A highly breathable flash-evaporated sheet and a method for manufacturing the same

By using a combination of doped CNT graphene aerogel and polyethylene in the flash sheet, using a high-pressure reactor and hot rolling process, the problem of low unit air permeability of the flash sheet is solved and high air permeability is achieved. Improved and maintained the stability of other performance.

CN117904795BActive Publication Date: 2024-10-11JIANGSU QINGYUN NEW MATERIAL TECH CO LTD
View PDF 16 Cites 0 Cited by

Patent Information

Application Number
CN202410319867.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-20
Publication Date
2024-10-11
Estimated Expiration
2044-03-20

AI Technical Summary

Technical Problem

The unit air permeability of existing flash evaporated sheets is not ideal, making it difficult to meet market demand.

Method used

Doped CNT graphene aerogel is used as breathable particles. It is cut and crushed and then dispersed with polyethylene in a spinning solvent. Highly breathable flash sheets are prepared through high-pressure reactor treatment and hot rolling processes.

Benefits of technology

The unit air permeability of the flash evaporated sheet is significantly improved, while the performance in terms of tensile strength and elongation is not affected, meeting market demand.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117904795B_ABST
    Figure CN117904795B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of flash textile technology, and in particular to a highly breathable flash sheet and a manufacturing method thereof. Aiming at the problem that the unit air permeability of flash sheets in the prior art is generally not ideal and needs to be further improved, the present invention provides a highly breathable flash sheet and a manufacturing method thereof, comprising polyethylene, wherein the unit air permeability of the flash sheet is 12 to 31 (s•mm 3 ) / mg; unit air permeability = (air permeability * thickness) / gram weight; the test standard for air permeability is ISO 5636‑5. The present invention provides a highly air-permeable flash-steamed sheet having a high unit air permeability, which can meet relevant market demands. At the same time, the present invention finds that after the crushed CNT graphene aerogel is applied to the preparation process of the flash-steamed sheet, the prepared flash-steamed sheet has a significant improvement in unit air permeability, while the performance of the flash-steamed sheet in other aspects, such as tensile strength, tensile elongation, etc., is not significantly affected.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of flash textiles, and in particular relates to a highly breathable flash sheet and a manufacturing method thereof. Background Art

[0002] Flash spinning technology, polymer spinning and then spunbonding process to make non-woven fabrics, this technology was invented by DuPont in the United States in 1955, named and patented in 1956. It is mainly reflected in US3081519A, US3169899A, US3860369A, which is DuPont's underlying core patent and has been cited more than 200 times. Around the 1980s, Asahi Kasei Corporation of Japan successfully developed a similar product, the trade name is "Suxer", flash sheet combines the material characteristics of cloth, paper and film.

[0003] For flash-steamed sheets, unit air permeability is an important performance index, but the unit air permeability of flash-steamed sheets in the prior art is generally not ideal and needs to be further improved.

[0004] For example, the Chinese invention patent application discloses a breathable flash-evaporated composite sheet and its manufacturing method [application number: 202210443208.5]. The invention application includes polyethylene; the water vapor transmission rate of the composite sheet is greater than 800g / (m·24h); the total luminous flux transmittance of the composite sheet is 6~20%; the initial nail rod tear strength F0 of the composite sheet is 40~65N; I=(F0-F1) / F0*100%; I is 2~30%; F0 is the initial nail rod tear strength of the composite sheet; F1 is the aged nail rod tear strength; the hot air aging test is: place the sample horizontally in an 80℃ oven for 672 hours, take it out and place it for 24 hours, and test the nail rod tear strength of the composite sheet again, which is counted as the aged nail rod tear strength.

[0005] This invention conducts relevant research on improving the water vapor transmission performance of flash-steamed composite sheets, but it still does not solve the problem of how to improve the unit air permeability of flash-steamed sheets. Summary of the invention

[0006] The object of the present invention is to provide a highly breathable flash sheet with a higher specific air permeability in view of the above problems.

[0007] Another object of the present invention is to provide a method for manufacturing a highly breathable flash sheet with a higher specific air permeability in order to solve the above problems.

[0008] In order to achieve the above object, the present invention adopts the following technical solutions:

[0009] A highly air-permeable flash sheet material, comprising polyethylene, wherein the unit air permeability of the flash sheet material is 12 to 31 (s•mm 3 ) / mg;

[0010] Unit air permeability = (air permeability * thickness) / gram weight;

[0011] The test standard for air permeability is ISO 5636-5.

[0012] In the above-mentioned high air permeability flash sheet, the unit air permeability of the flash sheet is 12 to 15 (s•mm 3 ) / mg.

[0013] In the above-mentioned highly permeable flash-steamed sheet, the unit air permeability of the flash-steamed sheet is 15 to 17 (s•mm 3 ) / mg.

[0014] In the above-mentioned high air permeability flash sheet, the unit air permeability of the flash sheet is 17 to 19 (s•mm 3 ) / mg.

[0015] In the above-mentioned high air permeability flash-steamed sheet, the unit air permeability of the flash-steamed sheet is 19 to 21 (s•mm 3 ) / mg.

[0016] In the above-mentioned high air permeability flash-steamed sheet, the unit air permeability of the flash-steamed sheet is 21 to 23 (s•mm 3 ) / mg.

[0017] In the above-mentioned highly permeable flash-steamed sheet, the unit air permeability of the flash-steamed sheet is 23-25 ​​(s•mm 3 ) / mg.

[0018] In the above-mentioned high air permeability flash-steamed sheet, the unit air permeability of the flash-steamed sheet is 25-27 (s•mm 3 ) / mg.

[0019] In the above-mentioned highly permeable flash-steamed sheet, the unit air permeability of the flash-steamed sheet is 27 to 29 (s•mm 3 ) / mg.

[0020] In the above-mentioned high air permeability flash-steamed sheet, the unit air permeability of the flash-steamed sheet is 29-31 (s•mm 3 ) / mg.

[0021] In the above-mentioned highly air-permeable flash-steamed sheet, the raw materials of the flash-steamed sheet include polyethylene and air-permeable particles, and the mass fraction of the air-permeable particles in the flash-steamed sheet is 5-8%.

[0022] A method for preparing the above-mentioned highly breathable flash-evaporated sheet comprises the following steps:

[0023] Step 1: Mix dichloromethane, 1,1-dichloro-2,2,2-trifluoroethane, monochlorodichloromethane and 1H-perfluorohexane in a mass ratio of 6:2:1:1 to obtain a spinning solvent, and disperse polyethylene and air-permeable particles in the spinning solvent to obtain a spinning mixture;

[0024] The air permeable particles are prepared by cutting and crushing CNT-doped graphene aerogel with a diameter of 1.2 cm and then passing through a 300-mesh sieve;

[0025] Step 2: Transfer the spinning mixture obtained in step 1 to a high-pressure reactor, and then heat it to 160-180° C.; after the heating is completed, introduce nitrogen and pressurize it to 12.5-13 MPa; finally heat it to 200-230° C. to obtain a flash spinning solution;

[0026] Step 3: flash-spinning the flash spinning solution through a spinning assembly to obtain flash-spun fibers, and the flash-spun fibers are laid on a web and then pre-pressed by at least two sets of pre-pressing rollers;

[0027] Step 4: After pre-pressing, the sheet is hot-rolled by at least three groups of hot-rolling rollers, and then calendered and wound to obtain a highly air-permeable flash-steamed sheet.

[0028] Compared with the prior art, the advantages of the present invention are:

[0029] 1. The present invention provides a highly air-permeable flash-evaporation sheet material having a relatively high unit air permeability and can meet relevant market demands.

[0030] The present invention finds that when the crushed CNT graphene aerogel is applied to the preparation process of the flash-steamed sheet, the unit air permeability of the prepared flash-steamed sheet is greatly improved. At the same time, the performance of the flash-steamed sheet in other aspects, such as tensile strength and tensile elongation, is not significantly affected. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is a scanning electron microscope micrograph of the product in Example 3; DETAILED DESCRIPTION

[0032] The present invention will be further described in detail below with reference to the accompanying drawings and specific implementation methods.

[0033] Example 1

[0034] This embodiment provides a highly air-permeable flash-evaporated sheet and a preparation method thereof. The raw materials of the flash-evaporated sheet include polyethylene and air-permeable particles, and the mass fraction of the air-permeable particles in the flash-evaporated sheet is 5%.

[0035] Highly breathable flash sheets are prepared by the following method:

[0036] Step 1: Mix dichloromethane, 1,1-dichloro-2,2,2-trifluoroethane, monochlorodichloromethane and 1H-perfluorohexane in a mass ratio of 6:2:1:1 to obtain a spinning solvent, and disperse polyethylene and air-permeable particles in the spinning solvent to obtain a spinning mixture;

[0037] The air permeable particles are prepared by cutting and crushing CNT-doped graphene aerogel with a diameter of 1.2 cm and then passing through a 300-mesh sieve;

[0038] Step 2: Transfer the spinning mixture obtained in step 1 to a high-pressure reactor, and then heat it to 160° C.; after the heating is completed, introduce nitrogen and pressurize it to 12.5 MPa; finally, heat it to 200° C. to obtain a flash spinning solution;

[0039] Step 3: flash-spinning the flash spinning solution through a spinning assembly to obtain flash-spun fibers, and the flash-spun fibers are laid on a web and then pre-pressed by at least two sets of pre-pressing rollers;

[0040] Step 4: After pre-pressing, the sheet is hot-rolled by at least three groups of hot-rolling rollers, and then calendered and wound to obtain a highly air-permeable flash-steamed sheet.

[0041] The air permeability of the prepared high air permeability flash sheet is tested according to the test standard described in ISO 5636-5 and according to the following formula:

[0042] Unit air permeability = (air permeability * thickness) / gram weight;

[0043] The specific air permeability of the highly air-permeable flash-evaporated sheet is calculated.

[0044] The doped CNT graphene aerogels in the present invention all adopt the same commercially available products.

[0045] Example 2

[0046] This embodiment provides a highly air-permeable flash-evaporated sheet and a preparation method thereof. The raw materials of the flash-evaporated sheet include polyethylene and air-permeable particles, and the mass fraction of the air-permeable particles in the flash-evaporated sheet is 8%.

[0047] Highly breathable flash sheets are prepared by the following method:

[0048] Step 1: Mix dichloromethane, 1,1-dichloro-2,2,2-trifluoroethane, monochlorodichloromethane and 1H-perfluorohexane in a mass ratio of 6:2:1:1 to obtain a spinning solvent, and disperse polyethylene and air-permeable particles in the spinning solvent to obtain a spinning mixture;

[0049] The air permeable particles are prepared by cutting and crushing CNT-doped graphene aerogel with a diameter of 1.2 cm and then passing through a 300-mesh sieve;

[0050] Step 2: Transfer the spinning mixture obtained in step 1 to a high-pressure reactor, and then heat it to 180° C.; after the heating is completed, introduce nitrogen and pressurize it to 13 MPa; finally, heat it to 230° C. to obtain a flash spinning solution;

[0051] Step 3: flash-spinning the flash spinning solution through a spinning assembly to obtain flash-spun fibers, and the flash-spun fibers are laid on a web and then pre-pressed by at least two sets of pre-pressing rollers;

[0052] Step 4: After pre-pressing, the sheet is hot-rolled by at least three groups of hot-rolling rollers, and then calendered and wound to obtain a highly air-permeable flash-steamed sheet.

[0053] The air permeability of the prepared high air permeability flash sheet is tested according to the test standard described in ISO 5636-5 and according to the following formula:

[0054] Unit air permeability = (air permeability * thickness) / gram weight;

[0055] The specific air permeability of the highly air-permeable flash-evaporated sheet is calculated.

[0056] Example 3

[0057] This embodiment provides a highly air-permeable flash-evaporated sheet and a preparation method thereof. The raw materials of the flash-evaporated sheet include polyethylene and air-permeable particles, and the mass fraction of the air-permeable particles in the flash-evaporated sheet is 6%.

[0058] Highly breathable flash sheets are prepared by the following method:

[0059] Step 1: Mix dichloromethane, 1,1-dichloro-2,2,2-trifluoroethane, monochlorodichloromethane and 1H-perfluorohexane in a mass ratio of 6:2:1:1 to obtain a spinning solvent, and disperse polyethylene and air-permeable particles in the spinning solvent to obtain a spinning mixture;

[0060] The air permeable particles are prepared by cutting and crushing CNT-doped graphene aerogel with a diameter of 1.2 cm and then passing through a 300-mesh sieve;

[0061] Step 2: Transfer the spinning mixture obtained in step 1 to a high-pressure reactor, and then heat it to 170° C.; after the heating is completed, introduce nitrogen and pressurize it to 12.7 MPa; finally, heat it to 220° C. to obtain a flash spinning solution;

[0062] Step 3: flash-spinning the flash spinning solution through a spinning assembly to obtain flash-spun fibers, and the flash-spun fibers are laid on a web and then pre-pressed by at least two sets of pre-pressing rollers;

[0063] Step 4: After pre-pressing, the sheet is hot-rolled by at least three groups of hot-rolling rollers, and then calendered and wound to obtain a highly air-permeable flash-steamed sheet.

[0064] The air permeability of the prepared high air permeability flash sheet is tested according to the test standard described in ISO 5636-5 and according to the following formula:

[0065] Unit air permeability = (air permeability * thickness) / gram weight;

[0066] The specific air permeability of the highly air-permeable flash-evaporated sheet is calculated.

[0067] The scanning electron microscope micrograph of the highly air-permeable flash-evaporated sheet is shown in FIG. Figure 1 shown.

[0068] Comparative Example 1

[0069] This comparative example provides a flash-evaporated sheet and a preparation method thereof. The raw material of the flash-evaporated sheet includes polyethylene.

[0070] Highly breathable flash sheets are prepared by the following method:

[0071] Step 1: Mix dichloromethane, 1,1-dichloro-2,2,2-trifluoroethane, monochlorodichloromethane and 1H-perfluorohexane in a mass ratio of 6:2:1:1 to obtain a spinning solvent, and disperse polyethylene in the spinning solvent to obtain a spinning mixture;

[0072] Step 2: Transfer the spinning mixture obtained in step 1 to a high-pressure reactor, and then heat it to 170° C.; after the heating is completed, introduce nitrogen and pressurize it to 12.7 MPa; finally, heat it to 220° C. to obtain a flash spinning solution;

[0073] Step 3: flash-spinning the flash spinning solution through a spinning assembly to obtain flash-spun fibers, and the flash-spun fibers are laid on a web and then pre-pressed by at least two sets of pre-pressing rollers;

[0074] Step 4: After pre-pressing, the sheet is hot-rolled by at least three groups of hot-rolling rollers, and then calendered and wound to obtain a highly air-permeable flash-steamed sheet.

[0075] The air permeability of the flash-steamed sheet is tested according to the test standard described in ISO 5636-5 and according to the following formula:

[0076] Unit air permeability = (air permeability * thickness) / gram weight;

[0077] The specific air permeability of the flash-evaporated sheet was calculated.

[0078] Comparative Example 2

[0079] This comparative example provides a flash-steamed sheet and a preparation method thereof. The raw materials of the flash-steamed sheet include polyethylene and air-permeable particles, and the mass fraction of the air-permeable particles in the flash-steamed sheet is 6%.

[0080] Highly breathable flash sheets are prepared by the following method:

[0081] Step 1: Mix dichloromethane, 1,1-dichloro-2,2,2-trifluoroethane, monochlorodichloromethane and 1H-perfluorohexane in a mass ratio of 6:2:1:1 to obtain a spinning solvent, and disperse polyethylene and air-permeable particles in the spinning solvent to obtain a spinning mixture;

[0082] The air permeable particles are prepared by cutting and crushing graphene and then passing through a 300-mesh sieve;

[0083] Step 2: Transfer the spinning mixture obtained in step 1 to a high-pressure reactor, and then heat it to 170° C.; after the heating is completed, introduce nitrogen and pressurize it to 12.7 MPa; finally, heat it to 220° C. to obtain a flash spinning solution;

[0084] Step 3: flash-spinning the flash spinning solution through a spinning assembly to obtain flash-spun fibers, and the flash-spun fibers are laid on a web and then pre-pressed by at least two sets of pre-pressing rollers;

[0085] Step 4: After pre-pressing, the sheet is hot-rolled by at least three groups of hot-rolling rollers, and then calendered and wound to obtain a highly air-permeable flash-steamed sheet.

[0086] The air permeability of the flash-steamed sheet is tested according to the test standard described in ISO 5636-5 and according to the following formula:

[0087] Unit air permeability = (air permeability * thickness) / gram weight;

[0088] The specific air permeability of the flash-evaporated sheet was calculated.

[0089] Comparative Example 3

[0090] This comparative example provides a flash-steamed sheet and a preparation method thereof. The raw materials of the flash-steamed sheet include polyethylene and air-permeable particles, and the mass fraction of the air-permeable particles in the flash-steamed sheet is 2%.

[0091] Highly breathable flash sheets are prepared by the following method:

[0092] Step 1: Mix dichloromethane, 1,1-dichloro-2,2,2-trifluoroethane, monochlorodichloromethane and 1H-perfluorohexane in a mass ratio of 6:2:1:1 to obtain a spinning solvent, and disperse polyethylene and air-permeable particles in the spinning solvent to obtain a spinning mixture;

[0093] The air permeable particles are prepared by cutting and crushing CNT-doped graphene aerogel with a diameter of 1.2 cm and then passing through a 300-mesh sieve;

[0094] Step 2: Transfer the spinning mixture obtained in step 1 to a high-pressure reactor, and then heat it to 170° C.; after the heating is completed, introduce nitrogen and pressurize it to 12.7 MPa; finally, heat it to 220° C. to obtain a flash spinning solution;

[0095] Step 3: flash-spinning the flash spinning solution through a spinning assembly to obtain flash-spun fibers, and the flash-spun fibers are laid on a web and then pre-pressed by at least two sets of pre-pressing rollers;

[0096] Step 4: After pre-pressing, the sheet is hot-rolled by at least three groups of hot-rolling rollers, and then calendered and wound to obtain a highly air-permeable flash-steamed sheet.

[0097] The air permeability of the flash-steamed sheet is tested according to the test standard described in ISO 5636-5 and according to the following formula:

[0098] Unit air permeability = (air permeability * thickness) / gram weight;

[0099] The specific air permeability of the flash-evaporated sheet was calculated.

[0100] Comparative Example 4

[0101] This comparative example provides a flash-steamed sheet and a preparation method thereof. The raw materials of the flash-steamed sheet include polyethylene and air-permeable particles, and the mass fraction of the air-permeable particles in the flash-steamed sheet is 10%.

[0102] Highly breathable flash sheets are prepared by the following method:

[0103] Step 1: Mix dichloromethane, 1,1-dichloro-2,2,2-trifluoroethane, monochlorodichloromethane and 1H-perfluorohexane in a mass ratio of 6:2:1:1 to obtain a spinning solvent, and disperse polyethylene and air-permeable particles in the spinning solvent to obtain a spinning mixture;

[0104] The air permeable particles are prepared by cutting and crushing CNT-doped graphene aerogel with a diameter of 1.2 cm and then passing through a 300-mesh sieve;

[0105] Step 2: Transfer the spinning mixture obtained in step 1 to a high-pressure reactor, and then heat it to 170° C.; after the heating is completed, introduce nitrogen and pressurize it to 12.7 MPa; finally, heat it to 220° C. to obtain a flash spinning solution;

[0106] Step 3: flash-spinning the flash spinning solution through a spinning assembly to obtain flash-spun fibers, and the flash-spun fibers are laid on a web and then pre-pressed by at least two sets of pre-pressing rollers;

[0107] Step 4: After pre-pressing, the sheet is hot-rolled by at least three groups of hot-rolling rollers, and then calendered and wound to obtain a highly air-permeable flash-steamed sheet.

[0108] The air permeability of the flash-steamed sheet is tested according to the test standard described in ISO 5636-5 and according to the following formula:

[0109] Unit air permeability = (air permeability * thickness) / gram weight;

[0110] The specific air permeability of the flash-evaporated sheet was calculated.

[0111] Application Example 1

[0112] A flash sheet 1 was prepared using the components described in Example 3;

[0113] A flash sheet 2 was prepared using the components described in Comparative Example 1;

[0114] A flash sheet 3 was prepared using the components described in Comparative Example 2;

[0115] A flash sheet 4 was prepared using the components described in Comparative Example 3;

[0116] A flash sheet 5 was prepared using the components described in Comparative Example 4;

[0117] The flash-steamed sheets 1-5 were cut into test samples of the same size and thickness. After measurement, the sample thickness was 0.185 mm and the sample weight was 72 g / m 2 .

[0118] The tensile strength, elongation and air permeability of the cut flash-steamed sheets 1-5 were measured respectively, and the unit air permeability was calculated.

[0119] Among them, the test standard for tensile strength and elongation is ASTM D5035;

[0120] The test standard for air permeability is ISO 5636-5;

[0121] The results are shown in the following table:

[0122]

[0123] Result analysis: By comparing flash-steamed sheets 1-5, it can be seen that the unit air permeability of flash-steamed sheet 1 is significantly improved, while other performance aspects, such as tensile strength and tensile elongation, are not significantly affected, thus achieving the intended purpose of the present invention.

[0124] The specific embodiments described herein are merely examples of the spirit of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in similar ways, but they will not deviate from the spirit of the present invention or exceed the scope defined by the appended claims.

Claims

1. A method for preparing a highly breathable flash sheet, comprising polyethylene, characterized in that: The following steps are involved: Step 1: dispersing polyethylene and air-permeable particles into a spinning solvent to obtain a spinning mixture; the air-permeable particles are obtained by cutting and crushing a 1.2 cm diameter doped CNT graphene aerogel and passing it through a 300 mesh sieve; Step 2: Transfer the spinning mixture obtained in step 1 to a high-pressure reactor, and then heat it to 160-180° C.; after the heating is completed, introduce nitrogen and pressurize it to 12.5-13 MPa; finally heat it to 200-230° C. to obtain a flash spinning solution; Step 3: flash-spinning the flash spinning solution through a spinning assembly to obtain flash-spun fibers, and the flash-spun fibers are laid on a web and then pre-pressed by at least two sets of pre-pressing rollers; Step 4: After pre-pressing, the sheet is hot-rolled by at least three sets of hot-rolling rollers, and then calendered and wound to obtain a highly air-permeable flash-steamed sheet; The unit air permeability of the flash sheet is 12 to 31 (s•mm 3 ) / mg; Unit air permeability = (air permeability * thickness) / gram weight; The test standard for air permeability is ISO 5636-5.

2. The method for preparing a highly air-permeable flash-evaporated sheet according to claim 1, characterized in that: The unit air permeability of the flash sheet is 12-15 (s•mm 3 ) / mg.

3. The method for preparing a highly air-permeable flash-evaporated sheet according to claim 1, characterized in that: The unit air permeability of the flash sheet is 15-17 (s•mm 3 ) / mg.

4. The method for preparing a highly air-permeable flash-evaporated sheet according to claim 1, characterized in that: The unit air permeability of the flash sheet is 17-19 (s•mm 3 ) / mg.

5. The method for preparing a highly air-permeable flash-evaporated sheet according to claim 1, characterized in that: The unit air permeability of the flash sheet is 19-21 (s•mm 3 ) / mg.

6. The method for preparing a highly air-permeable flash-evaporated sheet according to claim 1, characterized in that: The unit air permeability of the flash sheet is 21-23 (s•mm 3 ) / mg.

7. The method for preparing a highly air-permeable flash-evaporated sheet according to claim 1, characterized in that: The unit air permeability of the flash sheet is 23-25 ​​(s•mm 3 ) / mg.

8. The method for preparing a highly air-permeable flash-evaporated sheet according to claim 1, characterized in that: The unit air permeability of the flash sheet is 25-27 (s•mm 3 ) / mg.

9. The method for preparing a highly air-permeable flash-evaporated sheet according to claim 1, characterized in that: The unit air permeability of the flash sheet is 27-29 (s•mm 3 ) / mg.

10. The method for preparing a highly air-permeable flash-evaporated sheet according to claim 1, characterized in that: The unit air permeability of the flash sheet is 29-31 (s•mm 3 ) / mg.

11. The method for preparing a highly air-permeable flash-evaporated sheet according to claim 1, characterized in that: The raw materials of the flash-steamed sheet include polyethylene and air-permeable particles, and the mass fraction of the air-permeable particles in the flash-steamed sheet is 5-8%.

Citation Information

Patent Citations

  • Breathable flash evaporation composite sheet and manufacturing method thereof

    CN116988228A

  • Fibrillated strand

    US3081519A

  • Nonwoven fiberous sheet of continuous strand material and the method of making same

    US3169899A

  • Apparatus for making non-woven fibrous sheet

    US3860369A

  • CNT-infused carbon fiber materials and process therefor

    CN102640573A