Preparation method and application of medium-speed, medium-load, long-life, self-lubricating composite material

By using a combination of PTFE yarns woven with warp and weft yarns and reinforced yarns in the self-lubricating lining of large piling ships, combined with plasma etching and resin coating technology, the problem of existing self-lubricating materials under medium-speed and medium-load conditions has been solved. It solves the problems of high friction and wear and insufficient adhesion performance, and realizes long-life and maintenance-free self-lubricating composite materials, which meets the needs of large piling ships working for a long time at sea.

CN117901533BActive Publication Date: 2024-10-22CCCC SECOND HARBOR ENGINEERING CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311677544.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-08
Publication Date
2024-10-22
Estimated Expiration
2043-12-08

AI Technical Summary

Technical Problem

Existing self-lubricating liner materials are difficult to meet the high friction, wear and adhesion performance requirements of large piling ships under medium-speed and medium-load conditions where large piling ships work for long periods at sea, and there are problems with environmental pollution and complex processes.

Method used

A combination of PTFE yarns woven with warp and weft yarns and reinforced yarns are plasma etched and coated with epoxy resin and phenolic resin to form a unique self-lubricating composite material, which is used for spherical bearing linings to improve its friction and wear properties. and adhesive strength.

Benefits of technology

It achieves an operating life of more than 800 hours under medium-speed and medium-load conditions with a load of 90MPa, a swing frequency of 1.2Hz, and a swing angle of ±30° at normal temperature, and meets the requirements of peel strength ≥1.0N/mm, reducing repairs and maintenance. , achieving the effect of long-term maintenance-free operation, and at the same time, the operation is simple and there is no waste liquid pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117901533B_ABST
    Figure CN117901533B_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a medium-speed medium-load long-life, self-lubricating composite material, which relates to the field of self-lubricating materials. The preparation method comprises the following steps: S1. Weaving a fabric with warp yarn and weft yarn, wherein the warp yarn is a single-twisted PTFE yarn, and the weft yarn is a reinforcing yarn; S2. Plasma etching treatment is performed, and then epoxy resin slurry is coated on the working surface of the fabric, and a film formed by phenolic resin slurry is pasted on the pasting surface of the fabric; S3. After drying and pre-curing, a composite material in a pre-pressed state is obtained; S4. The pasting surface of the composite material obtained in step S3 is pasted to a metal substrate correspondingly, and the self-lubricating composite material is cured and formed. The flat peel strength of the composite material of the invention is ≥1.0N / mm, and the wear life under medium-speed and medium-load conditions is more than 800h, which can achieve the purpose of long-term operation and maintenance-free maintenance of large-size bearings at sea.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a self-lubricating material, in particular to a method for preparing a medium-speed, medium-load, long-life self-lubricating composite material and an application thereof in a spherical bearing. Background Art

[0002] Bearings are the core components of mechanical equipment and are known as the "joints" in the industrial field. The various performances of bearings directly affect the function and service life of the equipment. Spherical plain bearings are sliding bearings with the characteristics of surface contact, high load-bearing capacity, and adjustable center. They are widely used in various mechanical equipment. Self-lubricating spherical plain bearings are increasingly favored by various customers due to their self-lubricating and maintenance-free characteristics, and have become the development direction and value core of spherical plain bearings. Typical model GE30ET-2RS spherical plain bearings are as follows: Figure 1 As shown, it is composed of an outer steel ring 1, an inner steel ring 2, and a self-lubricating pad 3 which is pasted on the inner surface of the outer steel ring 1 and plays a lubricating role.

[0003] In recent years, large pile-driving vessels such as Xiongsheng Pile 17, Shuixinqi 1, and Yihangjin Pile have been officially put into construction. The luffing cylinders of various pile-driving vessels have adopted self-lubricating spherical bearings, such as the GEH700HTL / KY self-lubricating spherical bearings used in Shuixinqi 1. When large pile-driving vessels are working at sea, they need to work for a long time due to the particularity of their working environment, and it is difficult to maintain them. For the medium-speed and medium-load conditions with a load of 90MPa, a swing frequency of 1.2Hz, a swing angle of ±30° at normal temperature, and an operating life of more than 800h (3.456 million times), the existing self-lubricating liner materials are difficult to meet.

[0004] CN202010813774.1 provides a preparation method and a self-lubricating gasket, which adopts a plasma treatment method, but the object treated is a PTFE membrane, and its main effect is: providing more anti-friction medium for the self-lubricating spherical bearing, and the friction coefficient is lower in the initial state, but there is no clear working condition, and there is no long-term working characteristic; CN202110380861.7 provides an aramid III fiber reinforced self-lubricating gasket composite material and a preparation method thereof, which adopts chemical agents to modify the fabric, the process is complicated and easily produces excessive waste liquid to pollute the environment, and it is only suitable for low-frequency working conditions, that is, low-speed and heavy-load working conditions with a load of 250MPa, a swing frequency of 0.2Hz, and a swing angle of ±25° at room temperature, rather than medium and high frequency working conditions, and the number of operations is only 25,000 times, there is no life test data, and it cannot meet the needs of long-term operation.

[0005] Therefore, it is necessary to develop a long-life, self-lubricating, maintenance-free self-lubricating composite material, which can be used in the spherical bearings of the variable-length cylinder. It can not only meet the friction and wear performance requirements - the operating life is ≥800h with a load of 90MPa, a swing frequency of 1.2Hz, and a swing angle of ±30° under normal working temperature, but also meet the adhesion performance requirements - the peel strength is above 1.0N / mm, achieving the effect of long-term maintenance-free operation, reducing the repair and maintenance of the variable-length cylinder, and meeting its long-term work needs at sea. Summary of the invention

[0006] The purpose of the present invention is to solve the shortcomings of the above-mentioned background technology and to provide a long-life, self-lubricating, maintenance-free self-lubricating composite material, which is used in the spherical bearings of the variable-length oil cylinder. It can not only meet the friction and wear performance requirements - the operating life of the load is 90MPa, the swing frequency is 1.2Hz, and the swing angle is ±30° at room temperature is ≥800h, but also meet the adhesion performance requirements - the peel strength is above 1.0N / mm, so as to achieve the effect of long-term maintenance-free operation, reduce the repair and maintenance of the variable-length oil cylinder, and meet its long-term work needs at sea.

[0007] The technical solution of the present invention is: a method for preparing a medium-speed, medium-load, long-life, self-lubricating composite material, characterized by comprising the following steps:

[0008] S1. The fabric is woven by warp yarn and weft yarn, the warp yarn is a single-twisted PTFE yarn, and the weft yarn is a reinforcing yarn;

[0009] S2. Plasma etching is performed on the fabric obtained in step S1, and then epoxy resin slurry is coated on the working surface of the fabric, and a film formed by phenolic resin slurry is pasted on the pasting surface of the fabric, wherein the epoxy resin slurry formula includes the following raw materials in percentage by mass:

[0010]

[0011]

[0012] The functional powder is a mixture of graphene and silicon nitride in a mass ratio of 1:2 to 16, the solvent is ethanol or ethyl acetate, and the sum of the mass percentages of the nitrile-modified epoxy resin, graphite, functional powder, fumed silica, phthalic anhydride, and solvent is 100%;

[0013] S3. After drying and pre-curing, a composite material in a pre-pressed state is obtained;

[0014] S4. Paste the bonding surface of the composite material obtained in step S3 to the corresponding metal substrate, and solidify and shape to obtain a self-lubricating composite material.

[0015] Preferably, in step S1, the linear density of the PTFE yarn is 400±50D, the reinforcing yarn is one or more of cotton yarn, polyester fiber, and Kevlar fiber, and the weaving structure is a satin structure or a double weft structure. The linear density of 400±50D is 350-450D.

[0016] Preferably, in step S2, the plasma etching time is 10 to 40 minutes, the processing temperature is 20 to 35° C., and the system vacuum degree is 30 to 50 Pa.

[0017] Preferably, in step S2, the epoxy resin slurry formula includes the following raw materials in percentage by mass:

[0018]

[0019] Preferably, in step S3, the drying temperature is 40-50°C, the drying time is 2-3h, the pre-pressing temperature is 60-70°C, the pre-pressing time is 0.5-1h, and the pre-pressing pressure is 2-3MPa.

[0020] Preferably, in step S4, the curing temperature is 160° C. to 180° C., and the time is 2 h to 6 h.

[0021] Furthermore, the curing temperature is 170°C and the time is 3 hours.

[0022] The present invention also provides a self-lubricating composite material, which is prepared by any of the above methods for preparing the medium-speed, medium-load, long-life self-lubricating composite material.

[0023] Preferably, the peel strength of the self-lubricating composite material is ≥1.0N / mm, and when the composite material is used as a spherical bearing liner, the spherical bearing has an operating life of ≥800h under medium-speed and medium-load conditions with a load of 90MPa, a swing frequency of 1.2Hz, and a swing angle of ±30° at room temperature.

[0024] The present invention also provides one or more applications of the self-lubricating composite material on a spherical bearing, wherein the self-lubricating composite material is applied as a self-lubricating liner of the spherical bearing.

[0025] The PTFE yarn of the composite material of the present invention is made by a single yarn twisting process. The PTFE yarn is brown or brown yarn, which is made by high-temperature sintering of an emulsion during spinning. The cross section is elliptical or circular. The PTFE yarn has the characteristic of low friction, and mainly plays a role in reducing friction in the system. It is easy to form a transfer film during the friction and wear process, plays a role of self-lubrication, and can also extend the service life of the bearing. The reinforcing yarn is one or more of cotton yarn, polyester fiber, and Kevlar fiber. These three fibers mainly play a supporting role, have a good bearing effect, and at the same time improve the adhesion of the system, improve its peeling strength, and ensure that the composite material is not squeezed out or damaged when it works for a long time.

[0026] The fabric is woven from PTFE yarn and reinforcing yarn, the working surface of the fabric is impregnated with modified epoxy resin, and the adhesive surface is adhesively bonded with special phenolic resin. The synergistic effect of the two resins improves the adhesive state and friction and wear performance of the composite material, achieves the effect of long-term maintenance-free operation, reduces the repair and maintenance of the variable amplitude oil cylinder, and meets the requirements of long-term operation at sea.

[0027] The object of the plasma treatment used in the present invention is a fabric containing PTFE yarn rather than a PTFE membrane. The operation is simple, no waste liquid is generated, and there is almost no impact on the environment. At the same time, the system has good thermal conductivity through formula design and is suitable for medium and high frequency working conditions, that is, medium speed and medium load conditions with a load of 90MPa, a swing frequency of 1.2Hz, and a swing angle of ±30° at room temperature. The operating life can reach more than 800h (3.456 million times), which can meet the needs of long-term maintenance-free operation.

[0028] The surface etching treatment of the present invention is carried out by a plasma treatment system composed of hydrogen and argon. Due to the high crystallinity and non-polarity of PTFE, it has very low surface energy, resulting in poor wettability of PTFE. After the plasma surface etching treatment is carried out, the activity of the surface is improved, the wettability of the fabric and the resin is improved, and due to its low friction characteristics, the long-term operation ability of the bearing can be well maintained.

[0029] The beneficial effects of the present invention are:

[0030] 1. The PTFE yarn of the present invention mainly plays a role in reducing friction in the system, and easily forms a transfer film during the friction and wear process, plays a role in self-lubrication and can also extend the service life of the bearing. The reinforcing yarn mainly plays a role in the support, has a good load-bearing effect, and at the same time improves the adhesion of the system, improves its peeling strength, and ensures that the composite material is not squeezed out or damaged during long-term operation. The satin structure or the double-weft structure makes the fabric itself have more cavities, which is easier to impregnate more resin, improve wear resistance, and extend the service life of the bearing.

[0031] 2. The present invention designs a unique epoxy resin slurry. The addition of graphite and graphene in the formula can improve the heat dissipation of the system during operation, and the addition of silicon nitride and fumed silica can improve the wear resistance of the composite material and extend its service life. The main resin adopts epoxy resin modified by nitrile rubber, which has the advantages of good toughness and strong bearing capacity. The role of phthalic anhydride is to promote the curing of the system, and the role of the solvent is to disperse the system powder.

[0032] 3. The phenolic resin slurry used in the present invention is a modified special phenolic resin, which contains long-chain cashew phenolic resin and has the advantage of good wear resistance.

[0033] 4. The present invention performs plasma surface etching treatment on the fabric. Due to the high crystallinity and non-polarity of PTFE, it has very low surface energy, resulting in poor wettability of PTFE. After the plasma surface etching treatment, its surface activity is improved, and the wettability of the fabric and the resin is improved. Due to its low friction characteristics, the long-term operation ability of the bearing can be well maintained.

[0034] 5. The composite material plate of the present invention has a peel strength of ≥1.0N / mm and is applied to a typical bearing GE30ET-2RS to carry out a friction and wear performance test. The test conditions are a load of 90MPa, a swing frequency of 1.2Hz, and a swing angle of ±30° at room temperature. The wear life is more than 800h, which can achieve the purpose of long-term maintenance-free operation of large-size bearings at sea.

[0035] 6. The present invention is easy to operate, produces no waste liquid, and has almost no impact on the environment. The prepared composite material can meet the characteristics of long-term maintenance-free operation. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 Schematic diagram of the existing bearing joint structure

[0037] Figure 2 Schematic diagram of the peel strength test in Example 1

[0038] Figure 3 The peel strength test curve in Example 1

[0039] Figure 4 The surface conditions before and after the life test of the spherical bearing in Example 1

[0040] Figure 5 This is a curve diagram of the life test of the spherical bearing in Example 1.

[0041] Figure 6 Schematic diagram of the peel strength test in Example 2

[0042] Figure 7 The peel strength test curve in Example 2

[0043] Figure 8 The surface conditions before and after the life test of the spherical bearing in Example 2

[0044] Fig. 9 This is the life test curve of the spherical bearing in Example 2

[0045] Among them: 1-outer steel ring 2-inner steel ring 3-self-lubricating gasket. DETAILED DESCRIPTION

[0046] The following specific examples further illustrate the present invention in detail. The following specific examples further illustrate the present invention in detail. The drugs used in the examples are all commercially available products unless otherwise specified, and the methods used are all conventional methods in the art unless otherwise specified. In this example, PTFE yarn, weft yarn, and phenolic resin are all commercially available products.

[0047] Example 1

[0048] This embodiment provides a method for preparing a medium-speed, medium-load, long-life, self-lubricating composite material, comprising the following steps:

[0049] S1. A fabric is woven using warp yarn and weft yarn, wherein the warp yarn is a single-twisted PTFE yarn, and the weft yarn is a reinforcing yarn. In this embodiment, the warp yarn is a single-twisted 415D PTFE yarn (twist 100 twists / m), and the weft yarn is a cotton yarn, and the fabric is woven using a satin structure;

[0050] S2. The fabric obtained in step S1 is subjected to plasma etching treatment, the ion treatment system treatment time is 20min, the treatment temperature is 25°C, and the system vacuum degree is 35Pa;

[0051] Then, epoxy resin slurry is applied on the working surface of the fabric, and a film formed by phenolic resin slurry is pasted on the pasting surface of the fabric. The epoxy resin slurry formula includes the following raw materials in percentage by mass:

[0052]

[0053]

[0054] S3. After drying and pre-curing, the drying conditions are 45°C × 2h and the pre-curing conditions are 60°C × 0.5h × 2MPa to obtain a composite material in a pre-pressed state;

[0055] S4. Cut the composite material obtained in step S3, and the cutting direction is the direction of 45° clockwise rotation with respect to the PTFE warp direction (hereinafter referred to as left oblique direction). The cut gaskets are respectively pasted on a 120mm×20mm stainless steel plate and a typical model GE30ET-2RS for curing (the gasket pasting surface is the surface where the phenolic resin film is located), and the curing molding temperature is 165°C, the time is 4h, and the heating rate is 2.5°C / min.

[0056] Peel strength test: The stainless steel plate with composite material is tested on an electronic universal testing machine under the conditions of GJB5502. The test temperature is room temperature, the speed is 19.05mm / min, and the peel strength data is 1.45N / mm. The test sample is as follows Figure 2 The test curve is shown as Figure 3 As shown. Figure 2 , Figure 3 It can be seen that the peeling force is large in the stable stage of the peeling test, indicating that the product of the present invention has the advantage of high peeling strength and very good peeling perfection, almost reaching 100%.

[0057] Spherical bearing life test: After curing, the GE30ET-2RS spherical bearing was tested on a constant load spherical bearing life tester. Under medium speed and medium load conditions (load 90MPa at room temperature, swing frequency 1.2Hz, swing angle ±30°), the operating life was 962h, which is greater than the 800h standard of GJB5502. The test sample is shown in the figure below. Figure 4 The test curve is shown as Figure 5 As shown. Figure 4 , Figure 5 It can be seen that in the stable stage of friction and wear, the friction coefficient and friction torque are stable without obvious fluctuations, indicating that the product of the present invention has the advantage of long-term wear resistance.

[0058] Example 2

[0059] This embodiment provides a method for preparing a medium-speed, medium-load, long-life, self-lubricating composite material, comprising the following steps:

[0060] S1. A fabric is woven using warp yarn and weft yarn, wherein the warp yarn is a single-twisted PTFE yarn, and the weft yarn is a reinforcing yarn. In this embodiment, the warp yarn is a single-twisted 398D PTFE yarn (twist 100 twists / m), and the weft yarn is a cotton yarn, and the fabric is woven using a double weft structure;

[0061] S2. The fabric obtained in step S1 is subjected to plasma etching treatment, the ion treatment system treatment time is 20min, the treatment temperature is 25°C, and the system vacuum degree is 35Pa;

[0062] Then, epoxy resin slurry is applied on the working surface of the fabric, and a film formed by phenolic resin slurry is pasted on the pasting surface of the fabric. The epoxy resin slurry formula includes the following raw materials in percentage by mass:

[0063]

[0064] S3. After drying and pre-curing, the drying conditions are 45°C × 2h and the pre-curing conditions are 60°C × 0.5h × 2MPa to obtain a composite material in a pre-pressed state;

[0065] S4. Cut the composite material obtained in step S3 in a left oblique direction. The cut gaskets are respectively pasted on a 120mm×20mm stainless steel plate and a typical model GE30ET-2RS for curing (the gasket pasting surface is the surface where the phenolic resin film is located), the curing molding temperature is 170°C, the time is 3h, and the heating rate is 2.0°C / min.

[0066] Peel strength test: The stainless steel plate with gasket is tested on an electronic universal testing machine under the conditions of GJB5502. The test temperature is room temperature, the speed is 19.05mm / min, and the peel strength data is 1.54N / mm. The test sample is as follows Figure 6 The test curve is shown as Figure 7 As shown. Figure 6 , Figure 7 It can be seen that the peeling force is large in the stable stage of the peeling test, indicating that the product of the present invention has the advantage of high peeling strength and very good peeling perfection, almost reaching 100%.

[0067] Spherical bearing life test: After curing, the spherical bearing GE30ET-2RS was tested on a constant load spherical bearing life tester. Under medium speed and medium load conditions (load 90MPa at room temperature, swing frequency 1.2Hz, swing angle ±30°), the operating life was 1266h, which is greater than the 800h standard of GJB5502. The test sample is shown in the figure below. Figure 8 The test curve is shown as Fig. 9 As shown. Figure 8 , Fig. 9 It can be seen that in the stable stage of friction and wear, the friction coefficient and friction torque are stable without obvious fluctuations, indicating that the product of the present invention has the advantage of long-term wear resistance.

Claims

1. A method for preparing a medium-speed, medium-load, long-life, self-lubricating composite material. It is characterized in that The following steps are involved: S1. A fabric is woven using warp yarn and weft yarn, wherein the warp yarn is a single-twisted PTFE yarn, the weft yarn is a reinforcing yarn, the linear density of the PTFE yarn is 400±50D, the reinforcing yarn is one or more of cotton yarn, polyester fiber, and Kevlar fiber, and the weaving structure is a satin structure or a double weft structure; S2. The fabric obtained in step S1 is subjected to plasma etching treatment, wherein the plasma etching time is 10-40 min, the treatment temperature is 20-35° C., and the system vacuum degree is 30-50 Pa. Then, epoxy resin slurry is applied on the working surface of the fabric, and a film formed by phenolic resin slurry is attached to the adhesive surface of the fabric. The epoxy resin slurry formula includes the following raw materials in mass percentage: Nitrile modified epoxy resin 80~90%, Graphite 5.0~15.0%, Functional powder 0.2~1.2%, Fumed silica 2.0~5.0%, Phthalic anhydride 0.05~2%, Solvent 2.0~10.0%, The functional powder is a mixture of graphene and silicon nitride in a mass ratio of 1:2-16, the solvent is ethanol or ethyl acetate, and the sum of the mass percentages of the nitrile-modified epoxy resin, graphite, functional powder, fumed silica, phthalic anhydride, and solvent is 100%; S3. After drying and pre-curing, a composite material in a pre-pressed state is obtained; S4. Paste the bonding surface of the composite material obtained in step S3 to the corresponding metal substrate, and solidify and shape to obtain a self-lubricating composite material.

2. The method for preparing the medium-speed, medium-load, long-life, self-lubricating composite material according to claim 1, It is characterized in that In step S2, the epoxy resin slurry formula includes the following raw materials in percentage by mass: Nitrile modified epoxy resin 84~85%, Graphite 8.0~10.0%, Functional powder 0.85~0.9%, Fumed silica 2.0~3.0%, Phthalic anhydride 0.1~0.15%, Solvent 2.0~5.0%.

3. The method for preparing the medium-speed, medium-load, long-life, self-lubricating composite material according to claim 1, It is characterized in that In step S3, the drying temperature is 40-50°C, the drying time is 2-3h, the pre-pressing temperature is 60-70°C, the pre-pressing time is 0.5-1h, and the pre-pressing pressure is 2-3MPa.

4. The method for preparing the medium-speed, medium-load, long-life, self-lubricating composite material according to claim 1, It is characterized in that In step S4, the curing temperature is 160°C to 180°C, and the time is 2h to 6h.

5. The method for preparing the medium-speed, medium-load, long-life, self-lubricating composite material according to claim 4, It is characterized in that The curing temperature is 170°C and the time is 3 hours.

6. A self-lubricating composite material, It is characterized in that The composite material is prepared by the method for preparing a medium-speed, medium-load, long-life, self-lubricating composite material as described in any one of claims 1 to 5.

7. The composite material according to claim 6, It is characterized in that The self-lubricating composite material has a peel strength of ≥1.0 N / mm. When the self-lubricating composite material is used as a spherical bearing liner, the spherical bearing has an operating life of ≥800 h under medium-speed and medium-load conditions with a load of 90 MPa, a swing frequency of 1.2 Hz, and a swing angle of ±30° at room temperature.

8. Use of the composite material as claimed in claim 6 or 7 in a spherical bearing, It is characterized in that The self-lubricating composite material is applied as a self-lubricating liner of a spherical bearing.