Fireproof silicone sealant and preparation method thereof

By using specific components and treatment methods in silicone sealants, the curing speed and bonding strength are improved, and the problems of slow curing speed and insufficient flame retardant performance of traditional silicone sealants are solved, achieving more efficient curing and stability sex.

CN117887415BActive Publication Date: 2024-12-06东莞市乙霖电子材料有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410303034.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-18
Publication Date
2024-12-06
Estimated Expiration
2044-03-18

AI Technical Summary

Technical Problem

Traditional silicone sealants have slow curing speed, poor mechanical strength and adhesion, and insufficient stability and flame retardant properties in high temperature environments. Especially the dealcoholing and deacidifying types have irritating odors, corrosion on copper, and deacetones. The vulcanization rate is fast but the curing process is harsh and needs improvement.

Method used

Using α,ω-dihydroxypolydimethylsiloxane, hydroxy-terminated polydimethylsiloxane, isopropylene oxysilane crosslinking agent, phosphate esters and solid flame retardants, porous hollow glass microbeads and other groups The cross-linking reaction rate and bonding strength are improved through pre-silanization reaction and moisture absorption treatment, and curing is promoted through dimethyl ketone oxime.

Benefits of technology

It significantly improves the curing speed of the sealant, enhances the adhesion and mechanical strength, improves the flame retardant performance and stability, and reduces the curing time and maintenance needs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention discloses fireproof organosilicon sealant and preparation method thereof, the sealant includes α, ω-dihydroxy polydimethylsiloxane, hydroxyl-terminated polydimethylsiloxane, dimethyl silicone oil, cross-linking agent, flame retardant, filler, silane coupling agent, catalyst, accelerator and dimethyl ketone oxime; the preparation method includes pre-silylation reaction, solid-liquid kneading and sealant preparation of porous hollow glass microspheres. The present invention uses porous hollow glass microspheres with internal moisture as large-particle fillers, pre-silylation reaction is carried out on its surface, dimethyl ketone oxime is used to hydrolyze and deoxygenate under acidic conditions, and the curing speed is greatly increased without affecting the stability of the glue, so as to reduce the curing time after gluing; by compounding solid flame retardant and liquid flame retardant, the distribution uniformity of flame retardant components is improved, and the balance of organic and inorganic phases is made, so as to improve the strength of adhesion and adhesive layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of special sealants, in particular to fireproof organic silicon sealants and a preparation method thereof. Background Art

[0002] Silicone sealant is a neutral curing silicone sealant with good bonding strength and sealing performance for most materials. Compared with acrylic or polyurethane sealants, silicone sealant has better temperature resistance and electrical properties. Its temperature resistance range is -45℃~350℃, and it has excellent electrical properties. It is moisture-proof, corona-proof, shock-resistant and aging-resistant. It is widely used in the bonding and sealing of industry, building materials, automotive materials and various electronic appliances.

[0003] However, compared with acrylic or polyurethane sealants, traditional silicone sealants have a slow curing speed and poor mechanical strength, adhesion and flame retardancy. Therefore, flame retardants, cross-linking agents, and some fillers and additives need to be added during preparation.

[0004] According to the cross-linking agent, silicone sealants are divided into dealcoholization type, deacidification type, deketoxime type or deacetone type silicone sealants. The high temperature resistance of dealcoholization type silicone sealants is relatively poor compared with other types; deacidification type and deketoxime type silicone sealants have pungent odors and are corrosive to copper; deacetone type silicone sealants have better high temperature resistance, fast vulcanization rate, good storage stability, and no corrosion to metals. Therefore, deacetone type silicone sealants have certain application potential in the field of high temperature resistance.

[0005] The crosslinking agent used in silicone sealant can react with the hydroxyl groups on the molecular structure of silicone rubber, converting the linear silicone rubber into a crosslinked body with a three-dimensional network structure, so that the silicone sealant has a certain strength and elasticity, which is manifested as the vulcanization of the rubber material on a macro scale. The crosslinking agent of the deacetone type silicone sealant is isopropenyloxysilane, and its crosslinking mechanism is: the isopropenyloxy group first undergoes a hydrolysis reaction under the action of moisture in the air to generate silanol and isopropenol; the silanol generated by the hydrolysis of isopropenyloxysilane undergoes a condensation reaction with the silanol of silicone rubber to form a three-dimensional network structure crosslinked body; isopropenol is unstable and undergoes a tautomerism reaction to generate acetone, so it is called deacetone type.

[0006] During the vulcanization process of deacetone-type silicone sealant, a low-temperature and high-humidity environment is required, and the vulcanization time is 3-7 days. It needs to be carried out under dust-free and non-contacting conditions with a large amount of liquid water. At the same time, the vulcanization process needs to be finalized, that is, the vulcanization conditions are relatively harsh; and when the required adhesive layer is thicker (such as 4-6mm), the curing process is slower and needs to be improved urgently; in addition, the interface effect between the silicone cross-linking system and inorganic components such as flame retardants and fillers also needs to be improved. Summary of the invention

[0007] The purpose of the present invention is to solve the shortcomings of the prior art and to propose a fire-resistant organic silicon sealant and a preparation method thereof.

[0008] In order to achieve the above object, the present invention adopts the following technical solutions:

[0009] The present invention firstly provides a fireproof silicone sealant, comprising the following components in parts by weight:

[0010] 100 parts of α,ω-dihydroxy polydimethylsiloxane, i.e. 107 silicone rubber, with a viscosity of 30,000-40,000 cps, as the main ingredient;

[0011] 5-7 parts of hydroxyl-terminated polydimethylsiloxane, with a viscosity greater than 70,000 cps, has a viscosity-enhancing effect;

[0012] 10-15 parts of dimethyl silicone oil, as a thinner solvent, to facilitate mixing and discharging;

[0013] 10-15 parts of a crosslinking agent, which is isopropenyloxysilane, including methyl triisopropenyloxysilane and vinyl triisopropenyloxysilane, for moisture absorption and crosslinking;

[0014] 35-40 parts of flame retardant, which is a combination of phosphate flame retardant and solid flame retardant in a weight ratio of 2:8;

[0015] 30-35 parts of fillers, including 2μm silica powder (Jiangxi Bluestar Spark Organic Silicon Co., Ltd.) and porous hollow glass microspheres ≤60μm, as support to improve the mechanical strength of the sealant after molding; the weight ratio of silica powder to porous hollow glass microspheres in the filler is 1: (0.2-0.3), and the porous hollow glass microspheres ≤60μm (Xinghua Hongyang Glass Products Co., Ltd., with 1-30nm nano-through holes on the surface) are used as moisture carriers. During the cross-linking reaction, water vapor is continuously released to increase the cross-linking reaction rate;

[0016] 4-5 parts of silane coupling agent, γ-aminopropyltriethoxysilane (KH550), N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane (KH792), to promote the mixing uniformity of the organic phase and the inorganic phase;

[0017] 0.4-0.8 parts of a catalyst, tetramethylguanidinepropyltrimethoxysilane, to improve the efficiency of the cross-linking reaction;

[0018] 4-5 parts of an accelerator, which is any one of cobalt methacrylate, methacrylate accelerator, organic peroxide accelerator, disulfide accelerator and benzoic acid accelerator. The accelerator is used to accelerate the curing reaction of silicone rubber, reduce the curing time and improve production efficiency;

[0019] 0.8-1 part of dimethyl ketone oxime. Dimethyl ketone oxime is easily hydrolyzed, volatile and highly reducible. It can absorb moisture and consume oxygen to form a flame retardant area. It can volatilize during the curing process to form a water inlet channel, further promoting the cross-linking reaction.

[0020] The processing process of porous hollow glass microspheres is as follows:

[0021] 1) Screening: Vibrate and screen the porous hollow glass microspheres with a particle size of 1-1000 μm to obtain porous hollow glass microspheres with a particle size of ≤60 μm;

[0022] 2) Adsorption and removal of impurities: Use clean polyester fiber felt cloth (polyester fiber non-woven needle-punched fiber chemical fiber felt, Nangong Runhua Felt Co., Ltd., with the wool side facing up when in use) and place it at a 50° angle, pour porous hollow glass microbeads ≤60μm on the polyester fiber felt cloth, and let the porous hollow glass microbeads ≤60μm roll down from the top of the slope to the bottom of the slope;

[0023] After five times of adsorption and impurity removal treatment, the weight proportion of 40-60μm porous hollow glass microspheres increased from the initial 58.6% to 87.4%, and the roundness rate increased from the initial 85.7% to 97.1%, indicating that the adsorption process has the effect of removing small-size dust and broken particles, and the obtained porous hollow glass microspheres are of higher quality and improved loading efficiency;

[0024] 3) Loading: The porous hollow glass microspheres after adsorption and impurity removal were replaced by nitrogen shock for 2 hours, and then vacuumed at 0.1 kPa for 1 hour, and then stirred for 2 hours under the air intake conditions of 50°C and 100% humidity, and then taken out and drained for later use; by means of moisture absorption, the humid air entered the porous hollow glass microspheres, thereby obtaining porous hollow glass microspheres containing moisture.

[0025] Preferably, the phosphate flame retardant includes at least one of tricresyl phosphate (TCP) and triethyl phosphate (TEP), both of which are liquid flame retardants, and serves as an auxiliary flame retardant to facilitate uniform distribution of the flame retardant component.

[0026] Preferably, the solid flame retardant is a mixture of aluminum hydroxide and magnesium hydroxide in a weight ratio of 6:4, which serves as the main flame retardant and increases the firmness of the inorganic phase.

[0027] The present invention also provides a method for preparing the aforementioned fireproof silicone sealant, comprising the following steps:

[0028] S1. Pre-silanization reaction of porous hollow glass microspheres:

[0029] In anhydrous and oxygen-free atmosphere, porous hollow glass microspheres, dimethyl silicone oil, silane coupling agent and 85% phosphoric acid are mixed, the phosphoric acid addition amount accounts for 2.5-3% of the total weight of the system, and the mixture is stirred at high speed for 1.5-2h, and then dimethyl ketoxime is added dropwise and stirred for 15min, and dimethyl ketoxime is hydrolyzed under dilute acid conditions to remove excess water, and then a phosphate flame retardant is added dropwise and stirred to obtain a suspension, and the water content in the liquid phase is detected to be less than 1% (excluding the water content inside the porous hollow glass microspheres), and the pH is 7.2-7.4;

[0030] S2. Solid-liquid kneading:

[0031] Add α,ω-dihydroxy polydimethylsiloxane, hydroxyl-terminated polydimethylsiloxane, solid flame retardant and silicon powder into a kneader, mix and dehydrate, and cool to room temperature to obtain a base material colloid;

[0032] S3. Sealant preparation:

[0033] The base colloid and the suspending agent are placed in a high-speed mixer for mixing, and then the accelerator, the crosslinking agent and the catalyst are added in sequence, and a small amount of hydroxyl-terminated polydimethylsiloxane, dimethyl silicone oil or dimethyl ketoxime is added to adjust the viscosity or the dimethyl ketoxime content, and the sealant is obtained after mixing evenly.

[0034] Preferably, if the water content in the liquid phase of the suspension obtained in S1 is 1-2%, dimethyl ketoxime is continued to be added dropwise until the water content is less than 1%. If the water content in the liquid phase after the reaction is greater than 2%, the amount of phosphoric acid added should be reduced. Taking into account the pH limit of the system (the flame retardant component is alkaline) and the liquid water required for the hydrolysis reaction, the amount of phosphoric acid added obtained in the test accounts for 2.5-3% of the total weight of the system. This step promotes the hydrolysis of the silane coupling agent by adding a small amount of water, and dimethyl ketoxime can be used for hydrolysis and deoxygenation under acidic conditions.

[0035] Compared with the prior art, the present invention has the following beneficial effects:

[0036] 1. The present invention uses porous hollow glass microspheres loaded with moisture as large-diameter fillers, and performs a pre-silanization reaction on the surface, which greatly increases the curing speed without affecting the stability of the glue solution, thereby reducing the curing time after glue coating.

[0037] 2. The present invention uses dimethyl ketoxime to hydrolyze and deoxygenate under acidic conditions to ensure the stability of the glue system.

[0038] 3. The present invention improves the distribution uniformity of the flame retardant components and the balance of the organic and inorganic phases by compounding the solid flame retardant and the liquid flame retardant, thereby improving the adhesion and strength of the adhesive layer. DETAILED DESCRIPTION

[0039] The technical solutions in the embodiments of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.

[0040] 1. Preparation of glue:

[0041] The preparation method of the fireproof silicone sealant comprises the following steps:

[0042] 1. Processing process of porous hollow glass microspheres:

[0043] 1) Screening: Vibrate and screen the porous hollow glass microspheres with a particle size of 1-1000 μm to obtain porous hollow glass microspheres with a particle size of ≤60 μm;

[0044] 2) Adsorption and removal of impurities: Use clean polyester fiber felt cloth (polyester fiber non-woven needle-punched fiber chemical fiber felt, Nangong Runhua Felt Co., Ltd., with the wool side facing up when in use) and place it at a 50° angle, pour the porous hollow glass beads on the polyester fiber felt cloth, and let the porous hollow glass beads roll from the top of the slope to the bottom of the slope;

[0045] After five times of adsorption and impurity removal treatment, the weight proportion of 40-60μm porous hollow glass microspheres increased from the initial 58.6% to 87.4%, and the roundness rate increased from the initial 85.7% to 97.1%, indicating that the adsorption process has the effect of removing small-size dust and broken particles, and the obtained porous hollow glass microspheres are of higher quality and improved loading efficiency;

[0046] 3) Loading: The porous hollow glass microspheres after adsorption and impurity removal were replaced by nitrogen shock for 2 hours, and then vacuumed at 0.1 kPa for 1 hour, and then stirred for 2 hours under the air intake conditions of 50°C and 100% humidity, and then taken out and drained for later use; by means of moisture absorption, the humid air entered the porous hollow glass microspheres, thereby obtaining porous hollow glass microspheres containing moisture.

[0047] 2. Pre-silanization reaction of porous hollow glass microspheres:

[0048] In anhydrous and oxygen-free atmosphere, porous hollow glass microspheres, dimethyl silicone oil, silane coupling agent and 85% phosphoric acid are mixed, the phosphoric acid addition amount accounts for 2.5-3% of the total weight of the system, and the mixture is stirred at high speed for 1.5-2h, and then dimethyl ketoxime is added dropwise and stirred for 15min, and dimethyl ketoxime is hydrolyzed under dilute acid conditions to remove excess water, and then a phosphate flame retardant is added dropwise and stirred to obtain a suspension, and the water content in the liquid phase is detected to be less than 1% (excluding the water content inside the porous hollow glass microspheres), and the pH is 7.2-7.4;

[0049] When the water content in the liquid phase of the obtained suspension is 1-2%, continue to add dimethyl ketoxime until the water content is less than 1%; if the water content in the liquid phase after the reaction is greater than 2%, the amount of phosphoric acid added should be reduced. Considering the pH limit of the system (the flame retardant component is alkaline) and the liquid water required for the hydrolysis reaction, the amount of phosphoric acid added in the test accounts for 2.5-3% of the total weight of the system; this step promotes the hydrolysis of the silane coupling agent by adding a small amount of water (the solvent in phosphoric acid), which can be hydrolyzed and deoxygenated under acidic conditions by dimethyl ketoxime.

[0050] 3. Solid-liquid kneading:

[0051] Add α,ω-dihydroxy polydimethylsiloxane, hydroxyl-terminated polydimethylsiloxane, solid flame retardant and silicon powder into a kneader, mix and dehydrate, and cool to room temperature to obtain a base material colloid;

[0052] 4. Sealant preparation:

[0053] The base colloid and the suspending agent are placed in a high-speed mixer for mixing, and then the accelerator, the crosslinking agent and the catalyst are added in sequence, and a small amount of hydroxyl-terminated polydimethylsiloxane, dimethyl silicone oil or dimethyl ketoxime is added to adjust the viscosity or the dimethyl ketoxime content, and the sealant is obtained after mixing evenly.

[0054] 5. The formula used was tested, and the formula of each embodiment is as shown in Table 1 below:

[0055] Table 1. Formula of a fire-resistant silicone sealant

[0056]

[0057] It should be noted that the weight units of each component in Table 1 are kg;

[0058] The flame retardant is a combination of a phosphate flame retardant and a solid flame retardant in a weight ratio of 2:8. The phosphate flame retardant is compounded with tricresyl phosphate (TCP) and triethyl phosphate (TEP) in a volume ratio of 1:1. It is used as an auxiliary liquid flame retardant to facilitate the uniform distribution of the flame retardant components. The solid flame retardant is a mixture of aluminum hydroxide and magnesium hydroxide in a weight ratio of 6:4. It serves as the main flame retardant and increases the firmness of the inorganic phase.

[0059] The fillers include 2μm silica powder (Jiangxi Bluestar Starfire Silicone Co., Ltd.) and ≤60μm porous hollow glass microspheres, which serve as support to improve the mechanical strength of the sealant after molding;

[0060] The silane coupling agent is γ-aminopropyltriethoxysilane (KH550) or N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane (KH792), which promotes the mixing uniformity of the organic phase and the inorganic phase;

[0061] The catalyst is tetramethylguanidinepropyltrimethoxysilane, which is used to improve the efficiency of the cross-linking reaction;

[0062] Among them, cobalt methacrylate is used as the accelerator. The function of the accelerator is to accelerate the curing reaction of silicone rubber, reduce the curing time and improve production efficiency. According to the accelerators used in traditional silicone sealants, after preliminary replacement tests, any of cobalt methacrylate, organic peroxide accelerator, disulfide accelerator, methacrylate accelerator and benzoic acid accelerator can reduce the curing time of sealants. The difference is that organic peroxide accelerator and disulfide accelerator will react with dimethyl ketone oxime and turn yellow in the later stage. Methacrylate accelerator and benzoic acid accelerator have higher acid values, and produce neutralization reaction and agglomeration in the alkaline system with flame retardant, which is not conducive to the stability of the system.

[0063] The weight of dimethyl ketoxime is the actual usage of the pre-silanization reaction of the porous hollow glass microspheres. Dimethyl ketoxime is easily hydrolyzed, volatile and highly reducible. It can absorb moisture and consume oxygen to form a flame retardant area. It can volatilize during the curing process to form a water inlet channel, further promoting the cross-linking reaction.

[0064] 6. The role of porous hollow glass microspheres:

[0065] The following comparative tests were conducted:

[0066] Comparative Example 15:

[0067] The rest is the same as Example 2, except that the porous hollow glass microspheres are not subjected to a pre-silanization reaction, and the porous hollow glass microspheres, dimethyl silicone oil, silane coupling agent, phosphoric acid with a concentration of 85% and other components are mixed with the base colloid. The result is that there is too much water, which leads to too fast curing, and the finished sealant is not easy to preserve and is easy to agglomerate. Therefore, the porous hollow glass microspheres that carry moisture must undergo a pre-silanization reaction and surface dehydration to avoid affecting the mixing of the sealant.

[0068] Comparative Example 16:

[0069] The rest is the same as Example 2, except that moisture absorption under load is not performed. The curing time is compared with that of Example 2.

[0070] 2. Performance test:

[0071] 1. Test standard:

[0072] Refer to GB / T 32369-2015 to test the curing speed;

[0073] Refer to GB / T 13477.18-2002 and use a universal mechanical testing machine to measure the peeling adhesion of the adhesive layer;

[0074] Refer to GB / T 24267-2009 to measure the tensile modulus of the adhesive layer;

[0075] Referring to the flame retardant grade determination method in the UL94 standard, each sealant product was made into a colloid specimen after curing, and the flame retardant performance grade was measured respectively. The flame retardant grades are V0, V1 and V2 from high to low.

[0076] 2. Performance of each sealant product:

[0077] As shown in Table 2 below:

[0078] Table 2. Properties of a fire-resistant silicone sealant

[0079]

[0080] 3. Conclusion of single factor experiment:

[0081] 1) Amount of crosslinking agent:

[0082] Comparing Comparative Examples 1-2 with Example 2, too little cross-linking agent affects the tensile modulus and peel adhesion, while too much cross-linking agent easily causes solidification agglomeration and high viscosity, thus resulting in a lower tensile modulus.

[0083] 2) Flame retardant dosage:

[0084] Comparing Comparative Examples 3-4 with Example 2, too little flame retardant will affect the flame retardant properties, while too much will cause an imbalance between the inorganic and organic phases and poor tensile properties.

[0085] 3) Filling ingredients:

[0086] Comparing Comparative Examples 5-6 with Example 2, the total amount of filler is kept constant, the fineness of silicon powder is smaller than that of porous hollow glass microspheres, and as the amount of porous hollow glass microspheres increases, the amount of moisture increases, the curing speed is faster, but the strength is slightly reduced.

[0087] 4) Silane coupling agent dosage:

[0088] Comparing Comparative Examples 7-8 with Example 2, the silane coupling agent has a positive effect on the blending of organic and inorganic phases, but a large amount thereof may easily result in a lower viscosity and a slower curing speed of the finished sealant.

[0089] 5) Accelerator dosage:

[0090] Comparing Comparative Examples 9-10 with Example 2, the accelerator mainly affects the curing speed and has little effect on the adhesion and adhesive strength.

[0091] 6) Catalyst dosage:

[0092] Comparing Comparative Examples 11-12 with Example 2, the catalyst affects the curing speed and the degree of crosslinking, and thus affects the strength and adhesion, but too much catalyst is useless and increases the cost.

[0093] 7) Dosage of dimethyl ketoxime:

[0094] Comparing Comparative Examples 13-14 with Example 2, dimethyl ketoxime mainly affects the liquid water content of the system. The more water, the faster the curing, but it is easy to agglomerate, resulting in lower adhesion and strength.

[0095] 8) Impact of moisture absorption under load:

[0096] Comparing Comparative Example 16 with Example 2, the curing speed is significantly reduced by using porous hollow glass microspheres that are not subjected to load moisture absorption.

[0097] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. Fireproof silicone sealant, characterized in that: It includes the following components by weight: 100 parts of α,ω-dihydroxy polydimethylsiloxane with a viscosity of 30,000-40,000 cps; 5-7 parts of hydroxyl-terminated polydimethylsiloxane having a viscosity greater than 70,000 cps; 10-15 parts of dimethyl silicone oil; 10-15 parts of a crosslinking agent, which is isopropenyloxysilane, wherein the isopropenyloxysilane includes at least one of methyl triisopropenyloxysilane and vinyl triisopropenyloxysilane; 35-40 parts of flame retardant, which is a combination of phosphate flame retardant and solid flame retardant in a weight ratio of 2:8; 30-35 parts of filler, including silicon micropowder with a particle size of 2 μm and porous hollow glass microspheres with a particle size of ≤60 μm, wherein the weight ratio of silicon micropowder to porous hollow glass microspheres in the filler is 1:(0.2-0.3); 4-5 parts of a silane coupling agent, which is γ-aminopropyltriethoxysilane or N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane; 0.4-0.8 parts of a catalyst, which is tetramethylguanidinepropyltrimethoxysilane; 4-5 parts of accelerator, which is cobalt methacrylate; 0.8-1 part of dimethyl ketoxime; The processing process of the porous hollow glass microspheres is as follows: 1) Screening: Vibrate and screen the porous hollow glass microspheres with a particle size of 1-1000 μm to obtain porous hollow glass microspheres with a particle size of ≤60 μm; 2) Adsorption and impurity removal: Use a clean polyester fiber felt cloth and place it at a 50° angle, pour porous hollow glass microbeads ≤60μm on the polyester fiber felt cloth, and let the porous hollow glass microbeads ≤60μm roll down from the top of the slope to the bottom of the slope; 3) Loading: The porous hollow glass microspheres after adsorption and impurity removal were replaced by nitrogen shock for 2 hours, then vacuumed at 0.1 kPa for 1 hour, then stirred for 2 hours under the air intake conditions of 50° C. and 100% humidity, and then taken out and drained for later use; The porous hollow glass microspheres after the treatment process are then subjected to a pre-silanization reaction.

2. The fireproof silicone sealant according to claim 1, characterized in that: The phosphate flame retardant includes at least one of tricresyl phosphate and triethyl phosphate.

3. The fireproof silicone sealant according to claim 1, characterized in that: The solid flame retardant is a mixture of aluminum hydroxide and magnesium hydroxide in a weight ratio of 6:

4.

4. The method for preparing the fireproof silicone sealant according to claim 1, characterized in that: The following steps are involved: S1. Pre-silanization reaction of porous hollow glass microspheres: In anhydrous and oxygen-free atmosphere, porous hollow glass microspheres, dimethyl silicone oil, silane coupling agent and 85% phosphoric acid are mixed, the phosphoric acid addition amount accounts for 2.5-3% of the total weight of the system, and the mixture is stirred at high speed for 1.5-2h, then dimethyl ketoxime is added dropwise and stirred for 15min, then a phosphate flame retardant is added dropwise, and a suspension is obtained by stirring, and the water content in the liquid phase is detected to be less than 1%, and the pH is 7.2-7.4; S2. Solid-liquid kneading: Add α,ω-dihydroxy polydimethylsiloxane, hydroxyl-terminated polydimethylsiloxane, solid flame retardant and silicon powder into a kneader, mix and dehydrate, and cool to room temperature to obtain a base material colloid; S3. Sealant preparation: The base colloid and the suspending agent are placed in a high-speed mixer for mixing, and then the accelerator, the crosslinking agent and the catalyst are added in sequence, and a small amount of hydroxyl-terminated polydimethylsiloxane, dimethyl silicone oil or dimethyl ketoxime is added to adjust the viscosity or the dimethyl ketoxime content, and the sealant is obtained after mixing evenly.