A phenolic resin-coated platinum catalyst, its preparation method and application
By coating platinum catalysts with phenolic resin, the curing degradation problem of addition-type silicone potting compounds under different temperature environments was solved, and the stable dispersion and uniform curing of platinum catalysts in new energy vehicle battery packs were achieved.
Patent Information
- Application Number
- CN202410037525.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-10
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-01-10
AI Technical Summary
Existing addition-type silicone potting compounds cannot effectively exude platinum catalysts at room temperature and low temperature, resulting in curing degradation and making them unsuitable for the different temperature environments of new energy vehicle battery packs.
A platinum catalyst coated with phenolic resin was prepared by using phenolic resin as a carrier material, a foaming agent to form pores, a surfactant to promote compatibility, a platinum complex as the host material, and isopropanol as a solvent. The preparation process included mixing, spraying, coating, and stirring to form a phenolic resin-coated platinum catalyst with uniform particle size.
It effectively slows down the curing decay of addition-type silicone potting compound, ensures uniform dispersion of platinum catalyst in various temperature ranges, and improves product stability and applicability.
Abstract
Description
Technical Field
[0001] This invention relates to a phenolic resin-coated platinum catalyst, and also to a method for preparing and applying the phenolic resin-coated platinum catalyst, belonging to the field of adhesives for new energy vehicle battery packs. Background Technology
[0002] Addition-cure silicone potting compounds are a special type of polymer material that can cure at room temperature or by heating, with the curing speed increasing with temperature. During the curing process, addition-cure silicone potting compounds do not produce any byproducts. They are commonly used for waterproof potting protection of larger electronic components such as waterproof power supplies and communication modules. The rapid development of new energy electric vehicles has also driven the rapid development of power batteries, with continuously improving energy density and significantly enhanced driving range. However, this rapid development has also brought hidden dangers. The key technology of new energy electric vehicles lies in high-energy-density batteries, and the addition-cure silicone potting compounds used in new energy vehicle battery packs require extremely low density, currently mainly relying on the addition of a large number of hollow glass microspheres. As a lightweight filler, hollow glass microspheres contain substances on their surface that can cause curing degradation of the addition-cure silicone potting compound. To address this issue, most manufacturers now employ different treatment methods to modify hollow glass microspheres. For example, there are reports of using microcapsule platinum catalysts to improve hollow glass microspheres. However, the microcapsules are made of thermoplastic resin, and the platinum catalyst cannot effectively leach out of the microcapsules at room temperature and low temperature. This method is only suitable for use at higher temperatures and is not applicable at room temperature and low temperature. Summary of the Invention
[0003] The purpose of this invention is to provide a phenolic resin-coated platinum catalyst so that addition-type silicone potting compound is suitable for different temperature environments.
[0004] Another objective of this invention is to provide a method for preparing a phenolic resin-coated platinum catalyst.
[0005] Furthermore, the present invention aims to utilize a phenolic resin-coated platinum catalyst in the preparation of addition-type silicone potting compound.
[0006] To achieve the above objectives, the technical solution of the present invention further comprises a phenolic resin-coated platinum catalyst, comprising the following raw materials in parts by weight: 80 to 200 parts of phenolic resin, 4 to 20 parts of foaming agent, 1.5 to 12 parts of surfactant, 0.3 to 0.5 parts of platinum complex, 10 to 40 parts of isopropanol, 0.5 to 5 parts of catalyst, and 160 to 400 parts of water.
[0007] In this technical solution, phenolic resin serves as the adsorbent carrier resin for the platinum catalyst, the foaming agent is an auxiliary agent that helps the phenolic resin to form pores after curing, the surfactant is a compatibilizer that promotes the compatibility between the phenolic resin and water, the platinum complex is the main material of the platinum catalyst, and isopropanol is a solvent.
[0008] The foaming agent is one of dichloromethane, n-pentane, or a combination thereof.
[0009] The surfactant is at least one of fatty alcohol polyoxyethylene, fatty alcohol polyoxypropylene ether; or alkylphenol polyoxyethylene ether; or block copolymer of polysiloxane, polyoxyethylene, and polyoxypropylene.
[0010] The catalyst is one or any combination of oxalic acid, adipic acid, benzene nitric acid, phenolic nitric acid, toluene sulfonic acid, benzene sulfonic acid, and petroleum sulfonate.
[0011] The platinum complex is selected from the Karstedt catalyst (a diluent of platinum(O)-divinyltetramethyldisiloxane complex).
[0012] The isopropanol mentioned is of analytical grade.
[0013] The technical solution of the present invention also lies in the use of a method for preparing a phenolic resin-coated platinum catalyst, comprising the following steps: (1) Mix the foaming agent, surfactant, catalyst and half the weight of phenolic resin, stir, add water while stirring, heat to 100-120℃, filter, dry, and sieve to obtain phenolic resin microspheres. (2) Mix the platinum complex and isopropanol, stir, and obtain a platinum complex mixture; (3) Spray the platinum complex mixture from step (2) evenly onto the surface of the phenolic resin microspheres from step (1), and let it stand for 0.5-1.5 hours to obtain phenolic resin microspheres coated with platinum complex. (4) Mix the other half of the phenolic resin with the catalyst and isopropanol, and stir to obtain a phenolic resin mixture; (5) Place the phenolic resin microspheres coated with the platinum complex from step (3) into a spray tower. During the stirring process, uniformly coat the phenolic resin mixture from step (4) onto the surface of the phenolic resin microspheres coated with the platinum complex. During the high-speed stirring process of the airflow, raise the temperature to 100℃-120℃, stir, and sieve to obtain the phenolic resin coated platinum catalyst.
[0014] The specific process of step (1) is as follows: Phenolic resin, foaming agent, surfactant, and catalyst are added to a disperser, and the stirring speed is set to 1000 r / min-2000 r / min for 10 min-15 min. Then water is added, and the stirring speed is set to 3000 r / min-5000 r / min for 1 h-3 h. Then the temperature is heated to 100℃, and the stirring speed is set to 1000 r / min-2000 r / min for 2 h-4 h. The mixture is then filtered, dried, and sieved through an 80-mesh sieve to obtain phenolic resin microspheres.
[0015] The technical solution of this invention also employs the application of a phenolic resin-coated platinum catalyst in an addition-type silicone potting compound, wherein the addition-type silicone potting compound is composed of the following raw materials in parts by weight: Component A 100 to 200 parts vinyl silicone oil 5 to 70 parts of hydrogen-containing silicone oil 20 to 80 parts of hollow glass microspheres Inhibitor 0.01-0.05 parts; Component B 150 to 300 parts vinyl silicone oil 5 to 10 parts of dimethyl silicone oil 20 to 60 parts of hollow glass microspheres Coupling agent 2.5 parts to 6.5 parts 0.5 to 3 parts of phenolic resin-coated platinum catalyst 3 to 10 parts isopropanol.
[0016] The preparation method of addition-type silicone potting compound is as follows: (1) Add the weight proportions of vinyl silicone oil, hydrogen-containing silicone oil, hollow glass microspheres and inhibitor to a double planetary mixer and mix at a speed of 20-40 Hz for 5-10 min; turn on the vacuum and stir at 20-40 Hz for 20-30 min under vacuum conditions of 0.09±0.05 MPa; discharge the adhesive into a packaging bottle to complete the preparation of component A. (2) Add the weight proportions of vinyl silicone oil, dimethyl silicone oil, hollow glass microspheres, coupling agent, and phenolic resin-coated platinum catalyst to a double planetary mixer and stir at a speed of 20-40 Hz for 5-10 min; turn on the vacuum and stir at 20-40 Hz for 20-30 min under vacuum conditions of 0.09±0.05 MPa, and then discharge the gel into a packaging bottle to complete the preparation of component B.
[0017] The phenolic resin described in this invention is selected as a thermosetting phenolic resin with a viscosity of 12S to 500S and a solid content of 40% to 60%; the vinyl silicone oil is selected with a vinyl molar content of 0.10 to 0.50 mmol / g and a viscosity of 100 to 1000 cp; the hydrogen-containing silicone oil is selected with a hydrogen content of 0.1% to 1.5% and a viscosity of 30 to 300 cp; the hollow glass microspheres are selected with a true density of 0.12 to 0.70 g / cm³. 3 The particle size is 5-100 μm; the inhibitor is an unsaturated compound inhibitor, such as alkynol, vinyl siloxane, maleic acid and its derivatives, fumaric acid and its derivatives; dimethyl silicone oil with a viscosity of 200-1000 cp; the coupling agent is selected from at least one of silane coupling agents with vinyl, epoxy and methylpropylvinyloxy groups.
[0018] This invention employs phenolic resin-coated platinum catalyst to avoid the influence of substances on the surface of hollow glass microspheres on the platinum catalyst, effectively slowing down the curing decay of addition-type silicone potting compounds. The phenolic resin-coated platinum catalyst has a particle size of 150μm-200μm. Phenolic resin is characterized by high strength and brittleness, preventing breakage during stirring and premature leaching of the platinum catalyst. Simultaneously, during transport via a gear pump, the interaction of the gears can break up larger-diameter phenolic resin microspheres, ensuring uniform dispersion of the platinum catalyst in the adhesive. The micron-sized phenolic resin-coated platinum catalyst is easily and uniformly dispersed. After emulsification in water, the phenolic resin forms a water-in-oil emulsion, which solidifies into spheres after high-temperature curing. This method results in high sphericity, high sphericity, and uniform particle size. Compared to existing microencapsulated platinum catalysts, this invention reduces the amount of platinum catalyst used in the preparation of addition-type silicone potting compounds, ensuring product stability. The microencapsulated platinum catalyst of this invention is suitable for addition-type silicone potting compounds that cure within various temperature ranges. Detailed Implementation
[0019] Example 1 The phenolic resin-coated platinum catalyst of this embodiment contains the following raw materials in parts by weight: 80 parts phenolic resin, 4 parts foaming agent n-pentane, 1.5 parts surfactant fatty alcohol polyoxypropylene ether, 0.3 parts platinum complex Karstedt catalyst, 10 parts isopropanol, 0.5 parts catalyst benzenesulfonic acid, and 160 parts water.
[0020] Example 2 The phenolic resin-coated platinum catalyst of this embodiment contains the following raw materials in parts by weight: 140 parts phenolic resin, 12 parts foaming agent n-pentane, 6.5 parts surfactant fatty alcohol polyoxyethylene, 0.4 parts platinum complex Karstedt catalyst, 25 parts isopropanol, 3 parts catalyst oxalic acid, and 300 parts water.
[0021] Example 3 The phenolic resin-coated platinum catalyst of this embodiment contains the following raw materials in parts by weight: 200 parts phenolic resin, 20 parts foaming agent dichloromethane, 12 parts surfactant polysiloxane, 0.5 parts platinum complex Karstedt catalyst, 40 parts isopropanol, 5 parts catalyst adipic acid, and 400 parts water.
[0022] Example 4 This embodiment is a method for preparing the phenolic resin-coated platinum catalyst of Example 1, including the following steps: (1) 40 parts by weight of phenolic resin, 4 parts by weight of foaming agent n-pentane, 1.5 parts by weight of surfactant fatty alcohol polyoxypropylene ether, and 0.25 parts by weight of catalyst benzenesulfonic acid are added to a disperser, the stirring speed is set to 1000 r / min, and the stirring time is 15 min; then 160 parts by weight of water are added, the stirring speed is set to 3000 r / min, and the stirring time is 3 h; then the temperature is heated to 100℃, the stirring speed is set to 1000 r / min, and the stirring time is 4 h; the mixture is filtered, dried, and passed through an 80-mesh sieve to obtain phenolic resin microspheres; (2) Add 0.3 parts by weight of platinum complex Karstedt catalyst and 5 parts by weight of isopropanol to a disperser, set the stirring speed to 500 r / min and the stirring time to 15 min to obtain a platinum complex mixture; (3) The platinum complex mixture was evenly sprayed onto the surface of the phenolic resin microspheres and left to stand for 1 hour to obtain phenolic resin microspheres coated with platinum complex. (4) Add 40 parts by weight of phenolic resin, 0.25 parts by weight of catalyst and 5 parts by weight of isopropanol to a disperser, set the stirring speed to 1000 r / min and the stirring time to 15 min to obtain a phenolic resin mixture. (5) Platinum complex-coated phenolic resin microspheres are placed in a spray tower. During the airflow stirring process, the phenolic resin mixture is uniformly coated on the surface of the platinum complex-coated phenolic resin microspheres. During the high-speed airflow stirring process, the temperature is raised to 100°C and the stirring time is 1 hour. The mixture is then passed through a 70-mesh sieve to obtain the phenolic resin-coated platinum catalyst.
[0023] Example 5 This embodiment is the preparation method of the phenolic resin coated platinum catalyst of Example 2, including the following steps: (1) 70 parts by weight of phenolic resin, 12 parts by weight of foaming agent n-pentane, 6.5 parts by weight of surfactant fatty alcohol polyoxyethylene, and 1.5 parts by weight of catalyst oxalic acid are added to a disperser, the stirring speed is set to 1500 r / min, and the stirring time is 12 min; then 300 parts by weight of water are added, the stirring speed is set to 4000 r / min, and the stirring time is 2 h; then the temperature is heated to 100℃, the stirring speed is set to 1500 r / min, and the stirring time is 3 h; the mixture is filtered, dried, and passed through an 80-mesh sieve to obtain phenolic resin microspheres; (2) Add 0.4 parts by weight of platinum complex Karstedt catalyst and 13 parts by weight of isopropanol to a disperser, set the stirring speed to 650 r / min and the stirring time to 12 min to obtain a platinum complex mixture. (3) The platinum complex mixture was evenly sprayed onto the surface of the phenolic resin microspheres and left to stand for 1 hour to obtain phenolic resin microspheres coated with platinum complex. (4) Add 70 parts by weight of phenolic resin, 1.5 parts by weight of catalyst, and 12 parts by weight of isopropanol to a disperser, set the stirring speed to 1500 r / min, and the stirring time to 12 min to obtain a phenolic resin mixture; (5) Platinum complex-coated phenolic resin microspheres are placed in a spray tower. During the airflow stirring process, the phenolic resin mixture is uniformly coated on the surface of the platinum complex-coated phenolic resin microspheres. During the high-speed airflow stirring process, the temperature is raised to 110°C and the stirring time is 1 hour. The mixture is then passed through a 70-mesh sieve to obtain the phenolic resin-coated platinum catalyst.
[0024] Example 6 This embodiment is the preparation method of the phenolic resin coated platinum catalyst of Example 3, including the following steps: (1) 100 parts by weight of phenolic resin, 20 parts by weight of foaming agent dichloromethane, 12 parts by weight of surfactant polysiloxane, and 2.5 parts by weight of catalyst adipic acid are added to a disperser, the stirring speed is set to 2000 r / min, and the stirring time is 10 min; then 400 parts by weight of water are added, the stirring speed is set to 5000 r / min, and the stirring time is 1 h; then the temperature is heated to 100℃, the stirring speed is set to 2000 r / min, and the stirring time is 2 h; the mixture is filtered, dried, and passed through an 80-mesh sieve to obtain phenolic resin microspheres; (2) Add 0.5 parts by weight of platinum complex Karstedt catalyst and 20 parts by weight of isopropanol to a disperser, set the stirring speed to 800 r / min and the stirring time to 10 min to obtain a platinum complex mixture; (3) The platinum complex mixture was evenly sprayed onto the surface of the phenolic resin microspheres and left to stand for 1 hour to obtain phenolic resin microspheres coated with platinum complex. (4) Add 100 parts by weight of phenolic resin, 2.5 parts by weight of catalyst, and 20 parts by weight of isopropanol to a disperser. Set the stirring speed to 2000 r / min and the stirring time to 10 min to obtain a phenolic resin mixture. (5) Platinum complex-coated phenolic resin microspheres are placed in a spray tower. During the airflow stirring process, the phenolic resin mixture is uniformly coated on the surface of the platinum complex-coated phenolic resin microspheres. During the high-speed airflow stirring process, the temperature is raised to 120°C and the stirring time is 1 hour. The mixture is then passed through a 70-mesh sieve to obtain the phenolic resin-coated platinum catalyst.
[0025] Example 7 This embodiment illustrates the application of the phenolic resin-coated platinum catalyst from Example 1 in the preparation of addition-type organosilicon potting compounds.
[0026] The specific addition-type silicone potting compound is composed of the following raw materials in parts by weight: Component A: 100 parts vinyl silicone oil, 28 parts hydrogen-containing silicone oil, 0.01 parts inhibitor alkoxyhydroacetyl alcohol, and 20 parts hollow glass microspheres; wherein, the vinyl silicone oil has a vinyl molar content of 0.37 mmol / g, the hydrogen content of the hydrogen-containing silicone oil is 0.36%, and the viscosity is 30 cp; the true density of the hollow glass microspheres is (0.27~0.30) g / cm³. 3 Particle size D90: 65μm; Component B: 150 parts vinyl silicone oil, 5 parts dimethyl silicone oil, 20 parts hollow glass microspheres, 2.5 parts coupling agent KH560, 0.5 parts phenolic resin-coated platinum catalyst, and 3 parts isopropanol.
[0027] Example 8 This embodiment illustrates the application of the phenolic resin-coated platinum catalyst from Example 2 in the preparation of addition-type organosilicon potting compounds.
[0028] The specific addition-type silicone potting compound is composed of the following raw materials in parts by weight: Component A: 190 parts vinyl silicone oil, 24 parts hydrogen-containing silicone oil, 0.03 parts inhibitor alkoxyhydroacetyl alcohol, and 30 parts hollow glass microspheres; wherein, the vinyl silicone oil has a viscosity of 350 cp; the vinyl molar content is 0.19 mmol / g; the hydrogen content of the hydrogen-containing silicone oil is 0.36%; 22 parts have a viscosity of 30 cp and a hydrogen content of 0.8%; and 2 parts have a viscosity of 50 cp; the true density of the hollow glass microspheres is (0.27~0.30) g / cm³. 3 Particle size D90: 65μm; Component B: 220 parts vinyl silicone oil, 10 parts dimethyl silicone oil, 30 parts hollow glass microspheres, 4 parts coupling agent KH560, 1.8 parts phenolic resin-coated platinum catalyst, and 7 parts isopropanol.
[0029] Example 9 This embodiment illustrates the application of the phenolic resin-coated platinum catalyst from Example 3 in the preparation of addition-type silicone potting compounds.
[0030] The specific addition-type silicone potting compound is composed of the following raw materials in parts by weight: Component A: 190 parts vinyl silicone oil, 24 parts hydrogen-containing silicone oil, 0.05 parts alkoxyhydroacetyl alcohol inhibitor, and 80 parts hollow glass microspheres; wherein, the vinyl silicone oil has a viscosity of 350 cp; the vinyl molar content is 0.19 mmol / g; the hydrogen content of the hydrogen-containing silicone oil is 0.36%; 22 parts have a viscosity of 30 cp and a hydrogen content of 0.8%; and 2 parts have a viscosity of 50 cp; the true density of the hollow glass microspheres is (0.58~0.62) g / cm³. 3 Particle size D90: 65μm; Component B: 220 parts vinyl silicone oil, 10 parts dimethyl silicone oil, 60 parts hollow glass microspheres, 4 parts coupling agent KH560, 3 parts phenolic resin-coated platinum catalyst, and 10 parts isopropanol.
[0031] Example 10 This embodiment describes the preparation method of the addition-type silicone potting compound of Example 7, specifically including the following steps: (1) Add the weight proportions of vinyl silicone oil, hydrogen-containing silicone oil, hollow glass microspheres and inhibitor to a double planetary mixer and stir at 20 Hz for 10 min; turn on the vacuum and stir at 20 Hz for 30 min under vacuum conditions with a vacuum degree of 0.05 MPa, and discharge the glue into the packaging bottle to complete the preparation of component A. (2) Add the weight proportions of vinyl silicone oil, dimethyl silicone oil, hollow glass microspheres, coupling agent, and phenolic resin-coated platinum catalyst to a double planetary mixer and stir at 20 Hz for 10 min; turn on the vacuum and stir at 20 Hz for 30 min under vacuum conditions with a vacuum degree of 0.05 MPa, and discharge the gel into a packaging bottle to complete the preparation of component B.
[0032] Example 11 This embodiment describes the preparation method of the addition-type silicone potting compound of Example 8, specifically including the following steps: (1) Add the weight proportions of vinyl silicone oil, hydrogen-containing silicone oil, hollow glass microspheres and inhibitor to a double planetary mixer and mix at a speed of 30 Hz for 12 min; turn on the vacuum and stir at 30 Hz for 20 min under vacuum conditions with a vacuum degree of 0.09 MPa, and discharge the glue into the packaging bottle to complete the preparation of component A. (2) Add the weight proportions of vinyl silicone oil, dimethyl silicone oil, hollow glass microspheres, coupling agent, and phenolic resin-coated platinum catalyst to a double planetary mixer and stir at 30 Hz for 12 min; turn on the vacuum and stir at 30 Hz for 20 min under vacuum conditions with a vacuum degree of 0.09 MPa, and discharge the gel into a packaging bottle to complete the preparation of component B.
[0033] Example 12 This embodiment describes the preparation method of the addition-type silicone potting compound of Example 9, specifically including the following steps: (1) Add the weight proportions of vinyl silicone oil, hydrogen-containing silicone oil, hollow glass microspheres and inhibitor to a double planetary mixer and stir at 40 Hz for 10 min; turn on the vacuum and stir at 40 Hz for 10 min under vacuum conditions with a vacuum degree of 0.14 MPa, and discharge the glue into the packaging bottle to complete the preparation of component A. (2) Add the weight proportions of vinyl silicone oil, dimethyl silicone oil, hollow glass microspheres, coupling agent, and phenolic resin-coated platinum catalyst to a double planetary mixer and stir at 40 Hz for 10 min; turn on the vacuum and stir at 40 Hz for 10 min under vacuum conditions with a vacuum degree of 0.14 MPa, and discharge the gel into a packaging bottle to complete the preparation of component B.
[0034] Comparative Example 1: The method for preparing encapsulated platinum catalysts includes the following steps: (1) Add 146g of methyl silicone resin and 14g of vinylsiloxane to 730g of toluene, stir for 1h, then add 27g of platinum catalyst, and continue stirring for 1h to obtain a mixture. Then, place the mixture in a gas flow rate of 1m³ / h. 3 Drying under nitrogen at a rate of / min yielded a platinum catalyst coated with thermoplastic resin. (2) Add 57g of acrylic resin to 120g of water and mix for 20min at a stirring speed of 200r / min to obtain an acrylic resin mixture. Heat the acrylic resin mixture to 70℃, add 7g of sodium hydroxide, and stir at 80℃ for 1h to obtain an acrylic resin coating. (3) The acrylic resin coating obtained in step (2) is applied to the surface of the platinum catalyst coated with siloxane obtained in step (1), and then cured at 50°C for 3 hours to obtain the capsule-type platinum catalyst.
[0035] The addition-type silicone potting compound in this comparative example has the following raw material parts by weight: The composition includes 100 parts vinyl silicone oil, 28 parts hydrogen-containing silicone oil, 0.01 parts alkoxyhydroacetyl alcohol inhibitor, and 20 parts hollow glass microspheres; wherein the vinyl silicone oil has a vinyl molar content of 0.37 mmol / g, the hydrogen content of the hydrogen-containing silicone oil is 0.36%, and the viscosity is 30 cp; the true density of the hollow glass microspheres is (0.27~0.30) g / cm³. 3 Particle size D90: 65μm; Component B: 150 parts vinyl silicone oil, 5 parts dimethyl silicone oil, 20 parts hollow glass microspheres, 2.5 parts coupling agent KH560, 3 parts encapsulated platinum catalyst, and 3 parts isopropanol.
[0036] Comparative Example 2: The platinum catalyst was prepared by dissolving 0.3g of commercially available Karstedt catalyst in 100g of isopropanol.
[0037] The addition-type silicone potting compound in this comparative example has the following raw material parts by weight: Component A: 190 parts vinyl silicone oil, 24 parts hydrogen-containing silicone oil, 0.05 parts alkoxyhydroacetyl alcohol inhibitor, and 80 parts hollow glass microspheres; wherein, the vinyl silicone oil has a viscosity of 350 cp; the vinyl molar content is 0.19 mmol / g; the hydrogen content of the hydrogen-containing silicone oil is 0.36%; 22 parts have a viscosity of 30 cp and a hydrogen content of 0.8%; and 2 parts have a viscosity of 50 cp; the true density of the hollow glass microspheres is (0.58~0.62) g / cm³. 3 Particle size D90: 65μm; Component B: 220 parts vinyl silicone oil, 10 parts dimethyl silicone oil, 60 parts hollow glass microspheres, 4 parts coupling agent KH560, 0.8 parts platinum catalyst, and 10 parts isopropanol.
[0038] Experimental example: Curing experiment: The addition-type silicone potting compound components A and B were mixed and tested after being delivered by a gear pump.
[0039] The phenolic resin-coated platinum catalyst in Example 1 of this invention has a particle size of 170μm-190μm and a breakage rate of 95% under 10MPa pressure. The prepared addition-type silicone potting compound has a viscosity doubling time of 20 min and a viscosity loss time of 40 min at the time of preparation. After one month of storage, the viscosity doubling time is 19 min and the viscosity loss time is 38 min.
[0040] The phenolic resin-coated platinum catalyst in Example 2 of this invention has a particle size of 150μm-170μm and a breakage rate of 94% under 10MPa pressure. The resulting addition-type silicone potting compound has a viscosity doubling time of 18 min and a viscosity loss time of 37 min at the time of preparation. After one month of storage, the viscosity doubling time is 19 min and the viscosity loss time is 38 min.
[0041] The phenolic resin-coated platinum catalyst in Example 3 of this invention has a particle size of 180μm-200μm and a breakage rate of 97% under 10MPa pressure. The resulting addition-type silicone potting compound has a viscosity doubling time of 16 min and a viscosity loss time of 34 min at the time of preparation. After one month of storage, the viscosity doubling time is 17 min and the viscosity loss time is 35 min.
[0042] The encapsulated platinum catalyst of Comparative Example 1 had a particle size of 270 μm-320 μm and a breakage rate of 5% under 10 MPa pressure. The addition-type silicone potting compound prepared in Comparative Example 1 had a viscosity doubling time of 300 min and a viscosity loss time of 72 h at the time of preparation. After one month of storage, the viscosity doubling time was 220 min and the viscosity loss time was 48 h.
[0043] The addition-type silicone potting compound of Comparative Example 2 had a viscosity doubling time of 11 min and a loss of tack time of 27 min when it was made. After one month of storage, the viscosity doubling time was 50 min and the loss of tack time was 108 min.
[0044] Compared to the comparative example, the curing time of this invention during production is more suitable for the product's construction requirements. In particular, after one month of storage, the product's curing does not decline, and the resulting product has good stability.
Claims
1. A phenol formaldehyde resin-coated platinum catalyst characterized by: The raw materials contain the following parts by weight: 80 to 200 parts of phenolic resin, 4 to 20 parts of foaming agent, 1.5 to 12 parts of surfactant, 0.3 to 0.5 parts of platinum complex, 10 to 40 parts of isopropanol, 0.5 to 5 parts of catalyst, and 160 to 400 parts of water. It is prepared by the following steps: (1) Mix the foaming agent, surfactant, catalyst and half the weight of phenolic resin, stir, add water while stirring, heat to 100-120℃, filter, dry, and sieve to obtain phenolic resin microspheres. (2) Mix the platinum complex and isopropanol, stir, and obtain a platinum complex mixture; (3) Spray the platinum complex mixture from step (2) evenly onto the surface of the phenolic resin microspheres from step (1), and let it stand for 0.5-1.5 hours to obtain phenolic resin microspheres coated with platinum complex. (4) Mix the other half of the phenolic resin with the catalyst and isopropanol, and stir to obtain a phenolic resin mixture; (5) Place the phenolic resin microspheres coated with the platinum complex from step (3) into a spray tower. During the stirring process, uniformly coat the phenolic resin mixture from step (4) onto the surface of the phenolic resin microspheres coated with the platinum complex. During the high-speed stirring process of the airflow, raise the temperature to 100-120°C, stir, and sieve to obtain the phenolic resin coated platinum catalyst.
2. The phenolic resin-coated platinum catalyst of claim 1, wherein: The foaming agent is one of dichloromethane, n-pentane, or a combination thereof.
3. The phenolic resin-coated platinum catalyst of claim 1, wherein: The surfactant is at least one of fatty alcohol polyoxyethylene, fatty alcohol polyoxypropylene ether; or alkylphenol polyoxyethylene ether; or block copolymer of polysiloxane, polyoxyethylene, and polyoxypropylene.
4. The phenolic resin-coated platinum catalyst of claim 1, wherein: The catalyst is one or any combination of oxalic acid, adipic acid, benzene nitric acid, phenolic nitric acid, toluene sulfonic acid, benzene sulfonic acid, and petroleum sulfonate.
5. The phenolic resin-coated platinum catalyst of claim 1, wherein: The platinum complex is a Karstedt catalyst.
6. The phenolic resin-coated platinum catalyst of claim 1, wherein: The isopropanol mentioned is of analytical grade.
7. A method of making a phenolic resin-coated platinum catalyst, characterized by: Includes the following steps: (1) Mix the foaming agent, surfactant, catalyst and half the weight of phenolic resin, stir, add water while stirring, heat to 100-120℃, filter, dry, and sieve to obtain phenolic resin microspheres. (2) Mix the platinum complex and isopropanol, stir, and obtain a platinum complex mixture; (3) Spray the platinum complex mixture from step (2) evenly onto the surface of the phenolic resin microspheres from step (1), and let it stand for 0.5-1.5 hours to obtain phenolic resin microspheres coated with platinum complex. (4) Mix the other half of the phenolic resin with the catalyst and isopropanol, and stir to obtain a phenolic resin mixture; (5) Place the phenolic resin microspheres coated with the platinum complex from step (3) into a spray tower. During the stirring process, uniformly coat the phenolic resin mixture from step (4) onto the surface of the phenolic resin microspheres coated with the platinum complex. During the high-speed stirring process of the airflow, raise the temperature to 100-120°C, stir, and sieve to obtain the phenolic resin coated platinum catalyst.
8. The method of making a phenolic resin-coated platinum catalyst of claim 7, wherein: The specific process of step (1) is as follows: Phenolic resin, foaming agent, surfactant and catalyst are added to a disperser, the stirring speed is set to 1000r / min-2000r / min, the stirring time is 10min-15min, then water is added, the stirring speed is set to 3000r / min-5000r / min, the stirring time is 1h-3h, then the temperature is heated to 100℃, the stirring speed is set to 1000r / min-2000r / min, the stirring time is 2h-4h; filter, dry, and sieve through an 80-mesh sieve to obtain phenolic resin microspheres.
9. The application of a phenolic resin-coated platinum catalyst as described in any one of claims 1-6 in an addition-type silicone potting compound.
10. An addition-type silicone sealant comprising the phenolic resin-coated platinum catalyst according to any one of claims 1 to 6, characterized by: It consists of the following raw materials in parts by weight: Component A 100 to 200 parts vinyl silicone oil 5 to 70 parts of hydrogen-containing silicone oil 20 to 80 parts of hollow glass microspheres Inhibitor 0.01 to 0.05 parts; Component B 150 to 300 parts vinyl silicone oil 5 to 10 parts of dimethyl silicone oil 20 to 60 parts of hollow glass microspheres Coupling agent 2.5 parts to 6.5 parts 0.5 to 3 parts of phenolic resin-coated platinum catalyst 3 to 10 parts isopropanol.
Citation Information
Patent Citations
Capsule type platinum catalyst and preparation method thereof
CN114797994A
Phenolic foam and composition and method for preparing the same
US4444912A