A hot wire for thermal conductivity detector and preparation method thereof

By etching the hot wire of the thermal conductivity detector and depositing low-dimensional nanomaterials, a composite nanostructure is formed, which solves the problem of insufficient sensitivity and stability of the thermal conductivity detector and achieves higher detection sensitivity and longer service life. .

CN117888076BActive Publication Date: 2024-10-18SUZHOU HISILIFU BIOMEDICAL TECH CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202311843307.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-28
Publication Date
2024-10-18
Estimated Expiration
2043-12-28

AI Technical Summary

Technical Problem

Existing hot wires used in thermal conductivity detectors have insufficient sensitivity, insufficient stability, and short lifespan.

Method used

By etching the raw hot wire, depositing low-dimensional nanomaterials such as graphene, and depositing precious metals such as gold or platinum on the etched holes, a composite nanostructure is formed to enhance the conductivity and oxidation resistance of the hot wire.

Benefits of technology

It improves the sensitivity and stability of the thermal conductivity detector, extends its service life, can maintain the uniformity of thermal conductivity properties at high temperatures, and shows stronger corrosion resistance in corrosive gases. The minimum concentration of combustible gases can be detected up to 0.01ppm.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117888076B_ABST
    Figure CN117888076B_ABST
Patent Text Reader

Abstract

The present invention discloses a hot wire for a thermal conductivity detector and a preparation method thereof, wherein the preparation method comprises the following steps: etching a raw material hot wire; depositing low-dimensional nanomaterials on the surface of the hot wire and the etched holes. The present invention etches micro-nano holes on the hot wire for the thermal conductivity detector and then deposits low-dimensional nanomaterials to generate a composite nanostructure, which is uniformly composited on the microscopic interface to achieve uniformity of conductivity at all directions and interfaces, thereby ensuring the stability of the overall thermal conductivity device; enhancing the mechanical properties of the metal at high temperatures, such as tensile strength, etc., so that a thinner composite thermal conductive wire can be prepared to achieve more sensitive detection; the thermal conductivity detector using the hot wire has a stronger corrosion resistance, thereby increasing the service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of thermal conductivity detectors, and in particular to a hot wire for a thermal conductivity detector and a preparation method thereof. Background Art

[0002] Thermal conductivity detector (TCD), also known as thermal conductivity cell or hot wire detector, has a simple structure, stable performance, wide linear range and responds to various substances. It is the most commonly used, earliest and most widely used detector in gas chromatography. Its working principle is based on the different thermal conductivities of different gases. The sensitive element of the thermal conductivity detector usually uses a hot wire, such as tungsten wire, platinum wire, rhenium wire, and the hot wire forms a bridge. After a constant current passes through, the temperature of the hot wire rises, and the carrier gas molecules take away the heat of the hot wire when flowing through. When the carrier gas flow rate is stable, the heat of the hot wire taken away is also constant, and the bridge outputs a constant voltage signal. When the component to be measured enters the thermal conductivity cell together with the carrier gas, the thermal conductivity of the component to be measured is different from that of the pure carrier gas, and the heat of the hot wire taken away by it is also different, causing the temperature of the hot wire to change, and its resistance also changes accordingly, which in turn causes an unbalanced potential to be generated at the output end of the bridge as a signal output. Therefore, it is necessary to improve the resistance temperature sensitivity of the hot wire, the uniformity of the thermal conductivity of the hot wire under the flow field, and the ability of the hot wire to withstand corrosion and oxidation in different atmospheres, so as to produce a more sensitive, more stable and longer-lasting thermal conductivity detector. Summary of the invention

[0003] Therefore, the technical problem to be solved by the present invention is the problem that the existing hot wire for thermal conductivity detector has insufficient sensitivity, insufficient stability and short life, and thus provides a hot wire for thermal conductivity detector and a preparation method thereof.

[0004] To this end, the present invention adopts the following technical solutions:

[0005] A method for preparing a hot wire for a thermal conductivity detector comprises the following steps:

[0006] S1: Etching the raw material hot wire;

[0007] S2: Deposit low-dimensional nanomaterials on the hot wire surface and etched holes.

[0008] Preferably, after depositing the low-dimensional nanomaterial, the step of continuously depositing the noble metal is also included;

[0009] The noble metal includes at least one of gold and platinum, and the deposited thickness is 5-500nm.

[0010] Furthermore, the low-dimensional nanomaterial includes graphene, molybdenum disulfide or tellurene.

[0011] Preferably, in step S2, the depositing of low-dimensional nanomaterials is the deposition of graphene using chemical vapor deposition.

[0012] The deposition is carried out by introducing methane into the protective atmosphere and depositing at 800-1200° C. for 45-75 minutes;

[0013] The total gas flow rate is 20 sccm-200 sccm, and methane accounts for 1-2% of the total gas flow rate.

[0014] An annealing step is also included before deposition, wherein the annealing is performed at 350-1000° C. in a protective atmosphere for 20-40 minutes.

[0015] The protective atmosphere includes at least one of nitrogen, argon and hydrogen.

[0016] In step S1, the etching forms micrometer or nanometer-scale holes on the surface of the raw material hot wire;

[0017] Preferably, the etching includes room temperature pickling, room temperature plasma etching, acidic etching solution etching and 500° C. oxygen plasma etching performed in sequence.

[0018] The raw material heating wire is a metal heating wire, including one of rhenium tungsten wire, copper wire, tungsten wire and stainless steel wire, and has a diameter of 1-500 μm.

[0019] The present invention also provides a hot wire for a thermal conductivity detector, which is prepared by the above preparation method.

[0020] The technical solution of the present invention has the following advantages:

[0021] (1) The present invention etches micro-nano cavities in a thermal conductivity detector with a hot wire and then deposits low-dimensional nanomaterials to generate a composite nanostructure, thereby enhancing the electrical conductivity and anti-oxidation performance of the hot wire, and further enhancing the sensitivity of the thermal conductivity detector.

[0022] (2) The present invention uses a metal hot wire to form a microcavity hole structure after etching, and uses chemical vapor deposition to grow a high-quality graphene thin layer on the structure, which is filled inside these hole structures and coated on the entire inner and outer surfaces of the hot wire to form a nanostructured composite graphene metal hot wire. This structure can enhance the anti-oxidation and anti-corrosion properties of the metal surface, maintain the thermal conductivity of the metal at different temperatures, and especially maintain and enhance the thermal conductivity and uniformity of the surface and the inside in different directions. The composite material can maintain the uniformity of the electrical conductivity in all directions and at all interfaces by using graphene and metal to be uniformly compounded at the microscopic interface, thereby ensuring the stability of the overall thermal conductivity device. The hot wire uses graphene to enhance the mechanical properties of the metal at high temperatures, such as tensile strength, so that a thinner composite hot wire can be prepared, and more sensitive detection can be achieved by using multiple parallel hot wires. The thermal conductivity detector using this hot wire has a stronger corrosion resistance, and performs better than the existing hot wire in passing through corrosive gases such as hydrogen sulfide, thereby increasing the service life.

[0023] (3) After etching the metal hot wire and depositing low-dimensional nanomaterials on the surface and the etched holes, the present invention further deposits precious metals as catalysts. This structure can enable the hot wire to have catalytic oxidation capabilities. When the combustible gas flows through the surface of the hot wire, the catalytic oxidation releases heat, which can further increase the local temperature of the hot wire, thereby obtaining a greater resistance change. The hot wire prepared in this way solves the defects of the existing hot wire detection such as low sensitivity and non-selectivity. At the same time, it has a longer life, is more stable, and has higher sensitivity than catalytic combustion sensors. After the hot wire prepared in this way is assembled into a thermal conductivity detector, the minimum detection concentration of combustible gases (such as methane and carbon monoxide) can reach 0.01ppm. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0025] Figure 1 The tensile test results of Example 1 and Comparative Examples 1-2 are shown;

[0026] Figure 2 1 and 2 are corrosion resistance test results, wherein (A) is the test result of the rhenium tungsten alloy sheet treated by the scheme in Example 1, and (B) is the test result of the untreated rhenium tungsten alloy sheet. DETAILED DESCRIPTION

[0027] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.

[0028] If no specific experimental steps or conditions are specified in the examples, the experiments can be carried out according to the conventional experimental steps or conditions described in the literature in the art.

[0029] The following specific examples are further explanations of the present invention. The examples cited cannot list all the embodiments of the present invention. Only some of the embodiments are used as examples for explanation. The specific examples are as follows:

[0030] Example 1

[0031] This embodiment provides a hot wire for a thermal conductivity detector, wherein the raw material of the hot wire is a rhenium tungsten wire with a diameter of 50 μm and a rhenium content of 3%. The specific preparation method is as follows:

[0032] (1) Etching of rhenium tungsten wire:

[0033] 1. First, pickle with a mixture of nitric acid and sulfuric acid at room temperature for 30 minutes;

[0034] 2. Use oxygen plasma etching at room temperature for 20 minutes, and the plasma power is 50w;

[0035] 3. Etch with a mixture of nitric acid, sulfuric acid, hydrochloric acid, hydrofluoric acid, deionized water, and buffer NH4F for 30 minutes at room temperature;

[0036] 4. Use oxygen plasma etching at 500°C for 20 minutes, with a plasma power of 50W;

[0037] (2) The etched rhenium tungsten wire was fixed on a copper foil plate, marked and oriented, named a reaction plate, and the reaction plate was ultrasonically treated with acetone and deionized water for 10 min in turn, and then nitrogen was introduced for annealing, with the flow rate set to 100 sccm, the annealing temperature set to 1000°C, and the time set to 30 min.

[0038] (3) After annealing, methane is introduced for chemical vapor deposition to grow graphene. The deposition temperature is set to 1050°C, the time is set to 1 hour, and the methane flow rate accounts for 1% of the total gas flow rate. After the reaction is completed, heating and methane introduction are stopped, and nitrogen is continued to be introduced until the temperature drops to room temperature.

[0039] (4) After the reaction is completed, the hot wire is removed from the copper foil plate, placed in the opposite direction, and re-fixed, and the annealing and deposition steps are performed again.

[0040] (5) After the reaction furnace is cooled to room temperature, the reaction plate is taken out, the hot wire is removed, and the surface of the hot wire is cleaned with an air gun. The portion of the hot wire to which graphene is not attached is cut off, leaving only the portion with graphene deposited, which is the hot wire for the thermal conductivity detector.

[0041] Example 2

[0042] This embodiment provides a hot wire for a thermal conductivity detector, wherein the raw material of the hot wire is a rhenium tungsten wire with a diameter of 50 μm and a rhenium content of 3%. The specific preparation method is as follows:

[0043] (1) Etching of rhenium tungsten wire:

[0044] 1. First, pickle with a mixture of nitric acid and sulfuric acid at room temperature for 30 minutes;

[0045] 2. Use oxygen plasma etching at room temperature for 20 minutes, and the plasma power is 50w;

[0046] 3. Etch with a mixture of nitric acid, sulfuric acid, hydrochloric acid, hydrofluoric acid, deionized water, and buffer NH4F for 30 minutes at room temperature;

[0047] 4. Use oxygen plasma etching at 500°C for 20 minutes, with a plasma power of 50W;

[0048] (2) The etched rhenium tungsten wire was fixed on a copper foil plate, marked and oriented, named a reaction plate, and the reaction plate was ultrasonically treated with acetone and deionized water for 10 min in turn, and then nitrogen was introduced for annealing, with the flow rate set to 100 sccm, the annealing temperature set to 1000°C, and the time set to 30 min.

[0049] (3) After annealing, methane is introduced for chemical vapor deposition to grow graphene. The deposition temperature is set to 1050°C, the time is set to 1 hour, and the methane flow rate accounts for 1% of the total gas flow rate. After the reaction is completed, heating and methane introduction are stopped, and nitrogen is continued to be introduced until the temperature drops to room temperature.

[0050] (4) After the reaction is completed, the hot wire is removed from the copper foil plate, placed in the opposite direction, and re-fixed, and the annealing and deposition steps are performed again.

[0051] (5) Platinum was deposited by physical vapor deposition at 10 -2 Argon gas is filled under vacuum conditions of Pa to 10Pa, and argon gas is glow discharged under high voltage to ionize argon atoms into argon ions. Under the action of the electric field force, argon ions are accelerated to bombard the surface of the platinum target, so that the atoms on the target surface gain enough energy to escape, and the target will be sputtered and deposited on the surface of the workpiece. The time is set to 30 minutes, and the deposition thickness is about 50nm.

[0052] (6) After the reaction furnace is cooled to room temperature, the reaction plate is taken out, the hot wire is removed, and the surface of the hot wire is cleaned with an air gun. The portion of the hot wire to which graphene and metal platinum are not attached is cut off, leaving only the portion with graphene and metal platinum deposited, which is the hot wire for the thermal conductivity detector.

[0053] Example 3

[0054] This embodiment provides a hot wire for a thermal conductivity detector, wherein the raw material of the hot wire is a tungsten wire with a diameter of 200 μm, and the specific preparation method is as follows:

[0055] (1) Etching of tungsten wire:

[0056] 1. First, pickle with a mixture of nitric acid and sulfuric acid at room temperature for 30 minutes;

[0057] 2. Use oxygen plasma etching at room temperature for 20 minutes, and the plasma power is 50w;

[0058] 3. Etch with a mixture of nitric acid, sulfuric acid, hydrochloric acid, hydrofluoric acid, deionized water, and buffer NH4F for 30 minutes at room temperature;

[0059] 4. Use oxygen plasma etching at 500°C for 20 minutes, with a plasma power of 50W;

[0060] (2) Fix the etched tungsten wire on the copper foil plate, mark and determine the direction, name it as a reaction plate, and treat the reaction plate with acetone and deionized water ultrasonically for 10 min in turn, then introduce hydrogen for annealing with a flow rate of 20 sccm, an annealing temperature of 400 °C, and a time of 20 min.

[0061] (3) After annealing, methane is introduced for chemical vapor deposition to grow graphene. The deposition temperature is set to 800°C, the time is set to 45 min, and the methane flow rate accounts for 1.5% of the total gas flow rate. After the reaction is completed, heating and methane introduction are stopped, and nitrogen is continued to be introduced until the temperature drops to room temperature.

[0062] (4) After the reaction is completed, the hot wire is removed from the copper foil plate, placed in the opposite direction, and re-fixed, and the annealing and deposition steps are performed again.

[0063] (5) Platinum was deposited by physical vapor deposition at 10 -2 Argon gas is filled under vacuum conditions of Pa to 10Pa, and argon gas is glow discharged under high voltage to ionize argon atoms into argon ions. Under the action of the electric field force, argon ions are accelerated to bombard the surface of the platinum target, so that the atoms on the target surface gain enough energy to escape, and the target will be sputtered and deposited on the surface of the workpiece. The time is set to 30 minutes.

[0064] (6) After the reaction furnace is cooled to room temperature, the reaction plate is taken out, the hot wire is removed, and the surface of the hot wire is cleaned with an air gun. The portion of the hot wire to which graphene and metal platinum are not attached is cut off, leaving only the portion with graphene and metal platinum deposited, which is the hot wire for the thermal conductivity detector.

[0065] Example 4

[0066] This embodiment provides a hot wire for a thermal conductivity detector, wherein the raw material of the hot wire is a stainless steel wire with a diameter of 500 μm, and the specific preparation method thereof is as follows:

[0067] (1) Etching of stainless steel wire:

[0068] 1. First, pickle with a mixture of nitric acid and sulfuric acid at room temperature for 30 minutes;

[0069] 2. Use oxygen plasma etching at room temperature for 20 minutes, and the plasma power is 50w;

[0070] 3. Etch with a mixture of nitric acid, sulfuric acid, hydrochloric acid, hydrofluoric acid, deionized water, and buffer NH4F for 30 minutes at room temperature;

[0071] 4. Use oxygen plasma etching at 500°C for 20 minutes, with a plasma power of 50W;

[0072] (2) The etched stainless steel wire was fixed on a copper foil plate, marked and oriented, named a reaction plate, and the reaction plate was ultrasonically treated with acetone and deionized water for 10 min in turn, and then nitrogen was introduced for annealing, with the flow rate set to 200 sccm, the annealing temperature set to 800 °C, and the time set to 30 min.

[0073] (3) After annealing, methane is introduced for chemical vapor deposition to grow graphene. The deposition temperature is set to 1000° C., the time is set to 65 min, and the methane flow rate accounts for 1% of the total gas flow rate. After the reaction is completed, heating and methane introduction are stopped, and nitrogen is continued to be introduced until the temperature drops to room temperature.

[0074] (4) After the reaction is completed, the hot wire is removed from the copper foil plate, placed in the opposite direction, and re-fixed, and the annealing and deposition steps are performed again.

[0075] (5) Platinum was deposited by physical vapor deposition at 10 -2 Argon gas is filled under vacuum conditions of Pa to 10Pa, and argon gas is glow discharged under high voltage to ionize argon atoms into argon ions. Under the action of the electric field force, argon ions are accelerated to bombard the surface of the platinum target, so that the atoms on the target surface gain enough energy to escape, and the target will be sputtered and deposited on the surface of the workpiece. The time is set to 30 minutes.

[0076] (6) After the reaction furnace is cooled to room temperature, the reaction plate is taken out, the hot wire is removed, and the surface of the hot wire is cleaned with an air gun. The portion of the hot wire to which graphene and metal platinum are not attached is cut off, leaving only the portion with graphene and metal platinum deposited, which is the hot wire for the thermal conductivity detector.

[0077] Example 5

[0078] This embodiment provides a hot wire for a thermal conductivity detector, the raw material of which is a copper wire with a diameter of 5 μm. The specific preparation method is as follows:

[0079] (1) Etching the copper wire:

[0080] 1. First, pickle with a mixture of nitric acid and sulfuric acid at room temperature for 30 minutes;

[0081] 2. Use oxygen plasma etching at room temperature for 20 minutes, and the plasma power is 50w;

[0082] 3. Etch with a mixture of nitric acid, sulfuric acid, hydrochloric acid, hydrofluoric acid, deionized water, and buffer NH4F for 30 minutes at room temperature;

[0083] 4. Use oxygen plasma etching at 500°C for 20 minutes, with a plasma power of 50W;

[0084] (2) The etched copper wire was fixed on a copper foil plate, marked and oriented, and named as a reaction plate. The reaction plate was ultrasonically treated with acetone and deionized water for 10 min in turn, and then nitrogen was introduced for annealing. The flow rate was set to 80 sccm, the annealing temperature was set to 700 °C, and the time was set to 25 min.

[0085] (3) After annealing, methane is introduced for chemical vapor deposition to grow graphene. The deposition temperature is set to 1200° C., the time is set to 50 min, and the methane flow rate accounts for 2% of the total gas flow rate. After the reaction is completed, heating and methane introduction are stopped, and nitrogen is continued to be introduced until the temperature drops to room temperature.

[0086] (4) After the reaction is completed, the hot wire is removed from the copper foil plate, placed in the opposite direction, and re-fixed, and the annealing and deposition steps are performed again.

[0087] (5) After the reaction furnace is cooled to room temperature, the reaction plate is taken out, the hot wire is removed, and the surface of the hot wire is cleaned with an air gun. The portion of the hot wire to which graphene is not attached is cut off, leaving only the portion with graphene deposited, which is the hot wire for the thermal conductivity detector.

[0088] Comparative Example 1

[0089] In this comparative example, the raw material rhenium tungsten wire in Example 1 is directly used as the heating wire.

[0090] Comparative Example 2

[0091] The difference between this comparative example and Example 1 is that no deposition is performed after the etching process.

[0092] Test Example 1

[0093] The resistance test of the heating wires of Example 1-2 and Comparative Example 1-2 was performed at room temperature (25° C.), and the results are shown in Table 1 below:

[0094] Table 1: Heating wire resistance of the embodiment and the comparative example

[0095] Resistance (Ω) Comparative Example 1 110.4 Comparative Example 2 119.2 Example 1 99.1 Example 2 98.2

[0096] It can be seen from the above table that the hot wire obtained in the embodiment of the present application has lower resistance and its resistivity is better.

[0097] Test Example 2

[0098] The hot wires of Example 1-2 and Comparative Example 1-2 were respectively assembled into a four-arm bridge and connected to a thermal conductivity detection circuit for sensitivity and detection limit tests. The test method was based on GB / T 30431-2020 (with methane in nitrogen as the sample). The results are shown in the following table:

[0099] Table 2 Hot wire sensitivity of the embodiment and the comparative example

[0100]

[0101] Table 3 Hot wire detection limits of the embodiment and comparative example when the bridge current is 180 mA

[0102]

[0103] It can be seen from Tables 2 and 3 that the sensitivity of the hot wire obtained in Example 1 of the present application is significantly higher than that of the comparative examples at different bridge currents, and the detection sensitivity of Example 2 to methane is greatly improved relative to that of Example 1, and the calculated methane detection limit at a bridge current of 180 mA is approximately 0.0094 ppm.

[0104] Test Example 3

[0105] The hot wires of Example 1-2 and Comparative Example 1-2 were respectively assembled into four-arm bridges and connected to a thermal conductivity detection circuit for sensitivity and detection limit tests. The test method was based on GB / T 30431-2020 (using carbon dioxide in nitrogen as a sample). The results are shown in the following table:

[0106] Table 4 Hot wire detection limits of the embodiment and comparative example when the bridge current is 180 mA

[0107]

[0108] It can be seen from the above table that the detection sensitivity of Example 1 and Example 2 of the present application to carbon dioxide in nitrogen is not much different, and both are significantly higher than the control example.

[0109] Test Example 4

[0110] The tensile strength of the hot wires of Example 1 and Comparative Examples 1-2 was tested according to GB / T228.1-2021. The test results are as follows: Figure 1 As shown, it can be seen from the figure that Example 1 has higher tensile strength than the comparative example.

[0111] Test Example 5

[0112] The rhenium tungsten alloy sheet of the same material as that of Example 1 was treated by the scheme in Example 1, and then the treated material and the raw material were subjected to corrosion resistance test according to method B in GB / T24195-2009 / ISO16151:2005. The results are as follows: Figure 2 As shown, it can be seen that the surface of the rhenium tungsten alloy sheet treated by the scheme in Example 1 in (A) has basically no corrosion marks, while the surface of the untreated rhenium tungsten alloy sheet in (B) is severely corroded.

[0113] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.

Claims

1. A method for preparing a hot wire for a thermal conductivity detector, characterized in that: The steps include: S1: Etching the raw material hot wire; S2: Deposition of low-dimensional nanomaterials on the hot wire surface and etched holes; The raw material heating wire is a metal heating wire, including one of rhenium tungsten wire, copper wire, tungsten wire and stainless steel wire; In step S1, the etching forms micrometer or nanometer-scale holes on the surface of the raw material hot wire; The etching includes sequentially performing room temperature pickling, room temperature plasma etching, acid etching solution etching and 500° C. oxygen plasma etching; After depositing the low-dimensional nanomaterial, the method further includes the step of depositing the precious metal.

2. The preparation method according to claim 1, characterized in that: The noble metal includes at least one of gold and platinum, and the deposited thickness is 5-500nm.

3. The preparation method according to claim 1, characterized in that: The low-dimensional nanomaterial includes graphene, molybdenum disulfide or tellurene.

4. The preparation method according to claim 3, characterized in that: The depositing of low-dimensional nanomaterials in step S2 is to deposit graphene using chemical vapor deposition.

5. The preparation method according to claim 4, characterized in that: The graphene deposition is carried out by introducing methane into the protective atmosphere and depositing at 800-1200° C. for 45-75 minutes; the total gas flow rate is 20 sccm-200 sccm, and methane accounts for 1-2% of the total gas flow rate.

6. The preparation method according to claim 5, characterized in that: The method further includes an annealing step before depositing graphene, wherein the annealing step is performed at 350-1000° C. in a protective atmosphere for 20-40 minutes.

7. The preparation method according to claim 6, characterized in that: The protective atmosphere includes at least one of nitrogen, argon and hydrogen.

8. The preparation method according to any one of claims 1 to 7, characterized in that: The diameter of the raw material hot wire is 1-500 μm.

9. A hot wire for a thermal conductivity detector, characterized in that: Prepared by the preparation method according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • High-specific-surface-area boron-doped diamond electrode and preparation method and application thereof

    CN106435518A