water-absorbent resin according to claim 1, characterized in that: The pentylenimine cysteine ​​is prepared according to the following process: adding a solvent, DL-cysteine ​​and 4-pentenal into a flask, reacting at 55-70° C. for 6-12 hours, cooling, concentrating to remove the solvent, washing and drying to obtain pentylenimine cysteine.

4. The process for preparing a highly water-absorbent resin according to claim 3, characterized in that: The solvent is any one of ethanol, isopropanol and 1,4-dioxane.

5. The process for preparing a highly water-absorbent resin according to claim 1, characterized in that: The histidine acrylate is prepared according to the following process: S1, adding a reaction solvent, a catalyst, benzyloxycarbonyl-DL-histidine, and 2,2-bis(bromomethyl)-1,3-propanediol into a flask, stirring for reaction, extracting and separating, and concentrating the organic phase to obtain an intermediate; S2. Add dichloromethane, the intermediate and triethylamine into a flask, add acryloyl chloride dropwise at -5 to 5°C, then react at room temperature for 4-10 hours, concentrate the solvent, wash the product with petroleum ether, dissolve it in ethanol, add Pd / C catalyst, pass hydrogen, react at room temperature for 12-18 hours, filter, concentrate the filtrate, and recrystallize to obtain acrylate histidine.

6. The process for preparing a highly water-absorbent resin according to claim 5, characterized in that: In the S1, the reaction solvent is ethanol or methanol; the catalyst is sodium ethoxide or sodium methoxide.

7. The process for preparing a highly water-absorbent resin according to claim 5, characterized in that: The masses of the catalyst and benzyloxycarbonyl-DL-histidine in S1 are respectively (25-30)% and (220-280)% of the mass of 2,2-bis(bromomethyl)-1,3-propanediol.

8. The process for preparing a highly water-absorbent resin according to claim 5, characterized in that: In the S1, the reaction temperature is controlled at 65-80°C, and the reaction time is controlled at 2-4h.

9. The process for preparing a highly water-absorbent resin according to claim 5, characterized in that: The masses of triethylamine and acryloyl chloride in S2 are (25-32)% and (28-35)% of the intermediate mass, respectively.

10. Use of the highly absorbent resin according to any one of claims 1 to 9 in soil metal adsorption.

Citation Information

Patent Citations

  • Preparation method of enzymatically hydrolyzed sericin protein composite absorbent material

    CN103044636A

  • Cation functional polymers with natural amino acid as side group, preparation method and application of polymer

    CN103665222A

  • Preparation method of polyaspartic acid / polyacrylic acid interpenetrating network super absorbent resin

    CN104327208A

  • High-water-absorptivity resin and preparation method thereof

    CN105348444A

  • Biodegradable polyaspartic acid based chelate resin and preparation method thereof

    CN106046375A