A high water retention bonding mortar and its preparation method and application
By using materials such as modified polypropylene fiber and water-retaining thickener in the bonding mortar, a cross-linked network structure is formed, which solves the problems of poor water retention and insufficient bonding strength of the bonding mortar in the existing technology, and significantly improves the performance of the mortar. bond strength and durability.
Patent Information
- Application Number
- CN202410116975.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-29
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-01-29
AI Technical Summary
The existing bonding mortar has poor water retention and insufficient bonding strength, resulting in poor construction quality and prone to cracking and falling off problems.
It uses a combination of cement, sand, modified polypropylene fiber and water-retaining thickener to form a cross-linked network structure through materials such as modified metakaolin and carboxymethyl cellulose to improve the viscosity and waterproof performance of the mortar and enhance its adhesion. Knot strength and durability.
Significantly improve the water retention and bonding strength of the mortar, extend the service life, reduce water leakage, enhance the crack resistance and waterproof and anti-seepage capabilities, and improve the overall stability and durability.
Smart Images

Figure CN117886559B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building materials, in particular to a high-water-retaining bonding mortar and a preparation method and application thereof. Background Art
[0002] With the increasing severity of global climate change and energy shortage, green buildings have become an important development direction of the world's construction industry. Green buildings are environmentally friendly, energy-saving and efficient, providing strong support for creating a more livable and sustainable living environment for mankind. Among them, the thermal insulation technology of building envelope structures has become one of the important ways to save energy in buildings in my country. At present, the commonly used building wall insulation method is the insulation board exterior wall insulation system, which uses insulation boards to achieve thermal insulation and energy saving. As an important component of the exterior wall insulation system, the bonding mortar is mainly composed of cement, quartz sand, polymer binder and a variety of additives that are mechanically mixed and uniformly formed. It is used for bonding between walls and insulation boards and has the characteristics of fast curing time. The performance of the bonding mortar directly affects the stability and durability of the entire insulation system.
[0003] Currently, most of the bonding mortars on the market have average bonding strength, poor water retention, and are prone to cracking, which seriously affects the construction quality. Chinese patent CN103449788B discloses an external wall insulation board bonding mortar and a preparation method thereof, wherein the bonding mortar comprises the following raw materials in percentage by weight: 30%-65% of a bonding material, 30%-65% of a fine aggregate, 2%-6% of a polymer binder, 0.1%-0.3% of a thixotropic lubricant and 0.008%-0.012% of an accelerating setting agent, wherein the polymer binder is composed of a dispersible latex, a silicone hydrophobic agent and hydroxypropyl methylcellulose ether. The prepared external wall insulation board bonding mortar has high bonding strength, large bonding force and good waterproof and anti-seepage effects. However, although the use of a hydrophobic agent can improve the waterproof and anti-seepage properties of the bonding mortar, it will also cause the water retention of the mortar to decrease. When the mortar is hydrated, the water loss is relatively fast, resulting in the inability to fully proceed with the hydration, thereby affecting the bonding strength of the mortar, causing the insulation board to easily fall off the wall. Chinese patent application CN116813267A discloses a fast-hardening and fast-setting high-strength bonding mortar for assembled concrete composite wall panels, which is composed of the following components in parts by weight: 38-45 parts of ordinary Portland cement, 32-45 parts of sand and gravel, 10-25 parts of organosilane-modified fly ash, 1-3 parts of redispersible latex powder, 0.2-0.3 parts of polypropylene fiber, 0.3-1 parts of cellulose ether, 0.08-0.15 parts of fast-hardening agent, 0.05-0.1 parts of air-entraining agent, and 0-0.08 parts of water-reducing agent. The bonding mortar has a fast solidification speed, high strength, is not easy to crack, and has good water retention. However, bubbles are easily generated during use, and problems such as cracking and falling off may occur, which affect the overall service life. Summary of the invention
[0004] 1. Technical issues to be solved
[0005] In view of the deficiencies in the prior art, the present invention provides a high water-retention bonding mortar and a preparation method and application thereof, which solves the problems of poor water retention and general bonding strength of the bonding mortar, and prepares a bonding mortar with good durability.
[0006] (II) Technical solution
[0007] In order to achieve the above object, the present invention discloses a high water-retaining bonding mortar, comprising the following raw materials in parts by weight: 40-55 parts of cement, 45-60 parts of sand, 9-14 parts of water-retaining thickener, 3-5 parts of modified polypropylene fiber, 55-75 parts of deionized water and 0.3-0.5 parts of defoamer;
[0008] The water-retaining thickener is prepared from carboxymethyl cellulose, polyethylene glycol, modified metakaolin and acrylic acid;
[0009] The modified polypropylene fiber is prepared from modified metakaolin, polypropylene fiber and vinyl trimethoxysilane;
[0010] The preparation of the metakaolin comprises: firstly modifying the metakaolin with γ-aminopropyltriethoxysilane to obtain aminosilane-modified metakaolin, and then reacting hexadecenylsuccinic anhydride with the aminosilane-modified metakaolin to obtain modified metakaolin.
[0011] Preferably, the defoaming agent is polydimethylsiloxane.
[0012] Furthermore, the modified metakaolin is prepared by specifically comprising the following steps:
[0013] S1, drying metakaolin (MK) in a drying oven at 110° C. for 24 h, then mixing the dried metakaolin and γ-aminopropyltriethoxysilane evenly, and milling them in a ball mill. After the ball milling is completed, aminosilane-modified metakaolin is obtained;
[0014] S2. Ultrasonic disperse the aminosilane-modified kaolin in a mixed solvent of N,N-dimethylformamide and deionized water. After mixing evenly, add hexadecenylsuccinic anhydride, stir and mix to react. After the reaction is completed, wash with anhydrous ethanol and deionized water, filter, and vacuum dry at 60°C for 12 hours to obtain modified kaolin.
[0015] Preferably, in the specific preparation process of modified metakaolin, the mass ratio of the dried metakaolin and γ-aminopropyltriethoxysilane in S1 is 100:6-9.
[0016] Preferably, in the specific preparation process of modified metakaolin, the ball milling time in S1 is 60-90 min.
[0017] Preferably, in the specific preparation process of modified metakaolin, the mass ratio of aminosilane modified metakaolin, mixed solvent and hexadecenyl succinic anhydride in S2 is 100:1600-2000:15-21, wherein the volume ratio of N,N-dimethylformamide and deionized water in the mixed solvent is 9:1.
[0018] Preferably, in the specific preparation process of modified metakaolin, the reaction temperature in S2 is 55-65° C., and the reaction time is 6-8 h.
[0019] Preferably, the water-retaining thickener is prepared by specifically comprising the following steps: mixing carboxymethyl cellulose (CMC) and deionized water evenly, adding polyethylene glycol, stirring and mixing for 30 minutes, adding modified metakaolin and acrylic acid, stirring and mixing, introducing nitrogen, adding a crosslinking agent N,N'-methylenebisacrylamide and an initiator ammonium persulfate in a nitrogen atmosphere, stirring and mixing, reacting, and after the reaction is completed, washing with deionized water and anhydrous ethanol, and vacuum drying at 60°C for 6 hours to obtain a water-retaining thickener.
[0020] Preferably, in the specific preparation process of the water-retaining thickener, the mass ratio of the carboxymethyl cellulose, deionized water, polyethylene glycol, modified metakaolin, acrylic acid, N,N'-methylenebisacrylamide and ammonium persulfate is 100:2500-3000:1-3:1-2:210-350:0.1-0.2:3-5.
[0021] Preferably, in the specific preparation process of the water-retaining thickener, the reaction temperature is 70-80° C., and the reaction time is 45-60 min.
[0022] Preferably, the modified polypropylene fiber is prepared by specifically comprising the following steps: ultrasonically dispersing modified metakaolin in an ethanol aqueous solution, adding polypropylene fiber and vinyltrimethoxysilane after uniform dispersion, mixing evenly, adding an initiator, reacting, and after the reaction is completed, washing with deionized water, filtering, extracting with acetone, and drying in a vacuum drying oven at 60°C for 6 hours to obtain the modified polypropylene fiber.
[0023] Preferably, in the specific preparation process of the modified polypropylene fiber, the mass ratio of the modified metakaolin, ethanol aqueous solution, polypropylene fiber, vinyltrimethoxysilane and initiator is 7-10:1250-1500:100:3-5:1.8-2.5.
[0024] Preferably, in the specific preparation process of modified polypropylene fiber, the reaction temperature is 35-45° C., and the reaction time is 2-5 hours.
[0025] Preferably, in the specific preparation process of the modified polypropylene fiber, the ethanol aqueous solution is an ethanol aqueous solution with a mass concentration of 10%.
[0026] Preferably, in the specific preparation process of the modified polypropylene fiber, the initiator is dicumyl peroxide.
[0027] Preferably, the preparation method of the high water-retention bonding mortar comprises the following steps: mixing cement, sand and a water-retention thickener evenly, adding modified polypropylene fiber, deionized water and a defoaming agent, stirring and mixing evenly, and obtaining a high water-retention bonding mortar.
[0028] Preferably, the high water retention bonding mortar is used in building materials.
[0029] Furthermore, the high water retention bonding mortar is used in exterior wall insulation materials.
[0030] (III) Beneficial technical effects
[0031] In the present invention, sand is used as aggregate and cement is used as a binder to bind modified polypropylene fiber, sand and a water-retaining thickener to form an integral structure, thereby obtaining a high water-retaining bonding mortar. The modified polypropylene fiber is prepared by reacting modified kaolin, polypropylene fiber and vinyl trimethoxysilane. First, γ-aminopropyl triethoxysilane is used to modify metakaolin, and amino groups are introduced on the surface of metakaolin to obtain aminosilane-modified metakaolin. The amino groups on the surface of aminosilane-modified metakaolin react with the anhydride on hexadecene succinic anhydride, and alkenyl and carboxyl groups are introduced on the surface of metakaolin to obtain modified metakaolin. In the preparation process of the water-retaining thickener, carboxymethyl cellulose, polyethylene glycol, modified metakaolin and acrylic acid react under the action of a crosslinking agent N,N'-methylenebisacrylamide and an initiator ammonium persulfate to form a crosslinked network structure to obtain a water-retaining thickener, and a large number of carboxyl groups and hydroxyl groups are introduced. The modified metakaolin is used as a raw material, and a polymerization reaction occurs with polypropylene fiber and vinyl trimethoxysilane under the action of an initiator, and the metakaolin is grafted onto the surface of the polypropylene fiber to obtain the modified polypropylene fiber.
[0032] Metakaolin has excellent volcanic ash activity and is a highly active auxiliary cementitious material. Its active ingredients react with calcium hydroxide precipitated by cement hydration to form hydrated calcium aluminum feldspar and secondary CSH gel with gel properties, which can significantly improve the early strength of mortar, and the later strength is also continuously enhanced. At the same time, adding metakaolin to mortar can reduce water seepage, accelerate cement hydration, increase density, and thus improve the durability of mortar.
[0033] Polypropylene fiber has the advantages of high strength, good toughness, good chemical resistance, antimicrobial resistance and low price. It can be used as a filling material for concrete, plaster, etc. Adding polypropylene fiber to bonding mortar can improve the mortar's crack resistance, adhesion, durability and waterproof and heat insulation properties.
[0034] Compared with the prior art, the present invention has the following beneficial effects:
[0035] (1) The carboxymethyl cellulose used in the present invention can increase the overall viscosity of the mortar. Polyethylene glycol is a hydrophilic, non-toxic, and highly biocompatible polymer with excellent toughness. The molecular chain contains COC and -OH. The carboxymethyl cellulose contains a large number of hydroxyl groups. The acrylic acid and modified kaolin contain carboxyl groups. The high molecular copolymer after cross-linking polymerization has an excellent three-dimensional network structure. Through the stress transfer and dispersion between the cross-linked networks, the toughness and bonding properties of the system can be enhanced. It has a large number of hydrophilic groups, which gives the mortar high water retention and makes the water released from the mortar not easy to lose. At the same time, kaolin, as a composite filler, has good mechanical properties. Chemical modification can effectively avoid the agglomeration of kaolin and improve the strength of the mortar. Through the composite action of inorganic and organic functional groups, the precipitation of water can be effectively reduced, the water retention of the mortar can be improved, and the bonding strength of the mortar can be improved.
[0036] (2) The polypropylene fiber in the present invention forms a mesh structure in the mortar, which can withstand the internal stress caused by the shrinkage of the substrate, thereby enhancing the ability of the mortar to resist shrinkage, deformation and cracking, and can promote the bonding between the mortar and the base layer, improve the overall stability and durability, and at the same time have good hydrophobic properties and low water absorption. It works together with vinyl trimethoxysilane to greatly reduce the contact area between water and the mortar surface, making it difficult for water droplets on the surface of the bonding plaster mortar to penetrate into the pores through the capillaries, thereby reducing the water absorption rate and improving the waterproof and anti-seepage ability of the mortar. Under the action of the copolymer, the film-forming performance is also improved, the cohesion of the mortar is greatly improved, and the bonding force with the substrate is improved. The large number of active groups -OH and -COOH contained in the water-retaining thickener can form hydrogen bonds with the -COOH in the modified polypropylene fiber, which improves the dispersibility of the raw materials and the compatibility between the raw materials, and has good construction performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.
[0038] Figure 1 Flow chart for preparing high water retention bonding mortar;
[0039] Figure 2 Schematic diagram of the structure of synthetic modified kaolin. DETAILED DESCRIPTION
[0040] In order to facilitate the understanding of the present invention, the present invention will be described more fully below. Preferred embodiments of the present invention are given below. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.
[0041] Example 1
[0042] A method for preparing a high water-retention bonding mortar comprises the following steps:
[0043] By mass, 40 parts of cement, 45 parts of sand and 9 parts of water-retaining thickener are mixed evenly, and then 3 parts of modified polypropylene fiber, 55 parts of deionized water and 0.3 parts of defoaming agent are added, and after stirring and mixing evenly, a high water-retaining bonding mortar is obtained.
[0044] The modified metakaolin is prepared by the following steps:
[0045] S1, drying the metakaolin in a drying oven at 110° C. for 24 h, then mixing the dried metakaolin and γ-aminopropyltriethoxysilane in a mass ratio of 100:6, and milling them in a ball mill for 60 min. After the ball milling, aminosilane-modified metakaolin is obtained;
[0046] S2. Ultrasonic disperse the aminosilane-modified kaolin in a mixed solvent of N,N-dimethylformamide and deionized water in a volume ratio of 9:1. After mixing evenly, add hexadecenyl succinic anhydride and stir to mix. The mass ratio of aminosilane-modified kaolin, mixed solvent and hexadecenyl succinic anhydride is 100:1600:15. React at a temperature of 55°C for 8 hours. After the reaction is completed, wash with anhydrous ethanol and deionized water, filter, and vacuum dry at 60°C for 12 hours to obtain modified kaolin.
[0047] The water-retaining thickener comprises the following steps of preparing: mixing carboxymethyl cellulose and deionized water evenly, adding polyethylene glycol, stirring and mixing for 30 minutes, adding modified kaolin and acrylic acid, stirring and mixing, introducing nitrogen, and adding a crosslinking agent N,N'-methylenebisacrylamide and an initiator ammonium persulfate in a nitrogen atmosphere, wherein the mass ratio of the added carboxymethyl cellulose, deionized water, polyethylene glycol, modified kaolin, acrylic acid, N,N'-methylenebisacrylamide and ammonium persulfate is 100:2500:1:1:210:0.1:3, stirring and mixing, reacting, the reaction temperature is 70°C, the reaction time is 60 minutes, after the reaction is completed, washing with deionized water and anhydrous ethanol, and vacuum drying at 60°C for 6 hours to obtain a water-retaining thickener.
[0048] The modified polypropylene fiber is prepared by the following steps: ultrasonically dispersing the modified metakaolin in an ethanol aqueous solution, adding polypropylene fiber and vinyl trimethoxysilane after uniform dispersion, and adding initiator diisopropylbenzene peroxide after uniform mixing, wherein the mass ratio of the modified metakaolin, the ethanol aqueous solution, the polypropylene fiber, the vinyl trimethoxysilane and the initiator diisopropylbenzene peroxide is 7:1250:100:3:1.8, reacting at a temperature of 35°C for 5 hours, and after the reaction is completed, washing with deionized water, filtering, extracting with acetone, and drying in a vacuum drying oven at 60°C for 6 hours to obtain the modified polypropylene fiber.
[0049] Example 2
[0050] A method for preparing a high water-retention bonding mortar comprises the following steps:
[0051] By mass, 44 parts of cement, 50 parts of sand and 10 parts of water-retaining thickener are mixed evenly, and then 3.5 parts of modified polypropylene fiber, 62 parts of deionized water and 0.4 parts of defoaming agent are added, and after stirring and mixing evenly, a high water-retaining bonding mortar is obtained.
[0052] The modified metakaolin is prepared by the following steps:
[0053] S1, drying the metakaolin in a drying oven at 110° C. for 24 h, then mixing the dried metakaolin and γ-aminopropyltriethoxysilane in a mass ratio of 100:8, and milling them in a ball mill for 75 min. After the ball milling, aminosilane-modified metakaolin is obtained;
[0054] S2. Ultrasonic disperse the aminosilane-modified kaolin in a mixed solvent of N,N-dimethylformamide and deionized water in a volume ratio of 9:1. After mixing evenly, add hexadecenyl succinic anhydride and stir to mix. The mass ratio of aminosilane-modified kaolin, mixed solvent and hexadecenyl succinic anhydride is 100:1800:18. React at a temperature of 60°C for 7 hours. After the reaction is completed, wash with anhydrous ethanol and deionized water, filter, and vacuum dry at 60°C for 12 hours to obtain modified kaolin.
[0055] The water-retaining thickener comprises the following steps of preparing: mixing carboxymethyl cellulose and deionized water evenly, adding polyethylene glycol, stirring and mixing for 30 minutes, adding modified kaolin and acrylic acid, stirring and mixing, introducing nitrogen, and adding a crosslinking agent N,N'-methylenebisacrylamide and an initiator ammonium persulfate in a nitrogen atmosphere, wherein the mass ratio of the added carboxymethyl cellulose, deionized water, polyethylene glycol, modified kaolin, acrylic acid, N,N'-methylenebisacrylamide and ammonium persulfate is 100:2700:1.8:1.4:280:0.14:3.6, stirring and mixing, reacting, the reaction temperature is 75°C, the reaction time is 50 minutes, and after the reaction is completed, washing with deionized water and anhydrous ethanol, and vacuum drying at 60°C for 6 hours to obtain a water-retaining thickener.
[0056] The modified polypropylene fiber is prepared by the following steps: ultrasonically dispersing the modified metakaolin in an ethanol aqueous solution, adding polypropylene fiber and vinyl trimethoxysilane after uniform dispersion, and adding initiator diisopropylbenzene peroxide after uniform mixing, wherein the mass ratio of the modified metakaolin, the ethanol aqueous solution, the polypropylene fiber, the vinyl trimethoxysilane and the initiator diisopropylbenzene peroxide is 8:1350:100:3.8:2, reacting at a temperature of 40°C for 3 hours, and after the reaction is completed, washing with deionized water, filtering, extracting with acetone, and drying in a vacuum drying oven at 60°C for 6 hours to obtain the modified polypropylene fiber.
[0057] Example 3
[0058] A method for preparing a high water-retention bonding mortar comprises the following steps:
[0059] By mass, 44 parts of cement, 50 parts of sand and 10 parts of water-retaining thickener are mixed evenly, and then 3.5 parts of modified polypropylene fiber, 62 parts of deionized water and 0.4 parts of defoaming agent are added, and after stirring and mixing evenly, a high water-retaining bonding mortar is obtained.
[0060] The preparation steps of the modified metakaolin are the same as those in Example 2.
[0061] The water-retaining thickener comprises the following steps of preparing: mixing carboxymethyl cellulose and deionized water evenly, adding polyethylene glycol, stirring and mixing for 30 minutes, adding modified kaolin and acrylic acid, stirring and mixing, introducing nitrogen, and adding a crosslinking agent N,N'-methylenebisacrylamide and an initiator ammonium persulfate in a nitrogen atmosphere, wherein the mass ratio of the added carboxymethyl cellulose, deionized water, polyethylene glycol, modified kaolin, acrylic acid, N,N'-methylenebisacrylamide and ammonium persulfate is 100:2900:2.5:1.8:320:0.18:4.5, stirring and mixing, reacting, the reaction temperature is 75°C, the reaction time is 55 minutes, and after the reaction is completed, washing with deionized water and anhydrous ethanol, and vacuum drying at 60°C for 6 hours to obtain a water-retaining thickener.
[0062] The modified polypropylene fiber is prepared by the following steps: ultrasonically dispersing the modified metakaolin in an ethanol aqueous solution, adding polypropylene fiber and vinyl trimethoxysilane after uniform dispersion, and adding initiator diisopropylbenzene peroxide after uniform mixing, wherein the mass ratio of the modified metakaolin, the ethanol aqueous solution, the polypropylene fiber, the vinyl trimethoxysilane and the initiator diisopropylbenzene peroxide is 9:1450:100:4.2:2.2, reacting at a temperature of 40°C for 4 hours, and after the reaction is completed, washing with deionized water, filtering, extracting with acetone, and drying in a vacuum drying oven at 60°C for 6 hours to obtain the modified polypropylene fiber.
[0063] Example 4
[0064] A method for preparing a high water-retention bonding mortar comprises the following steps:
[0065] By mass, 50 parts of cement, 55 parts of sand and 12 parts of water-retaining thickener are mixed evenly, and then 4.5 parts of modified polypropylene fiber, 70 parts of deionized water and 0.4 parts of defoaming agent are added, and after stirring and mixing evenly, a high water-retaining bonding mortar is obtained.
[0066] The preparation steps of the modified metakaolin are the same as those in Example 2.
[0067] The preparation steps of the water-retaining thickener are the same as those in Example 3.
[0068] The preparation steps of the modified polypropylene fiber are the same as those in Example 3.
[0069] Example 5
[0070] A method for preparing a high water-retention bonding mortar comprises the following steps:
[0071] By mass, 55 parts of cement, 60 parts of sand and 14 parts of water-retaining thickener are mixed evenly, and then 5 parts of modified polypropylene fiber, 75 parts of deionized water and 0.5 parts of defoaming agent are added, and after stirring and mixing evenly, a high water-retaining bonding mortar is obtained.
[0072] The modified metakaolin is prepared by the following steps:
[0073] S1, drying the metakaolin in a drying oven at 110° C. for 24 h, then mixing the dried metakaolin and γ-aminopropyltriethoxysilane in a mass ratio of 100:9, and milling them in a ball mill for 90 min. After the ball milling, aminosilane-modified metakaolin is obtained;
[0074] S2. Ultrasonic disperse the aminosilane-modified kaolin in a mixed solvent of N,N-dimethylformamide and deionized water in a volume ratio of 9:1. After mixing evenly, add hexadecenyl succinic anhydride and stir to mix. The mass ratio of the aminosilane-modified kaolin, the mixed solvent and the hexadecenyl succinic anhydride is 100:2000:21. React at a temperature of 65°C for 6 hours. After the reaction is completed, wash with anhydrous ethanol and deionized water, filter, and vacuum dry at 60°C for 12 hours to obtain modified kaolin.
[0075] The water-retaining thickener comprises the following steps of preparing: mixing carboxymethyl cellulose and deionized water evenly, adding polyethylene glycol, stirring and mixing for 30 minutes, adding modified kaolin and acrylic acid, stirring and mixing, introducing nitrogen, and adding a crosslinking agent N,N'-methylenebisacrylamide and an initiator ammonium persulfate in a nitrogen atmosphere, wherein the mass ratio of the added carboxymethyl cellulose, deionized water, polyethylene glycol, modified kaolin, acrylic acid, N,N'-methylenebisacrylamide and ammonium persulfate is 100:3000:3:2:350:0.2:5, stirring and mixing, reacting, the reaction temperature is 80°C, the reaction time is 45 minutes, after the reaction is completed, washing with deionized water and anhydrous ethanol, and vacuum drying at 60°C for 6 hours to obtain a water-retaining thickener.
[0076] The modified polypropylene fiber is prepared by the following steps: ultrasonically dispersing the modified metakaolin in an ethanol aqueous solution, adding polypropylene fiber and vinyl trimethoxysilane after uniform dispersion, and adding initiator diisopropylbenzene peroxide after uniform mixing, wherein the mass ratio of the modified metakaolin, the ethanol aqueous solution, the polypropylene fiber, the vinyl trimethoxysilane and the initiator diisopropylbenzene peroxide is 10:1500:100:5:2.5, reacting at a temperature of 45°C and a reaction time of 2 hours. After the reaction is completed, washing with deionized water, filtering, extracting with acetone, and drying in a vacuum drying oven at 60°C for 6 hours to obtain the modified polypropylene fiber.
[0077] Comparative Example 1
[0078] A method for preparing a bonding mortar comprises the following steps:
[0079] By mass, 50 parts of cement, 55 parts of sand and 12 parts of water-retaining thickener are mixed evenly, and then 4.5 parts of polypropylene fiber, 70 parts of deionized water and 0.4 parts of defoaming agent are added, and the mixture is stirred and mixed evenly to obtain a bonding mortar.
[0080] The preparation steps of the modified metakaolin are the same as those in Example 2.
[0081] The preparation steps of the water-retaining thickener are the same as those in Example 3.
[0082] Comparative Example 2
[0083] A method for preparing a bonding mortar comprises the following steps:
[0084] By mass, 50 parts of cement, 55 parts of sand and 12 parts of carboxymethyl cellulose are mixed evenly, and then 4.5 parts of modified polypropylene fiber, 70 parts of deionized water and 0.4 parts of defoaming agent are added, and the mixture is stirred and mixed evenly to obtain a bonding mortar.
[0085] The preparation steps of the modified metakaolin are the same as those in Example 2.
[0086] The preparation steps of the modified polypropylene fiber are the same as those in Example 3.
[0087] Comparative Example 3
[0088] A method for preparing a bonding mortar comprises the following steps:
[0089] By mass, 50 parts of cement, 55 parts of sand and 12 parts of thickener are mixed evenly, and then 4.5 parts of modified polypropylene fiber, 70 parts of deionized water and 0.4 parts of defoaming agent are added, and the mixture is stirred and mixed evenly to obtain a bonding mortar.
[0090] The preparation steps of the modified metakaolin are the same as those in Example 2.
[0091] The preparation steps of the modified polypropylene fiber are the same as those in Example 3.
[0092] The thickener is prepared by the following steps: uniformly mixing carboxymethyl cellulose and deionized water, modifying kaolin, stirring and mixing, introducing nitrogen, and adding a crosslinking agent N,N'-methylenebisacrylamide and an initiator ammonium persulfate in a nitrogen atmosphere, wherein the mass ratio of the added carboxymethyl cellulose, deionized water, modified kaolin, N,N'-methylenebisacrylamide and ammonium persulfate is 100:2900:1.8:0.18:4.5, stirring and mixing, reacting, the reaction temperature is 75°C, the reaction time is 55 minutes, and after the reaction is completed, washing with deionized water and anhydrous ethanol, and vacuum drying at 60°C for 6 hours to obtain a thickener.
[0093] The cement used in the examples and comparative examples of the present invention was purchased from Jiangnan Xiaoyetian Cement Co., Ltd., P·Ⅱ52.5 cement, density 3.17g / cm 3 , specific surface area 388m 2 / kg; sand is fine sand, purchased from Shanghai Huanyu Building Engineering Materials Co., Ltd., with a fineness modulus of 2.0, industrial grade; kaolin was purchased from Lingshou County Shifeng Mining Processing Plant, with the item number sf-gp and a particle size of 1250 mesh; polypropylene fiber was purchased from Beijing Wantuming Technology Co., Ltd., with a diameter of 20 μm and the item number 20200405; the CAS number of vinyl trimethoxysilane is 2768-02-7; the CAS number of hexadecenyl succinic anhydride is 32072-96-1; carboxymethyl cellulose (CMC) was purchased from Chengdu Kelon Chemical Reagent Company, 300-800 mPa, CP; polyethylene glycol was purchased from Shanghai Chemical Reagent Company, which is PEG-800; other raw materials and reagents not specified are commercially available.
[0094] The bonding mortars prepared in Examples 1-5 and Comparative Examples 1-3 were subjected to relevant performance tests, and the specific test methods are as follows:
[0095] (1) Water retention performance test: The water retention performance of the bonding mortar was tested in accordance with the provisions of JGT291-2011 "Dry-mixed mortar for masonry and plastering for construction", and the water retention rate was used to indicate the water retention effect;
[0096] (2) Bond strength test: Conduct the bond strength test in accordance with the provisions of JG149-2003 "Expanded polystyrene board thin plastering exterior wall insulation system";
[0097] (3) Flexural strength test: The specimens were formed and cured in accordance with the provisions of DL / T5126-2001 "Test Procedure for Polymer Modified Cement Mortar", and the operation method and test result processing were carried out in accordance with the regulations to test the flexural strength of the bonding mortar;
[0098] The test results are shown in Table 1:
[0099] Table 1
[0100]
[0101] According to the test results in Table 1, it can be seen that the bonding mortars corresponding to Examples 1-5 of the present invention have excellent water retention performance, 7d bonding strength and 7d flexural strength. The water retention rate of the bonding mortar corresponding to Example 4 can reach 99.1%, and the bonding strength of the sample corresponding to Example 5 can reach 4.6MPa at 7d, and the flexural strength at 7d can reach 6.4MPa. In Comparative Example 1, polypropylene fiber is directly added to the bonding mortar without modification, and the dispersibility and compatibility are deteriorated, which has little effect on the water retention rate, which is 98.7%. It has a certain effect on the bonding strength and flexural strength. The corresponding sample has a 7d bonding strength of 4.1MPa and a 7d flexural strength of 5.5MPa. In Comparative Example 2, carboxymethyl cellulose was used instead of a water-retaining thickener to be added to the bonding mortar, and the water retention rate was greatly reduced to 83.1%, which had a certain effect on the bonding strength and flexural strength. The bonding strength of the corresponding sample at 7d was 4.1MPa. Without the introduction of metakaolin and polyethylene glycol, the flexibility was reduced, and the flexural strength at 7d was 5.0MPa. In Comparative Example 3, acrylic acid polymer and polyethylene glycol were not introduced, and the water retention rate was 85.2%. The bonding strength of the corresponding sample at 7d was 4.3MPa, and the flexural strength at 7d was 5.3MPa.
[0102] Although the embodiments of the present invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that all equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the patent coverage of the present invention.
Claims
1. A high water retention bonding mortar, It is characterized in that The invention comprises the following raw materials in parts by weight: 40-55 parts of cement, 45-60 parts of sand, 9-14 parts of water-retaining thickener, 3-5 parts of modified polypropylene fiber, 55-75 parts of deionized water and 0.3-0.5 parts of defoamer; The water-retaining thickener is prepared from carboxymethyl cellulose, polyethylene glycol, modified metakaolin and acrylic acid; The water-retaining thickener comprises the following steps of: uniformly mixing carboxymethyl cellulose and deionized water, adding polyethylene glycol, stirring and mixing for 30 minutes, adding modified metakaolin and acrylic acid, stirring and mixing, introducing nitrogen, adding a crosslinking agent N,N'-methylenebisacrylamide and an initiator ammonium persulfate in a nitrogen atmosphere, stirring and mixing, reacting, and after the reaction is completed, washing with deionized water and anhydrous ethanol, and vacuum drying at 60° C. for 6 hours to obtain a water-retaining thickener; The mass ratio of the carboxymethyl cellulose, deionized water, polyethylene glycol, modified metakaolin, acrylic acid, N,N'-methylenebisacrylamide and ammonium persulfate is 100:2500-3000:1-3:1-2:210-350:0.1-0.2:3-5; The modified polypropylene fiber is prepared by modified metakaolin, polypropylene fiber and vinyl trimethoxysilane; The modified polypropylene fiber is prepared by ultrasonically dispersing the modified metakaolin in an ethanol aqueous solution, adding polypropylene fiber and vinyl trimethoxysilane after the dispersion is uniform, adding an initiator after mixing, reacting, washing with deionized water after the reaction is completed, filtering, extracting with acetone, and drying in a vacuum drying oven at 60° C. for 6 hours to obtain the modified polypropylene fiber; The mass ratio of the modified metakaolin, ethanol aqueous solution, polypropylene fiber, vinyl trimethoxysilane and initiator is 7-10:1250-1500:100:3-5:1.8-2.5, the reaction temperature is 35-45°C, and the reaction time is 2-5h; The modified metakaolin is specifically prepared by the following steps: S1, drying the metakaolin in a drying oven at 110° C. for 24 hours, then mixing the dried metakaolin and γ-aminopropyltriethoxysilane evenly, and milling them in a ball mill. After the ball milling is completed, aminosilane-modified metakaolin is obtained; S2, ultrasonically dispersing the aminosilane-modified metakaolin in a mixed solvent of N,N-dimethylformamide and deionized water, and after mixing evenly, adding hexadecenyl succinic anhydride, stirring and mixing, reacting, and after the reaction is completed, washing with anhydrous ethanol and deionized water, filtering, and vacuum drying at 60° C. for 12 hours to obtain modified metakaolin; The mass ratio of the dried metakaolin and γ-aminopropyltriethoxysilane in S1 is 100:6-9, and the ball milling time is 60-90 min; The mass ratio of aminosilane-modified metakaolin, mixed solvent and hexadecenyl succinic anhydride in S2 is 100:1600-2000:15-21, wherein the volume ratio of N,N-dimethylformamide and deionized water in the mixed solvent is 9:
1.
2. A method for preparing the high water retention bonding mortar according to claim 1, It is characterized in that The method comprises the following steps: mixing cement, sand and a water-retaining thickener evenly, adding modified polypropylene fiber, deionized water and a defoamer, stirring and mixing evenly, and obtaining a high-water-retaining bonding mortar.
3. Use of the high water retention bonding mortar as claimed in claim 1 in building materials.
Citation Information
Patent Citations
An exterior wall thermal insulation board bonding mortar and its preparation method
CN103449788B
Quick-hardening and quick-setting high-strength adhesive mortar for fabricated concrete composite wallboard
CN116813267A
Anti-cracking anti-seepage dry-mixed plastering mortar dry-mixed material and plastering mortar
CN110240448A
Adhesive mortar
CN112707696A