A nuclear power plant dispersed fuel pellet and its preparation method
By coating the surface of high-uranium-density fuel microspheres with an isolation layer and a matrix layer, the problems of high-uranium-density fuel pellets being prone to reaction and unevenly dispersed at high temperatures are solved, thereby improving the safety and stability of nuclear power plant fuel.
Patent Information
- Application Number
- CN202311731764.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-15
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-12-15
AI Technical Summary
Existing high-uranium-density fuel pellets are prone to react with coolant in the event of cladding failure, leading to breakage and leakage of radioactive materials, which affects reactor safety. Furthermore, existing improvement methods have problems such as reduced fuel consumption, chemical reaction risks, or uneven dispersion.
An isolation layer and a matrix layer are coated on the surface of high uranium density fuel microspheres. The isolation layer is made of V, Nb, Ta, Cr, Mo, W or CrN, and the matrix layer is UO2. Dense dispersed fuel pellets are formed through heat treatment and sintering.
This achieved uniform dispersion of high uranium density fuel and improved high-temperature oxidation resistance, avoiding chemical reactions and crack formation, and enhancing the safety and stability of fuel pellets.
Smart Images

Figure CN117854755B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of nuclear fuel technology, and in particular to a dispersed fuel pellet for nuclear power plants and its preparation method. Background Technology
[0002] Among the many candidates for accident-tolerant fuel (ATF) to replace uranium dioxide (UO2) fuel currently used in commercial reactors, high-uranium-density fuels such as uranium silicide (U3Si2), uranium nitride (UN), uranium carbide (UC), and uranium boride (UB2) all have poor high-temperature oxidation resistance. In the event of an accident with cladding failure, high-uranium-density fuel pellets are prone to react with the coolant, leading to pellet breakage and leakage of radioactive materials into the primary circuit, affecting reactor safety. To obtain high-uranium-density fuel that meets service requirements, the nuclear fuel industry currently improves high-uranium-density fuel mainly through four methods: 1) By doping with corrosion-resistant materials or fuel, especially by having the corrosion-resistant materials occupy the grain boundaries of the high-uranium-density fuel, the corrosion resistance of the high-uranium-density fuel is improved (see patents US20110206174A1 and US20190237206A1); 2) By coating the surface of the high-uranium-density fuel particles with corrosion-resistant materials or fuel coatings, the coating can be UO2 (see patents US11062810B2 and US20190074095A1); 3) In the core... The surface of the block is wrapped with a waterproof layer, which can also be a flammable and toxic layer, see patents US10803999B2, US20190139654A1, US20210202116A1, US20210020321A1; 4) High uranium density fuel is made into microspheres and dispersed in a ceramic / metal fuel matrix to form a dispersed structure, see patents US20200168351A1, US20200234833A1, CN112992390A, CN113012827A, CN113035385A.
[0003] However, the first method involves adding corrosion-resistant materials and fuel that occupy some space of the high-uranium-density fuel, affecting the uranium load of the fuel pellets. Furthermore, some high-uranium-density fuel remains exposed on the outer layer of the pellets, failing to completely isolate it from the coolant. The second method suffers from the potential for chemical reactions between the high-uranium-density fuel particles and the corrosion-resistant materials or fuel coating (UO2) covering their surface. The third method results in rapid cracking of the pellets due to thermal stress during operation, and the waterproof layer covering the pellet surface cannot completely isolate it from the coolant after cracking. The fourth method suffers from uneven microsphere dispersion and the potential for chemical reactions between the high-uranium-density fuel microspheres and the matrix. Summary of the Invention
[0004] The technical problem to be solved by the present invention is to provide a nuclear power plant dispersed fuel pellet and a method for preparing the same.
[0005] The technical solution adopted by the present invention to solve its technical problem is: a nuclear power plant dispersed fuel pellet, comprising a plurality of high uranium density fuel microspheres, an isolation layer covering the surface of each high uranium density fuel microsphere, and a substrate layer covering the surface of the isolation layer; the raw material of the isolation layer is solidified on the surface of the high uranium density fuel microspheres by heat treatment;
[0006] The raw materials for the isolation layer are V, Nb, Ta, Cr, Mo, W or CrN, and the raw material for the matrix layer is UO2; the dispersed fuel pellets for nuclear power plants include: 10-50 parts by weight of high uranium density fuel microspheres, 1-15 parts by weight of raw materials for the isolation layer, and 50-200 parts by weight of raw materials for the matrix layer.
[0007] Preferably, the particle size of the raw material in the isolation layer is less than 10 μm; and / or, the average thickness of the isolation layer is 10-50 μm.
[0008] Preferably, the high uranium density fuel microspheres are UN, UC, UB2 or U3Si2; and / or, the particle size of the high uranium density fuel microspheres is 600-1000 μm.
[0009] Preferably, the average thickness of the substrate layer is 100-1500 μm.
[0010] A method for preparing the above-mentioned dispersed fuel pellets for nuclear power plants includes the following steps:
[0011] S1. First coating: Take 10-50 parts by weight of high uranium density fuel microspheres, spray adhesive onto the surface of the high uranium density fuel microspheres, and at the same time coat the surface of the high uranium density fuel microspheres with 1-15 parts by weight of the material of the isolation layer to obtain fuel microspheres with one coating.
[0012] S2. Heat treatment: Heat treatment is performed on the fuel microspheres that have been coated once in a vacuum environment or under a protective gas.
[0013] S3, Second coating: Coat the surface of the fuel microspheres coated in step S2 with 50-200 parts by weight of the matrix layer material to obtain the fuel microspheres with secondary coating; place the fuel microspheres with secondary coating in a mold and press them to obtain fuel pellet blanks;
[0014] S4. Sintering treatment: The fuel pellet blanks are sintered in a vacuum environment, under protective gas or reducing gas to obtain dispersed fuel pellets for nuclear power plants.
[0015] Preferably, in step S1, the adhesive is prepared by mixing polyvinyl alcohol and water in a volume ratio of 1:(40-60), or the adhesive is prepared by dissolving paraffin in carbon tetrachloride in a molar ratio of 1:(3-5).
[0016] Preferably, in step S2, heat treatment is performed in a vacuum environment or under a protective gas, with a heating temperature of 900-1300℃ and a heating time of 0.8-1.2h.
[0017] Preferably, in step S3, the pressing pressure is 100-500 MPa.
[0018] Preferably, in step S4, sintering is performed in a vacuum environment, under a protective gas or a reducing gas, and the sintering method is hot pressing sintering or spark plasma sintering. The sintering temperature is 1800-2200℃, the sintering time is 8-12min, and the sintering pressure is 25-35MPa.
[0019] Preferably, the protective gas is argon, helium, or nitrogen, and the reducing gas is a mixture of an inert gas and hydrogen, or a mixture of an inert gas and carbon monoxide, wherein the inert gas is argon or helium.
[0020] The beneficial effects of this invention are:
[0021] The nuclear power plant dispersed fuel pellets of the present invention have an isolation layer between the matrix layer and the high uranium density fuel microspheres to prevent chemical reactions that may occur when the high uranium density fuel microspheres come into contact with the raw material UO2 in the matrix layer. The isolation layer and the matrix layer are sequentially coated on the surface of the high uranium density fuel microspheres, so that the high uranium density fuel microspheres can be uniformly dispersed in the raw material of the matrix layer. This solves the problems of uneven microsphere dispersion and potential chemical reactions between the high uranium density fuel microspheres and the matrix in dispersed fuels, thereby solving the problem of poor high-temperature oxidation resistance of high uranium density fuels.
[0022] This invention produces uniform and dense dispersed fuel pellets for nuclear power plants. By coating with an isolation layer, the high-uranium density fuel microspheres are prevented from reacting with the substrate layer. By heat-treating the high-uranium density fuel microspheres coated with the isolation layer, the raw material of the isolation layer is prevented from falling into the raw material of the substrate layer during the second coating process. The second coating process coats the surface of the high-uranium density fuel microspheres with the raw material of the substrate layer, thus solving the problem of uneven distribution of high-uranium density fuel microspheres in dispersed fuel pellets. Attached Figure Description
[0023] The present invention will be further described below with reference to the accompanying drawings and embodiments. In the accompanying drawings:
[0024] Figure 1 This is a scanning electron microscope image of a nuclear power plant dispersed fuel pellet from Embodiment 1 of the present invention. Detailed Implementation
[0025] To provide a clearer understanding of the technical features, objectives, and effects of this invention, the invention will be further described in detail below with reference to embodiments. These embodiments are only used to explain the invention and do not constitute a limitation on the scope of protection of this invention.
[0026] A nuclear power plant dispersed fuel pellet includes a plurality of high-uranium-density fuel microspheres, an isolation layer covering the surface of each high-uranium-density fuel microsphere, and a substrate layer covering the surface of the isolation layer. The raw material of the isolation layer is solidified on the surface of the high-uranium-density fuel microspheres through heat treatment. The number of high-uranium-density fuel microspheres can be selected according to actual needs, and this invention does not limit this number.
[0027] The high-uranium-density fuel microspheres are made of UN (uranium nitride), UC (uranium carbide), UB2 (uranium boride), or U3Si2 (uranium silicide). The particle size of the high-uranium-density fuel microspheres is 600-1000 μm, specifically, the particle size can be selected as 600 μm, 700 μm, 800 μm, 900 μm, or 1000 μm.
[0028] The raw materials for the isolation layer are V (vanadium), Nb (niobium), Ta (tantalum), Cr (chromium), Mo (molybdenum), W (tungsten), or CrN (chromium nitride). The particle size of the raw materials for the isolation layer is less than 10 μm, and this particle size is not specifically limited, as long as it is less than 10 μm. The isolation layer should not be too thick, and the average thickness of the isolation layer is 10-50 μm. Specifically, the average thickness of the isolation layer can be selected from 10 μm, 20 μm, 30 μm, 40 μm, and 50 μm. The average thickness of the isolation layer can be selected according to the particle size of the high uranium density fuel microspheres and the actual requirements for the isolation effect. An average thickness of 10-50 μm is sufficient, and this invention does not impose a specific limitation. If the actual thickness of the isolation layer is within the range of the selected average thickness ± 5 μm, the thickness of the isolation layer can be considered uniform. In some embodiments, the raw materials for the isolation layer may also be composed of at least one of V, Nb, Ta, Cr, Mo, W, and CrN.
[0029] The raw material for the substrate layer is UO2. The substrate layer should not be too thick, and its average thickness is 100-1500 μm. Specifically, the average thickness of the substrate layer can be selected from 100 μm, 300 μm, 500 μm, 800 μm, 1000 μm, 1200 μm, and 1500 μm. The average thickness of the substrate layer can be selected based on the actual requirements of the particle size of the high-uranium density fuel microspheres and the weight fraction of the raw material in the substrate layer. An average thickness of 100-1500 μm is sufficient, and this invention does not impose a specific limitation.
[0030] The dispersed fuel pellets for nuclear power plants consist of: 10-50 parts by weight of high uranium density fuel microspheres, 1-15 parts by weight of buffer material, and 50-200 parts by weight of matrix material. Specifically, the weight percentages of high uranium density fuel microspheres can be 10, 20, 30, 40, or 50 parts; the weight percentages of buffer material can be 1, 3, 5, 7, 9, 12, or 15 parts; and the weight percentages of matrix material can be 50, 60, 70, 80, 90, 100, 120, 150, 180, or 200 parts.
[0031] The nuclear power plant dispersed fuel pellets of this invention feature an isolation layer between the matrix layer and high-uranium-density fuel microspheres to prevent potential chemical reactions between the high-uranium-density fuel microspheres and the UO2 raw material in the matrix layer. Two layers of material are coated on the surface of the high-uranium-density fuel microspheres, allowing them to be uniformly dispersed within the raw material in the matrix layer. This solves the problems of uneven microsphere dispersion and potential chemical reactions between the high-uranium-density fuel microspheres and the matrix in dispersed fuels. The double-layer protection of the isolation layer and the matrix layer also addresses the issue of poor high-temperature oxidation resistance of high-uranium-density fuels.
[0032] A method for preparing the above-mentioned dispersed fuel pellets for nuclear power plants includes the following steps:
[0033] S1. First Coating: Take 10-50 parts by weight of high uranium density fuel microspheres, spray an adhesive onto the surface of the high uranium density fuel microspheres, and simultaneously coat the surface of the high uranium density fuel microspheres with 1-15 parts by weight of the material for the isolation layer, thus obtaining fuel microspheres with one coating. The adhesive is made by mixing polyvinyl alcohol and water in a volume ratio of 1:(40-60). The volume ratio of polyvinyl alcohol to water can be selected according to actual needs and is not limited in this invention. Alternatively, the adhesive can be made by dissolving paraffin in carbon tetrachloride in a molar ratio of 1:(3-5). The molar ratio of paraffin to carbon tetrachloride can be selected according to actual needs and is not limited in this invention. The content of the adhesive is not limited; it can be added in appropriate amounts according to actual needs, so that the surface of the high uranium density fuel microspheres can adhere to the material of the isolation layer.
[0034] Before step S1, the high uranium density fuel microspheres can be sieved to obtain high uranium density fuel microspheres with a particle size of 600-1000 μm. The particle size can be selected from 600 μm, 700 μm, 850 μm, 900 μm, and 1000 μm.
[0035] After the first coating process, the surface of the high-uranium density fuel microspheres is covered with the raw material of the isolation layer, with no exposed surface. Before step S2, the coated fuel microspheres are sieved to obtain an isolation layer with an average thickness of 10-50 μm, avoiding an excessively thick isolation layer.
[0036] S2. Heat Treatment: The coated fuel microspheres are heat-treated in a vacuum environment or under a protective gas atmosphere. Specifically, the heat treatment is carried out in a vacuum environment or under a protective gas atmosphere, with a heating temperature of 900-1300℃ and a heating time of 0.8-1.2h. Specifically, the heating temperature can be selected from 900℃, 1000℃, 1100℃, 1200℃, and 1300℃, and the heating time can be selected from 0.8h, 0.9h, 1.0h, 1.1h, and 1.2h.
[0037] After the material for coating the high-uranium density fuel microspheres with the insulating layer is applied, the material in the insulating layer is prone to detachment during the process of coating the substrate layer. This results in uneven thickness of the insulating layer, and some of the material in the insulating layer may disperse into the substrate layer, potentially exposing the surface of the high-uranium density fuel microspheres and affecting the effectiveness of the insulating layer. This invention heat-treats the high-uranium density fuel microspheres coated with the insulating layer material, ensuring that the material in the insulating layer is firmly coated (solidified) on the surface of the high-uranium density fuel microspheres. This prevents the material in the insulating layer from dispersing into the substrate layer during the second coating process, thus enabling the insulating layer to provide better insulation.
[0038] S3. Second Coating: 50-200 parts by weight of the matrix layer material are coated onto the surface of the fuel microspheres coated in step S2 to obtain second-coated fuel microspheres. The second-coated fuel microspheres are then placed in a mold and pressed to obtain a fuel pellet blank. Specifically, the pressing pressure is 100-500 MPa, and can be 100 MPa, 200 MPa, 300 MPa, 400 MPa, or 500 MPa. The mold can be cylindrical, plate-shaped, or other shapes; this invention is not limited to any particular shape.
[0039] Before pressing, the fuel microspheres that have undergone secondary coating are sieved to obtain a matrix layer with an average thickness of 100-1500 μm, in order to avoid the matrix layer being too thick or having uneven thickness.
[0040] S4. Sintering Treatment: The fuel pellet blanks are sintered in a vacuum environment under a protective gas or a reducing gas to obtain dispersed fuel pellets for nuclear power plants. Specifically, sintering is carried out in a vacuum environment under a protective gas or a reducing gas. The sintering method is hot pressing sintering or spark plasma sintering. The sintering temperature is 1800-2200℃, the sintering time is 8-12 min, and the sintering pressure is 25-35 MPa. Specifically, the sintering temperature can be selected from 1800℃, 1900℃, 2000℃, 2100℃, and 2200℃; the sintering time can be selected from 8 min, 9 min, 10 min, 11 min, and 12 min; and the sintering pressure can be selected from 25 MPa, 28 MPa, 30 MPa, 33 MPa, and 35 MPa.
[0041] After pressing in step S3 and sintering in step S4, dense nuclear power plant dispersed fuel pellets are obtained. In this process, the matrix layers of all the secondary coated fuel microspheres are fused together to form the matrix of the fuel pellet, allowing the primary coated fuel microspheres to be evenly distributed in the matrix, i.e., high uranium density fuel microspheres are evenly dispersed in the matrix.
[0042] Both steps S1 and S3 above can be performed using a coating machine. Step S1 is as follows: S1, First coating: Take 10-50 parts by weight of high uranium density fuel microspheres and place them and 1-15 parts by weight of the isolation layer material in the coating machine. The pot of the coating machine rotates, coating the surface of the high uranium density fuel microspheres with the isolation layer material, and simultaneously spraying an adhesive onto the surface of the high uranium density fuel microspheres to obtain fuel microspheres with one coating. Step S3 is as follows: S3, Place the fuel microspheres with one coating from step S2 and 50-200 parts by weight of the matrix layer material in the coating machine. The pot of the coating machine rotates, coating the surface of the fuel microspheres with the matrix layer material to obtain fuel microspheres with two coatings. In addition, steps S1 and S3 can also use existing coating methods to coat the high uranium density fuel microspheres with the isolation layer and the matrix layer, which will not be elaborated here.
[0043] In the heat treatment of step S2 and the sintering treatment of step S4, the protective gas is argon, helium, or nitrogen, and the reducing gas is a mixture of inert gas and hydrogen, or a mixture of inert gas and carbon monoxide, wherein the inert gas is argon or helium. Specifically, the heat treatment can use a heating atmosphere of vacuum, argon, helium, or nitrogen, and the sintering atmosphere of the sintering treatment can use a vacuum, argon, helium, nitrogen, a mixture of argon and hydrogen, a mixture of argon and carbon monoxide, a mixture of helium and hydrogen, or a mixture of helium and carbon monoxide.
[0044] This invention produces uniform and dense dispersed fuel pellets for nuclear power plants. By coating with an isolation layer, the high-uranium density fuel microspheres are prevented from reacting with the substrate layer. By heat-treating the high-uranium density fuel microspheres coated with the isolation layer, the raw material of the isolation layer is prevented from falling into the raw material of the substrate layer during the second coating process. The second coating process coats the surface of the high-uranium density fuel microspheres with the raw material of the substrate layer, thus solving the problem of uneven distribution of high-uranium density fuel microspheres in dispersed fuel pellets.
[0045] The following is an illustration through specific examples:
[0046] The nuclear power plant dispersed fuel pellets of Examples 1 to 3 were prepared using the above-described preparation method of the present invention. The raw materials for the high uranium density fuel microspheres, the isolation layer and the matrix layer are shown in Table 1. The process parameters of the preparation methods corresponding to Examples 1 to 3 are shown in Table 2.
[0047] Table 1. Raw materials for high uranium density fuel microspheres, isolation layers, and substrate layers in Examples 1-3
[0048]
[0049] Table 2. Process parameters of the preparation methods in Examples 1-3
[0050]
[0051]
[0052] The density of the dispersed fuel pellets from nuclear power plants in Examples 1-3 was all higher than 95%. Scanning electron microscopy (SEM) observation of the dispersed fuel pellets from Example 1 yielded the following results: Figure 1 As shown, the thickness of the isolation layer is 10-50 μm. The isolation layer is dense and uniform in thickness. All the secondary coated fuel microspheres are fused together to form the matrix of the fuel pellet, so that the high uranium density fuel microspheres are uniformly dispersed in the matrix.
[0053] It is understood that the above embodiments only illustrate preferred embodiments of the present invention, and their descriptions are relatively specific and detailed, but they should not be construed as limiting the scope of the present invention. It should be noted that those skilled in the art can freely combine the above technical features without departing from the concept of the present invention, and can also make several modifications and improvements, all of which fall within the protection scope of the present invention. Therefore, all equivalent transformations and modifications made with respect to the scope of the claims of the present invention should fall within the scope of the claims of the present invention.
Claims
1. A method for preparing dispersed fuel pellets for nuclear power plants, characterized in that, Includes the following steps: S1. First coating: Take 10-50 parts by weight of high uranium density fuel microspheres, spray adhesive onto the surface of the high uranium density fuel microspheres, and at the same time coat the surface of the high uranium density fuel microspheres with 1-15 parts by weight of the material of the isolation layer to obtain fuel microspheres with one coating. S2. Heat treatment: The one-time coated fuel microspheres are heat-treated in a vacuum environment or under a protective gas atmosphere at a temperature of 900-1300℃ for 0.8-1.2 hours. S3. Second coating: Coat the surface of the fuel microspheres coated in the first coating step in S2 with 50-200 parts by weight of the matrix layer material to obtain the fuel microspheres with a second coating; place the fuel microspheres with a second coating in a mold and press them to obtain fuel pellet blanks; S4. Sintering treatment: The fuel pellet blank is sintered in a vacuum environment, under a protective gas or a reducing gas to obtain nuclear power plant dispersed fuel pellets. The nuclear power plant dispersed fuel pellets include a plurality of high uranium density fuel microspheres, an isolation layer covering the surface of each high uranium density fuel microsphere, and a substrate layer covering the surface of the isolation layer; the raw material of the isolation layer is solidified on the surface of the high uranium density fuel microspheres by heat treatment. The raw material for the isolation layer is V, Nb, Ta, Cr, Mo, W or CrN, and the raw material for the matrix layer is UO2; the nuclear power plant dispersed fuel pellets include: 10-50 parts by weight of the high uranium density fuel microspheres, 1-15 parts by weight of the raw material for the isolation layer, and 50-200 parts by weight of the raw material for the matrix layer.
2. The method for preparing dispersed fuel pellets for nuclear power plants according to claim 1, characterized in that, The raw material particle size of the isolation layer is less than 10 μm; and / or the average thickness of the isolation layer is 10-50 μm.
3. The method for preparing dispersed fuel pellets for nuclear power plants according to claim 1, characterized in that, The high uranium density fuel microspheres are UN, UC, UB2 or U3Si2; and / or, the particle size of the high uranium density fuel microspheres is 600-1000 μm.
4. The method for preparing dispersed fuel pellets for nuclear power plants according to claim 1, characterized in that, The average thickness of the substrate layer is 100-1500 μm.
5. The method for preparing dispersed fuel pellets for nuclear power plants according to claim 1, characterized in that, In step S1, the adhesive is prepared by mixing polyvinyl alcohol and water in a volume ratio of 1:(40-60), or by dissolving paraffin in carbon tetrachloride in a molar ratio of 1:(3-5).
6. The method for preparing dispersed fuel pellets for nuclear power plants according to claim 1, characterized in that, In step S3, the pressing pressure is 100-500 MPa.
7. The method for preparing dispersed fuel pellets for nuclear power plants according to claim 1, characterized in that, In step S4, sintering is performed in a vacuum environment, under a protective gas or a reducing gas. The sintering method is hot pressing sintering or spark plasma sintering. The sintering temperature is 1800-2200℃, the sintering time is 8-12min, and the sintering pressure is 25-35MPa.
8. The method for preparing dispersed fuel pellets for nuclear power plants according to claim 1, characterized in that, The protective gas is argon, helium, or nitrogen, and the reducing gas is a mixture of an inert gas and hydrogen, or a mixture of an inert gas and carbon monoxide, wherein the inert gas is argon or helium.
Citation Information
Patent Citations
High-safety uranium silicide composite fuel pellet
CN112992390A
Water-corrosion-resistant uranium nitride composite fuel pellet
CN113012827A
Boron-containing uranium silicide monolithic burnable poison pellet
CN113035385A
Coated U3Si2 pellets with enhanced water and steam oxidation resistance
US10803999B2
Manufacture of large grain powders with granular coatings
US11062810B2