A lithium supplement and its preparation method and application
By uniformly dispersing modified lithium oxalate in the lamellar structure of modified graphene, the problem of high decomposition potential and low efficiency of lithium oxalate in lithium-ion batteries is solved, achieving more efficient lithium-ion battery performance and reducing decomposition voltage and improves decomposition efficiency.
Patent Information
- Application Number
- CN202410124036.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-29
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-01-29
AI Technical Summary
As a lithium replenishing agent, lithium oxalate has high decomposition potential and low decomposition efficiency, which results in its high decomposition voltage and low decomposition efficiency in lithium-ion batteries, limiting its application in lithium-ion batteries.
By combining modified lithium oxalate with modified graphene, the modified lithium oxalate is recrystallized and evenly dispersed in the randomly stacked lamellar structure of modified graphene to form a lithium replenishing agent, and the modified graphene provides abundant holes. and specific surface area, shortening the ion transmission path and reaction zone, and improving the decomposition kinetics of lithium oxalate.
It reduces the decomposition voltage of lithium oxalate, improves its decomposition efficiency, makes its decomposition potential closer to the matching point of commercial positive electrode and electrolyte, and improves the energy density and cycle life of lithium-ion batteries.
Smart Images

Figure CN117913260B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of lithium battery technology, and in particular to a lithium supplement and a preparation method and application thereof. Background Art
[0002] During the formation process of lithium-ion batteries, SEI growth on the negative electrode surface consumes active lithium, resulting in battery energy loss. The irreversible capacity loss of the most widely used graphite negative electrode is greater than 6%, while the irreversible capacity of the silicon-based negative electrode is more than 10% to 20%, which limits the high gram capacity advantage of the silicon-based system. Pre-lithiation technology can be regarded as providing an additional lithium source with specific materials or reagents. In order to increase the internal lithium content of the entire lithium-ion battery, a variety of pre-lithiation methods have been developed, which can be mainly divided into positive electrode pre-lithiation technology and negative electrode pre-lithiation technology.
[0003] Negative electrode pre-lithiation technology is the most common and relatively simple pre-lithiation strategy, including lithium foil pre-lithiation, lithium metal powder pre-lithiation, chemical pre-lithiation and electrochemical pre-lithiation. Negative electrode pre-lithiation technology faces the key challenge of the inherent high reactivity of lithium metal, which reacts with solvents and adhesives. In addition, lithium metal has low safety during the processing of lithium-ion batteries, which greatly hinders its large-scale application. On the contrary, positive electrode pre-lithiation materials exhibit excellent chemical stability and high open circuit voltage, which provides another direction for pre-lithiation. Positive electrode pre-lithiation technology can be better combined with the existing production process of lithium-ion batteries, and has the advantages of low safety risks, low equipment transformation investment, and scalability. The positive electrode lithium supplementation technology can compensate for the active lithium, which can improve the shortcomings of the low first efficiency of silicon-based negative electrodes and give full play to their high capacity advantages.
[0004] Lithium oxalate (Li 2 C 2 O 4 ) consists of an oxalate anion bonded to two lithium ions and has a high theoretical charge capacity (525 mAh g -1 ), excellent air stability, low discharge capacity (<10%), poor cycle performance, high thermodynamic stability (decomposed above 400°C), and no residue (gas released after decomposition). However, the insulating and slow lithium ion diffusion kinetics always lead to high decomposition potential (>4.8V) and low decomposition efficiency (<20%). Therefore, the existing technology needs to be improved. Summary of the invention
[0005] In view of the above-mentioned deficiencies in the prior art, the purpose of the present application is to provide a lithium supplement and a preparation method and application thereof, aiming to solve the problem of high decomposition potential and low separation efficiency of lithium oxalate as a lithium supplement in the prior art.
[0006] The technical solution of this application is as follows:
[0007] In a first aspect of the present application, a lithium supplement is provided, comprising modified lithium oxalate and modified graphene; wherein the modified lithium oxalate is obtained by recrystallization treatment, the modified graphene comprises a randomly stacked lamella structure, and the modified lithium oxalate is uniformly dispersed in the lamella structure of the modified graphene.
[0008] Optionally, the mass ratio of the modified lithium oxalate to the modified graphene is 1-10:0.01-10.
[0009] The second aspect of the present application provides a method for preparing the lithium supplement provided by the present application, comprising the steps of: providing lithium oxalate and the modified graphene; mixing the modified graphene and the lithium oxalate, and heating to obtain the lithium supplement, wherein the lithium oxalate is recrystallized after heating to form the modified lithium oxalate.
[0010] Optionally, the step of mixing the modified graphene and the lithium oxalate includes: providing water and anhydrous ethanol; dissolving the lithium oxalate in water to obtain an aqueous lithium oxalate solution, dispersing the modified graphene in the aqueous lithium oxalate solution to obtain a mixed solution; and dropping the mixed solution into anhydrous ethanol.
[0011] Optionally, the mass ratio of the lithium oxalate, the modified graphene, the water and the anhydrous ethanol is: 1-10:0.01-10:20:80.
[0012] Optionally, the method for preparing the modified graphene includes the steps of: providing a metal salt solution and graphene oxide; mixing the graphene oxide and the metal salt solution, heating, cooling, drying, and then performing a thermal reduction treatment to obtain the modified graphene.
[0013] Optionally, the metal element in the metal salt solution includes at least one of iridium, palladium, platinum, gold, silver, cobalt, iron, nickel, copper, manganese and molybdenum.
[0014] Optionally, the thermal reduction treatment is performed in a mixed atmosphere of argon and ammonia.
[0015] In a third aspect of the present application, a composite positive electrode is provided, comprising a conductive agent, a binder and a lithium supplement agent provided in the present application.
[0016] In a fourth aspect of the present application, a lithium-ion battery is provided, comprising the composite positive electrode, electrolyte, separator and negative electrode provided in the present application.
[0017] Beneficial effects of this application:
[0018] The lithium supplement provided by the present application includes modified lithium oxalate and modified graphene, wherein the modified lithium oxalate is recrystallized to reduce its size, thereby providing sufficient reaction points and shortening the ion transmission path. The modified graphene includes a randomly stacked sheet structure with abundant pores, which gives the modified graphene a higher specific surface area, provides a path for the rapid transmission of lithium ions and electrons, and provides sufficient three-phase reaction areas, so that the modified lithium oxalate is evenly dispersed in the sheet structure of the modified graphene, providing a large amount of space for the decomposition and diffusion of the modified lithium oxalate, improving its decomposition kinetics, reducing its decomposition voltage, and improving its decomposition efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the following briefly introduces the drawings required for describing the embodiments.
[0020] Figure 1 A graph showing the relationship between the specific capacity and voltage of lithium oxalate provided in an embodiment of the present application;
[0021] Figure 2 This is a scanning electron microscope image of the lithium supplement provided in the embodiment of the present application;
[0022] Figure 3 A graph showing the relationship between specific capacity and voltage of the lithium supplement provided in the embodiments of the present application;
[0023] Figure 4 A graph showing the relationship between specific capacity and voltage of a composite positive electrode containing a lithium supplement provided in an embodiment of the present application;
[0024] Figure 5 This is an impedance test diagram of a composite positive electrode containing a lithium supplement provided in an embodiment of the present application;
[0025] Figure 6 A graph showing the relationship between specific capacity and voltage of a full battery containing a lithium supplement provided in an embodiment of the present application;
[0026] Figure 7 This is a test chart of the specific capacity and coulombic efficiency of a full battery containing a lithium supplement provided in an embodiment of the present application. DETAILED DESCRIPTION
[0027] In order to make the purpose, technical solutions and advantages of the present application clearer, the technical solutions in the embodiments of the present application will be clearly and completely described below in combination with the drawings and embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments of the present application, all other embodiments obtained by ordinary technicians in this field without making creative work belong to the protection scope of the present application. In the absence of conflict, the following embodiments and features in the embodiments can be combined with each other.
[0028] It should be noted that if there are descriptions involving "first", "second", etc. in the implementation of this application, the descriptions of "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or suggesting their relative importance and implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the fact that ordinary technicians in the field can implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by this application.
[0029] Lithium oxalate consists of an oxalate anion bonded to two lithium ions and has a high theoretical charge capacity (525 mAh g -1 ), excellent air stability, low discharge capacity (<10%), poor cycle performance, high thermodynamic stability (decomposed above 400°C), and no residue (released gas after decomposition). However, the insulating and slow lithium ion diffusion kinetics always lead to its high decomposition potential (>4.8V) and low decomposition efficiency (<20%), such as Figure 1 As shown. That is, the decomposition voltage of the original lithium oxalate is above 4.8V, and the decomposition efficiency is low (less than 20%), which is incompatible with the current battery system. At present, the voltage of commercial cathode materials and the decomposition voltage of electrolyte are below 4.5V, so lowering the decomposition voltage of lithium oxalate is the key. In the prior art, by introducing certain oxide dopants (such as NiO (10wt%), Mo 2 C (30 wt%)) to solve the problem of Li 2 C 2 O 4 However, relatively high dopant dosages can reduce energy density and cycle life.
[0030] Based on this, in a first aspect of an embodiment of the present application, a lithium supplement is provided, comprising modified lithium oxalate and modified graphene; wherein the modified lithium oxalate has been subjected to recrystallization treatment, the modified graphene comprises a randomly stacked lamella structure, and the modified lithium oxalate is uniformly dispersed in the graphene lamella structure.
[0031] The modified lithium oxalate is recrystallized to effectively reduce the size of lithium oxalate, thereby providing sufficient reaction sites and shortening the ion transmission path. The modified graphene includes a randomly stacked sheet structure with abundant pores, which gives the modified graphene a higher specific surface area, providing a path for the rapid transmission of lithium ions and electrons, and providing sufficient three-phase reaction areas, so that lithium oxalate is evenly dispersed in the sheet structure of graphene, providing a large amount of space for the decomposition and diffusion of lithium oxalate, improving the decomposition kinetics of lithium oxalate, reducing its decomposition voltage, and improving its decomposition efficiency.
[0032] In one embodiment, the mass ratio of modified lithium oxalate to modified graphene is 1-10:0.01-10. Preferably, the mass ratio of modified lithium oxalate to modified graphene is 1:0.01-3.
[0033] The second aspect of the embodiment of the present application provides a method for preparing the lithium supplement in the embodiment of the present application:
[0034] Providing lithium oxalate and the modified graphene; mixing the modified graphene and the lithium oxalate, and heating to obtain a lithium supplement.
[0035] In one embodiment, the heating temperature is 80-100° C., for example, the heating temperature is 80° C., 85° C., 90° C., 95° C. or 100° C. The heating time is 12-24 h, for example, the heating time is 12 h, 14 h, 16 h, 18 h, 20 h, 22 h or 24 h.
[0036] The lithium supplement is obtained by mixing lithium oxalate and modified graphene and heating and evaporating them. During the heating and evaporation process, the lithium oxalate recrystallizes and reduces its size, thereby providing sufficient reaction sites and shortening the ion transmission path.
[0037] In one embodiment, the step of mixing modified graphene and lithium oxalate comprises:
[0038] Water and anhydrous ethanol are provided; lithium oxalate is dissolved in water to obtain a lithium oxalate solution, modified graphene is dispersed in the lithium oxalate solution to obtain a mixed solution; and the mixed solution is dropped into the anhydrous ethanol.
[0039] In one embodiment, the mass ratio of lithium oxalate, modified graphene, water and anhydrous ethanol is 1-10:0.01-10:20:80.
[0040] In one embodiment, the method for preparing modified graphene comprises:
[0041] Providing a metal salt solution and graphene oxide; mixing the graphene oxide and the metal salt solution, heating, cooling, drying, and then performing a thermal reduction treatment.
[0042] The graphene oxide and metal salt solution are mixed by magnetic stirring and ultrasonic dispersion, and then transferred to a hydrothermal reactor for heating.
[0043] In one embodiment, the mass ratio of graphene oxide to the metal salt solution is 1:50 to 300. For example, the mass ratio of graphene oxide to the metal salt solution is 1:50, 1:100, 1:150, 1:200, 1:250 or 1:300.
[0044] In one embodiment, the metal element in the metal salt solution includes at least one of iridium, palladium, platinum, gold, silver, cobalt, iron, nickel, copper, manganese, and molybdenum. The metal salt solution may be a metal chloride solution.
[0045] In one embodiment, the time of magnetic stirring and ultrasonic dispersion is 2 to 10 hours. For example, the time of magnetic stirring and ultrasonic dispersion is 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours or 10 hours.
[0046] In one embodiment, the heating temperature in the hydrothermal reactor is 150-250° C., for example, the heating temperature is 150° C., 170° C., 190° C., 210° C., 230° C. or 250° C., etc. The heating time is 3-13 h, for example, the heating time is 3 h, 4 h, 5 h, 6 h, 7 h, 8 h, 9 h, 10 h, 11 h or 12 h, etc.
[0047] In one embodiment, drying is performed by cool drying.
[0048] In one embodiment, the specific step of thermal reduction includes transferring the dried sample to a tube furnace for high-temperature thermal reduction. The temperature of thermal reduction is 700-1000°C, for example, the temperature of thermal reduction is 700°C, 800°C, 900°C or 1000°C. The time of thermal reduction is 0.5-6h. For example, the time of thermal reduction is 0.5h, 1h, 2h, 4h, 5h or 6h.
[0049] In one embodiment, during the thermal reduction process, the tubular furnace introduces argon and ammonia into the reaction chamber at a rate of 50-200 ml / min, wherein the flow rate of argon is 150 sccm and the flow rate of ammonia is 50 sccm.
[0050] The decomposition products of ammonia will introduce nitrogen doping, which will greatly improve the structure and conductivity of graphene. At the same time, the uneven distribution of atomic charge density during the doping process is conducive to promoting the adsorption of lithium oxalate and material activity. The defects and disorder produced provide active sites for the adsorption of lithium oxalate and increase the density of reaction active sites, thereby improving the reaction activity of lithium oxalate and reducing its decomposition voltage.
[0051] According to a third aspect of the embodiments of the present application, a composite positive electrode is provided, comprising a conductive agent, a binder and the lithium supplement agent in the embodiments of the present application.
[0052] In one embodiment, the method for preparing the composite positive electrode comprises the steps of:
[0053] The lithium supplement agent, the conductive agent and the binder in the embodiment of the present application are taken in a ratio of 10:1:1, and are uniformly dispersed in an N-methylpyrrolidone (NMP) solvent to obtain a slurry;
[0054] The slurry was uniformly coated on aluminum foil and dried in vacuum at 110 °C for 12 h to obtain a composite positive electrode.
[0055] The conductive agent includes at least one of conductive carbon black, conductive graphite, vapor-grown carbon fiber, carbon nanotubes, and graphene. The binder includes at least one of polyvinylidene fluoride, polytetrafluoroethylene, sodium carboxymethyl cellulose, methyl cellulose, ethyl cellulose, polyacrylic acid, sodium alginate, chitosan, and PETDO:PSS. Preferably, the binder uses polyvinylidene fluoride (PVDF).
[0056] According to a fourth aspect of the embodiments of the present application, a lithium-ion battery is provided, comprising the composite positive electrode, electrolyte, separator and negative electrode in the embodiments of the present application.
[0057] The following is further described by means of specific examples.
[0058] Example 1
[0059] (1) The graphene oxide aqueous solution and the nickel chloride solution were mixed evenly in a mass ratio of 1:200, and after magnetic stirring and ultrasonic dispersion for 3 hours, they were transferred to a hydrothermal reactor for subsequent hydrothermal treatment. The hydrothermal temperature was controlled at 180°C and the time was controlled for 6 hours. After the reactor was cooled to room temperature, a precursor gel was obtained. After freeze-drying to remove moisture, the sample was transferred to a tubular furnace for high-temperature thermal reduction. The thermal reduction temperature was set at 900°C and the time was 1 hour. At the same time, the tubular furnace passed Ar (150 sccm) / NH3 (50 sccm) mixed gas into the reaction chamber at a rate of 100 ml / min. After the thermal reduction was completed, modified graphene was obtained.
[0060] (2) Dissolve 1g of lithium oxalate in deionized water to obtain a lithium oxalate aqueous solution, disperse 0.1g of modified graphene in the lithium oxalate aqueous solution, then dropwise add the solution into anhydrous ethanol, heat at 100°C for 24h to obtain a lithium supplement. The lithium supplement was observed using a SEM microscope. The results are as follows: Figure 2 As shown. Figure 2 It can be seen that the lithium supplement has a porous 3D layered structure with abundant pores. The randomly stacked layer structure of modified graphene gives the material a higher specific surface area, thus providing a fast path for the rapid transmission of lithium ions and electrons, providing sufficient three-phase reaction area, and promoting the uniform dispersion of lithium oxalate in the graphene layered structure, providing a large amount of space for the decomposition and diffusion of lithium oxalate.
[0061] Example 2
[0062] 100 mg of the lithium supplement in Example 1, 10 mg of conductive carbon black, and 10 mg of PVDF were uniformly dispersed in NMP solvent to obtain a slurry. The slurry was uniformly coated on aluminum foil and vacuum dried at 110°C for 12 hours to obtain a composite positive electrode. The composite positive electrode, negative electrode, electrolyte, and separator were prepared into a battery in an argon glove box. The battery was kept stationary for 36 hours. The battery was charged at a charging current density of 1 mA / g to 100 mA / g. The charging cut-off voltage was 4.5 V. The test results are as follows: Figure 3 As shown, Ni / N-rGO-Li 2 C 2 O 4 Represents the prepared battery. Figure 3 It can be seen that the decomposition voltage of lithium oxalate is mostly below 4.3V. When charged to 4.5V, the decomposition efficiency can reach 100%. The lithium supplement in the embodiment of the present application effectively reduces the decomposition overpotential of lithium oxalate, making the decomposition potential of lithium oxalate better matched with the commercial positive electrode and electrolyte.
[0063] Example 3
[0064] 8 mg of the lithium supplement in Example 1, 80 mg of NCM811 positive electrode material, 10 mg of conductive carbon black, and 10 mg of PVDF were uniformly dispersed in NMP solvent to obtain slurry. The slurry was uniformly coated on aluminum foil and vacuum dried at 110° C. for 12 h to obtain a composite positive electrode.
[0065] Take 80mg NCM811 positive electrode material, 10mg conductive carbon black, and 10mg PVDF, and evenly disperse them in NMP solvent to obtain slurry. The slurry is evenly coated on aluminum foil and vacuum dried at 110℃ for 12h to obtain a comparative composite positive electrode. The composite positive electrode and comparative composite positive electrode are prepared into batteries with the negative electrode, electrolyte and diaphragm in an argon glove box, respectively. The battery is kept stationary for 36 hours, and the battery is charged at a charging current density of 1mA / g to 100mA / g. The charging cut-off voltage is 4.5V. The test results are as follows: Figure 4 and Figure 5 As shown in the figure, NCM+Ni / N-rGO-Li 2 C 2 O 4 represents a battery made of a composite positive electrode, and NCM represents a battery made of a comparative composite positive electrode. Figure 4 and Figure 5 It can be seen that the first cycle is charged to 4.5V, and the first charge capacity is 270.3mAh g -1 , compared with 242.2mAh g of the composite cathode -1 Improved by 28.1mAh g -1The first charge specific capacity is increased by 11.7%, and the impedance of the entire battery is reduced, indicating that the lithium supplement agent in the embodiment of the present application effectively supplements lithium to the positive electrode.
[0066] Example 4
[0067] Take 8 mg of the lithium supplement in Example 1, 80 mg of NCM811 positive electrode material, 10 mg of conductive carbon black, and 10 mg of PVDF, and evenly disperse them in NMP solvent to obtain slurry. The slurry is evenly coated on aluminum foil and vacuum dried at 110°C for 12 hours to obtain a composite positive electrode. The composite positive electrode, silicon oxygen negative electrode, electrolyte, and separator form a full battery.
[0068] Take 80mg NCM811 positive electrode material, 10mg conductive carbon black, and 10mg PVDF, and evenly disperse them in NMP solvent to obtain slurry. The slurry is evenly coated on aluminum foil and vacuum dried at 110℃ for 12h to obtain a composite positive electrode. The composite positive electrode, silicon-oxygen negative electrode, electrolyte, and separator form a control group full battery.
[0069] The full battery containing the lithium supplement in the example of the present application and the full battery of the control group were tested for electrical performance at 4.5V. The results are as follows: Figure 6 and Figure 7 As shown in the figure, NCM+Ni / N-rGO-Li 2 C 2 O 4 represents a battery made of a composite positive electrode, and NCM represents a battery made of a comparative composite positive electrode. Figure 6 and Figure 7 It can be seen that the initial discharge capacity of the full battery is only 119.8 mAh g -1 In sharp contrast, the first discharge capacity of the full battery containing the lithium supplement in the embodiment of the present application is 156.3 mAh g -1 . It is 30.4% higher than the bare NCM / / SiOx battery. After 50 charge and discharge cycles, the full battery containing the lithium supplement in the embodiment of the present application has a capacity retention rate of about 68.2%, which is much higher than the full battery of the control group (about 46.7%).
[0070] In summary, the lithium supplement provided by the present application includes modified lithium oxalate and modified graphene, wherein the modified lithium oxalate is recrystallized and reduced in size, thereby providing sufficient reaction points and shortening the ion transmission path. The modified graphene includes a randomly stacked sheet structure with abundant pores, which gives the modified graphene a higher specific surface area, provides a path for the rapid transmission of lithium ions and electrons, and provides sufficient three-phase reaction areas, so that lithium oxalate is evenly dispersed in the sheet structure of graphene, providing a large amount of space for the decomposition and diffusion of lithium oxalate, improving the decomposition kinetics of lithium oxalate, reducing its decomposition voltage, and improving its decomposition efficiency.
[0071] It should be understood that the application of the present application is not limited to the above examples. For ordinary technicians in this field, improvements or changes can be made based on the above description. All these improvements and changes should fall within the scope of protection of the claims attached to this application.
Claims
1. A lithium supplement, characterized in that: The lithium supplement agent includes modified lithium oxalate and modified graphene; Wherein, the modified lithium oxalate is obtained by recrystallization treatment, the modified graphene includes a randomly stacked sheet structure, and the modified lithium oxalate is dispersed in the sheet structure of the modified graphene; The preparation method of the lithium supplement comprises: Providing a nickel chloride solution and graphene oxide, mixing the graphene oxide and the nickel chloride solution, heating, cooling, and drying, and then performing a thermal reduction treatment in a mixed atmosphere of argon and ammonia to obtain the modified graphene; wherein the heating is performed in a hydrothermal reactor, the heating temperature is 180° C., the heating time is 6 hours, the thermal reduction treatment temperature is 900° C., and the thermal reduction treatment time is 1 hour; Lithium oxalate is dissolved in water to obtain a lithium oxalate aqueous solution, the modified graphene is dispersed in the lithium oxalate aqueous solution to obtain a mixed solution, the mixed solution is dropped into anhydrous ethanol, and heated to obtain the lithium supplement agent.
2. The lithium supplement according to claim 1, characterized in that: The mass ratio of the modified lithium oxalate to the modified graphene is 1-10:0.01-10.
3. The lithium supplement according to claim 1, characterized in that: The mass ratio of the lithium oxalate, the modified graphene, the water and the anhydrous ethanol is 1-10:0.01-10:20:
80.
4. A composite positive electrode, characterized in that: The invention comprises a conductive agent, a binder and the lithium supplement agent according to any one of claims 1 to 3.
5. A lithium ion battery, characterized in that: The invention comprises the composite positive electrode as claimed in claim 4, an electrolyte, a separator and a negative electrode.