Preparation method and application of tin-modified cuprous oxide nanowire three-dimensional copper-based current collector
The preparation of three-dimensional copper-based current collectors with tin-modified cuprous oxide nanowires solves the problem of dendrite growth caused by uneven distribution of lithium ions in lithium metal batteries, achieving uniform deposition of lithium and long-term stability of the battery.
Patent Information
- Application Number
- CN202410082932.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-19
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-01-19
AI Technical Summary
During the deposition process of lithium metal batteries, the uneven distribution of lithium ions leads to uneven nucleation and dendrite growth of lithium nuclei, resulting in battery failure and capacity fading.
Tin-modified cuprous oxide nanowires are used as a three-dimensional copper-based current collector, copper hydroxide nanowires are grown by electrodeposition, oxidized to CuO@Cu by air heat treatment, and then in situ exchange reaction is performed in an ethanol solution of tin tetrachloride pentahydrate. , and finally the Sn@Cu2O@Cu anode material was prepared through plasma reduction, forming a three-dimensional copper-based current collector with a larger specific surface area and pore structure, and improving the uniformity of lithium deposition.
It achieves dense growth of lithium, reduces the current density, extends the cycle life and stability of the battery, and maintains high Coulombic efficiency and discharge specific capacity.
Smart Images

Figure CN117913284B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a preparation method and application of a copper-based current collector. Background Art
[0002] With the progress of society and industrial development, the rapid development of portable devices and electric vehicles has stimulated the urgent demand for "next-generation" rechargeable batteries. Lithium metal anodes (LMA) are a promising potential solution because they have a high capacity of 3860 mAhg -1 The ultra-high theoretical capacity and the lowest redox electrode potential (-3.04V compared to the standard hydrogen electrode) of LMA make this property an important material for the next generation of high-energy batteries and have attracted great interest from researchers. However, the development of lithium metal batteries is still faced with a series of challenges. First, the uneven deposition of lithium metal and the uncontrollable dendrite growth during the repeated deposition / stripping of lithium metal anodes can easily lead to battery failure, and there are serious safety hazards in organic electrolyte systems. Secondly, the ultra-high activity of lithium metal makes it easy for it to react irreversibly with electrolytes and cathode materials, resulting in rapid capacity decay of the battery. In addition, due to the host-free characteristics of the lithium metal anode, the infinite volume change of the anode and the uneven deposition / stripping of lithium ions during battery operation, this can easily lead to the rupture and regeneration of the solid electrolyte interface layer (SEI), as well as the growth of dendrites. These problems will lead to the continuous loss of lithium and electrolyte, and the formation of "dead lithium", resulting in low CE and battery failure. To solve the above problems of LMAs, researchers have proposed various strategies, including the use of solid electrolytes, electrolyte additives, artificial SEI, and the construction of three-dimensional hosts. These strategies have made some progress in suppressing dendrites, but still cannot meet the requirements of practical applications of LMAs. It is worth noting that the three-dimensional host strategy is considered to be an effective method to simultaneously alleviate volume changes and inhibit dendrite growth, and has great potential in overcoming long-term challenges associated with lithium metal (such as dendrite growth and capacity loss).
[0003] However, during the lithium deposition process, due to the uneven distribution of lithium ions on the electrode surface, the lithium ions also show uneven nucleation when accepting electrons and being reduced. In the subsequent lithium deposition, lithium ions tend to gather on the surface of the uneven lithium nucleus and preferentially deposit on the lithium nucleus to form a larger lithium nucleus. It is very easy to induce lithium nucleation and growth at the tip, thus forming uncontrollable lithium dendrites. Summary of the invention
[0004] The purpose of the present invention is to solve the problem that in the prior art, during the lithium deposition process, due to the uneven distribution of lithium ions on the electrode surface, the lithium ions also show uneven nucleation when accepting electrons and being reduced. In the subsequent lithium deposition, the lithium ions tend to gather on the surface of the uneven lithium nucleus and preferentially deposit on the lithium nucleus to form a larger lithium nucleus, which easily induces lithium nucleation and growth at the tip, thereby forming uncontrollable lithium dendrites. A preparation method and application of a tin-modified cuprous oxide nanowire three-dimensional copper-based current collector are provided.
[0005] The tin-modified cuprous oxide nanowire three-dimensional copper-based current collector prepared by the present invention is firstly grown copper hydroxide nanowires as a precursor on the surface of copper foam by electrodeposition, oxidized to CuO@Cu by air heat treatment, and the obtained CuO@Cu is immersed in an ethanol solution of tin tetrachloride pentahydrate for in-situ replacement reaction, and then reduced by plasma to obtain a three-dimensional Sn@Cu 2 O@Cu anode material. The specific scheme is as follows:
[0006] A method for preparing a tin-modified cuprous oxide nanowire three-dimensional copper-based current collector is specifically completed by the following steps:
[0007] 1. Preparation of CuO@Cu:
[0008] The copper foam was used as the working electrode, the platinum sheet was used as the counter electrode, and the sodium hydroxide solution was used as the electrolyte. -2 ~20mAcm -2 Electrodepositing for a period of time at a current density of 1000 nm to generate copper hydroxide nanowires to obtain a reaction product I; washing the reaction product I, vacuum drying it, and then placing it in a muffle furnace for heat treatment for a period of time, and taking it out after the temperature drops to room temperature to obtain a copper oxide nanowire / foam copper composite material;
[0009] 2. Preparation of Sn@Cu 2 O@Cu:
[0010] ① Immerse the copper oxide nanowire / foam copper composite material in a mixed solution of NaCl and anhydrous ethanol, and then add SnCl 4 ·5H 2 O ethanol solution, continue to stir and react for a period of time after the addition is completed, then let it stand, then wash and vacuum dry to obtain reaction product II;
[0011] ②. Place the reaction product II in a plasma reaction chamber, raise the temperature to 200°C to 300°C, introduce hydrogen into the plasma reaction chamber, maintain the pressure of the reaction chamber at 10Pa to 20Pa during the glow discharge process, and the power of the radio frequency plasma is 250W to 300W. Continue to treat the reaction product II for 120 seconds to 240 seconds, take it out after the temperature drops to room temperature, and obtain a tin-modified cuprous oxide nanowire three-dimensional copper-based current collector.
[0012] A tin-modified cuprous oxide nanowire three-dimensional copper-based current collector is used as an anode for lithium metal batteries.
[0013] Principle of the present invention:
[0014] The tin-modified cuprous oxide nanowire three-dimensional copper-based current collector prepared by the present invention has a larger specific surface area and pore structure, which can reduce local current density and alleviate volume expansion; in addition, the interface modification of the current collector can give it better lithium affinity, making the deposition of lithium more uniform; this strategy of changing the lithium deposition mode in the nucleation stage is conducive to the dense growth of lithium and the formation of a dendrite-free lithium metal negative electrode; the invention grows Sn@Cu on the surface of foam copper by electrochemical deposition, high-temperature oxidation in air, in-situ replacement and plasma reduction 2 O nanowires; by introducing lithiophilic Sn metal to induce uniform deposition of lithium, combined with a three-dimensional substrate with rich internal space, the current density is reduced, thereby maximizing the use of the internal structure of the three-dimensional host to adapt to the volume change of lithium during the cycle and stabilize the interface; in this invention, a strategy of modifying a three-dimensional foam copper skeleton by electrodeposition and applying it to the lithium metal anode host is studied. During the initial discharge process, Sn@Cu 2 The Sn layer on O@Cu is transformed into LiSn alloy, which provides a large number of active sites for lithium deposition and reduces the nucleation barrier.
[0015] Advantages of the present invention:
[0016] 1. The Sn@Cu@Cu@Sn@Cu@Sn@Cu@Cu@Sn@Cu@ 2 The electrochemical performance of O@Cu was tested and the results showed that at 1 mA cm -2 The current density is 1 mAh cm -2 Under the surface capacity, using Sn@Cu 2 The average coulombic efficiency of the half-cell assembled by O@Cu was as high as 98.47% in 400 cycles, and the assembled symmetric battery could stably cycle for more than 1400h, indicating that the three-dimensional anode material for lithium metal batteries provided by the present invention has excellent lithium deposition / stripping stability; when combined with lithium iron phosphate (LiFePO 4 ) During cathode assembly, Sn@Cu 2 O@Cu electrode has an initial capacity of 96 mAhg at 5C-1 After 1000 cycles, it shows 93 mAh g -1 The high discharge specific capacity and 96.87% capacity retention rate indicate that the lithium metal battery anode material provided by the present invention has a high cycle life;
[0017] 2. The present invention has novel design ideas and simple experimental operations, and can enable lithium to densely nucleate in a three-dimensional body and stably deposit in a porous structure, thereby achieving a higher pore utilization rate. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 The surface and scanning electron microscope images of the samples, a is the surface of the copper foam, b and c are scanning electron microscope images of the copper foam, and d is the Sn@Cu prepared in Example 1. 2 The surface of O@Cu, e and f are Sn@Cu prepared in Example 1 2 SEM image of O@Cu;
[0019] Figure 2 Sn@Cu prepared in Example 1 2 SEM Mapping of O@Cu, where a is Sn@Cu prepared in Example 1 2 Scanning electron microscope images of O@Cu, b is Cu, c is Sn, d is O;
[0020] Figure 3 Sn@Cu prepared in Example 1 2 X-ray photoelectron spectroscopy images of O@Cu, a is Sn, b is Cu;
[0021] Figure 4 Sn@Cu prepared in Example 1 2 Transmission electron microscopy (TEM) and high-resolution transmission electron microscopy (HRTEM) images of O@Cu. Figure a is a transmission electron microscopy image, and figure b is a high-resolution transmission electron microscopy image.
[0022] Figure 5 The scanning electron microscope images of the samples after lithium deposition, a and b in the figure are scanning electron microscope images of CuO@Cu prepared in step 1 of Example 1 after lithium deposition, c and d are scanning electron microscope images of Sn@Cu prepared in Example 1 2 SEM image of O@Cu after lithium deposition;
[0023] Figure 6 The Sn@Cu prepared in Example 1 2 The O@Cu assembled half-cell has a current density of 1 mAh cm -2 、Li-plating capacity is 1 mAhcm -2 Coulomb efficiency under
[0024] Figure 7 The Sn@Cu prepared in Example 12 Symmetrical cells assembled from O@Cu at 1 mA cm -2 The current density is 1 mAh cm -2 Cyclic stability diagram under area capacity;
[0025] Figure 8 The Sn@Cu prepared in Example 1 2 O@Cu and LiFePO 4 (LFP) Sn@Cu paired assembly 2 Coulombic efficiency and discharge capacity of O@Cu@Li||LFP full cell at 5C. DETAILED DESCRIPTION
[0026] Specific implementation method 1: This implementation method is a method for preparing a tin-modified cuprous oxide nanowire three-dimensional copper-based current collector, which is specifically completed according to the following steps:
[0027] 1. Preparation of CuO@Cu:
[0028] The copper foam was used as the working electrode, the platinum sheet was used as the counter electrode, and the sodium hydroxide solution was used as the electrolyte. -2 ~20mAcm --2 Electrodepositing for a period of time at a current density of 1000 nm to generate copper hydroxide nanowires to obtain a reaction product I; washing the reaction product I, vacuum drying it, and then placing it in a muffle furnace for heat treatment for a period of time, and taking it out after the temperature drops to room temperature to obtain a copper oxide nanowire / foam copper composite material;
[0029] 2. Preparation of Sn@Cu 2 O@Cu:
[0030] ① Immerse the copper oxide nanowire / foam copper composite material in a mixed solution of NaCl and anhydrous ethanol, and then add SnCl 4 ·5H 2 O ethanol solution, continue to stir and react for a period of time after the addition is completed, then let it stand, then wash and vacuum dry to obtain reaction product II;
[0031] ②. Place the reaction product II in a plasma reaction chamber, raise the temperature to 200°C to 300°C, introduce hydrogen into the plasma reaction chamber, maintain the pressure of the reaction chamber at 10Pa to 20Pa during the glow discharge process, and the power of the radio frequency plasma is 250W to 300W. Continue to treat the reaction product II for 120 seconds to 240 seconds, take it out after the temperature drops to room temperature, and obtain a tin-modified cuprous oxide nanowire three-dimensional copper-based current collector.
[0032] Specific implementation method 2: This implementation method is different from specific implementation method 1 in that the concentration of the sodium hydroxide solution in step 1 is 1 mol / L to 2 mol / L. The other steps are the same as those in specific implementation method 1.
[0033] Specific embodiment 3: This embodiment differs from specific embodiment 1 or 2 in that the electrodeposition time in step 1 is 5 minutes to 20 minutes. The other steps are the same as those in specific embodiment 1 or 2.
[0034] Specific embodiment 4: This embodiment differs from specific embodiments 1 to 3 in that: in step 1, the reaction product I is washed 3 to 5 times with deionized water and anhydrous ethanol respectively; the vacuum drying temperature in step 1 is 60°C to 100°C, and the vacuum drying time is 12h to 24h. The other steps are the same as those of specific embodiments 1 to 3.
[0035] Specific embodiment 5: This embodiment differs from specific embodiments 1 to 4 in that the temperature of the heat treatment in step 1 is 250° C. to 300° C. and the time of the heat treatment is 2 h to 5 h. The other steps are the same as those of specific embodiments 1 to 4.
[0036] Specific embodiment 6: This embodiment differs from specific embodiments 1 to 5 in that the mixed solution of NaCl and anhydrous ethanol described in step 2① is prepared by mixing a NaCl solution with a concentration of 100 g / L to 200 g / L and anhydrous ethanol, wherein the volume ratio of the NaCl solution to the anhydrous ethanol is 0.2:20. The other steps are the same as those of specific embodiments 1 to 5.
[0037] Specific embodiment 7: This embodiment differs from specific embodiments 1 to 6 in that: the SnCl 4 ·5H 2 The concentration of the ethanol solution is 0.7 g / L to 1 g / L; the SnCl 4 ·5H 2 The volume ratio of the 0 ethanol solution to the mixed solution of NaCl and anhydrous ethanol is 10:(20-25). The other steps are the same as those in the first to sixth embodiments.
[0038] Specific embodiment eight: This embodiment differs from specific embodiments one to seven in that: the stirring reaction time after the dropwise addition in step two ① is 1h to 2h; the standing time in step two ① is 1h to 2h; the cleaning is to use deionized water and anhydrous ethanol to clean 3 to 5 times respectively; the vacuum drying temperature is 40℃ to 65℃, and the vacuum drying time is 5h to 20h. The other steps are the same as those in specific embodiments one to seven.
[0039] Specific embodiment 9: This embodiment differs from specific embodiments 1 to 8 in that the flow rate of hydrogen introduced into the plasma reaction chamber in step 2② is 15 sccm to 20 sccm. The other steps are the same as those of specific embodiments 1 to 8.
[0040] Specific embodiment 10: This embodiment is a tin-modified cuprous oxide nanowire three-dimensional copper-based current collector used as a lithium metal battery anode.
[0041] The following examples are used to verify the beneficial effects of the present invention:
[0042] Example 1: A method for preparing a tin-modified cuprous oxide nanowire three-dimensional copper-based current collector is specifically completed by the following steps:
[0043] 1. Preparation of CuO@Cu:
[0044] The copper foam was used as the working electrode, the platinum sheet was used as the counter electrode, and the sodium hydroxide solution with a concentration of 1 mol / L was used as the electrolyte. -2 The reaction product I was washed three times with deionized water and anhydrous ethanol, dried under vacuum at 60°C for 12h, and then heat treated in a muffle furnace at 250°C for 2h. After the temperature dropped to room temperature, the reaction product I was taken out to obtain a copper oxide nanowire / foam copper composite material (CuO@Cu).
[0045] 2. Preparation of Sn@Cu 2 O@Cu:
[0046] ① Immerse the copper oxide nanowire / foam copper composite material in a mixed solution of NaCl and anhydrous ethanol, and then add SnCl 4 ·5H 2 O ethanol solution, continue to stir the reaction for 1 hour after the addition is completed, then let it stand for 1 hour, then use deionized water and anhydrous ethanol to wash three times respectively, and vacuum dry at 65°C for 20 hours to obtain reaction product II;
[0047] The mixed solution of NaCl and anhydrous ethanol described in step 2① is prepared by mixing a NaCl solution having a concentration of 100 g / L and anhydrous ethanol, wherein the volume ratio of the NaCl solution to the anhydrous ethanol is 0.2:20;
[0048] SnCl described in step 2① 4 ·5H 2 The concentration of O ethanol solution is 0.7 g / L;
[0049] SnCl described in step 2① 4 ·5H 2The volume ratio of O ethanol solution to the mixed solution of NaCl and anhydrous ethanol is 10:20.3;
[0050] ②, the reaction product II was placed in a plasma reaction chamber, the temperature was raised to 200 ° C, and a reduction reaction was carried out by plasma treatment. 15 sccm of hydrogen was introduced into the plasma reaction chamber. The pressure of the reaction chamber was maintained at 10Pa during the glow discharge process. The power of the radio frequency plasma was 250W. The reaction product II was continuously treated for 120 seconds. After the temperature dropped to room temperature, it was taken out to obtain a tin-modified cuprous oxide nanowire three-dimensional copper-based current collector (Sn@Cu 2 O@Cu).
[0051] Figure 1 The surface and scanning electron microscope images of the samples, a is the surface of the copper foam, b and c are scanning electron microscope images of the copper foam, and d is the Sn@Cu prepared in Example 1. 2 The surface of O@Cu, e and f are Sn@Cu prepared in Example 1 2 SEM image of O@Cu;
[0052] from Figure 1 From a, we can see that the sample copper foam is golden yellow, and from b and c, we can see that the surface of the copper foam is smooth. Figure 1 It can be seen from Figure d that the surface treated by plasma reduction appears red and black; Figure 1 As can be seen from e and f: Sn@Cu prepared in Example 1 2 Uniform and dense Sn@Cu is grown on the surface of O@Cu 2 O nanowires.
[0053] Figure 2 Sn@Cu prepared in Example 1 2 SEM Mapping of O@Cu, where a is Sn@Cu prepared in Example 1 2 Scanning electron microscope images of O@Cu, b is Cu, c is Sn, d is O;
[0054] from Figure 2 It can be seen that Cu and O elements are evenly distributed in Sn@Cu 2 On the O@Cu nanowires, the Sn element is evenly distributed after plasma reduction, which proves that the Sn element is successfully introduced into the current collector.
[0055] Figure 3 Sn@Cu prepared in Example 1 2 X-ray photoelectron spectroscopy images of O@Cu, a is Sn, b is Cu;
[0056] from Figure 3From a, we can see that the peaks of Sn 3d at 494.5eV and 486.1eV belong to the single substance Sn metal; Figure 3 From b, we can see that the Cu 2p spectrum shows two main peaks belonging to Cu 2p 1 / 2 and Cu 2p 3 / 2 Cu 2p orbital 1 / 2 There are two peaks at 953.1eV and 951.0eV, which belong to Cu1 + and Cu. Cu 2p 3 / 2 There are two peaks at 933.2eV and 931.1eV, which belong to Cu 1+ XPS shows that the prepared sample contains tin, cuprous oxide and copper.
[0057] Figure 4 Sn@Cu prepared in Example 1 2 Transmission electron microscopy (TEM) and high-resolution transmission electron microscopy (HRTEM) images of O@Cu. Figure a is a transmission electron microscopy image, and figure b is a high-resolution transmission electron microscopy image.
[0058] from Figure 4 In a, we can see that a single Sn@Cu 2 The diameter of the O nanowires is about 200 nanometers and Figure 4 The high-resolution transmission electron microscopy image in (b) shows that the interplanar spacing is 0.21 nm, 0.245 nm, and 0.29 nm, corresponding to Cu(111), Cu 2 O(110), Sn(200) crystal planes.
[0059] In order to study the uniformity of lithium metal deposition on the surface of the current collector, the CuO@Cu prepared in step 1 of Example 1 and the Sn@Cu prepared in Example 1 were prepared. 2 O@Cu deposited lithium (Sn@Cu prepared in Example 1 2 O@Cu was used as the positive electrode, with the treated side close to the separator, and the lithium sheet was used as the negative electrode to assemble a button cell. The electrolyte was 1M LITFSI dissolved in DOL / DME (v:v=1:1) + 2% LiNO 3 , 40 μl on each of the positive and negative electrodes. -2 The Sn@Cu 2 The surface deposition capacity of O@Cu electrode is 5 mAh cm -2 Lithium, after disassembling the battery, we get Li@Sn@Cu 2 O@Cu electrode;) CuO@Cu and Sn@Cu after a certain amount of lithium deposition 2 O@Cu was analyzed by SEM, see Figure 5 As shown;
[0060] Figure 5 The scanning electron microscope images of the samples after lithium deposition, a and b in the figure are scanning electron microscope images of CuO@Cu prepared in step 1 of Example 1 after lithium deposition, c and d are scanning electron microscope images of Sn@Cu prepared in Example 1 2 SEM image of O@Cu after lithium deposition;
[0061] Figure 5 a and b are electrodeposition of 5 mAh cm -2 Scanning electron microscope image of the CuO@Cu surface of lithium. It is not difficult to see that the lithium metal deposited on the CuO@Cu surface is not uniform. Many dendritic lithium grows on the edge of the deposition area, and is mainly concentrated on the skeleton. The high-magnification image shows that its surface is rough and uneven. These dendritic lithium will break from the root during charging and discharging, generating a large amount of "dead lithium"; Figure 5 c and d are electrodeposited 5 mAh cm -2 Sn@Cu on Li metal 2 SEM image of the O@Cu surface shows that a large amount of lithium metal is deposited on the surface of the current collector. There is no dendritic lithium generated at the edge of the deposition and in the cavity, and the deposition on the skeleton surface is very uniform. From the high-power image, it can be seen that the surface of the current collector is smooth, indicating that lithium metal is deposited on Sn@Cu. 2 O@Cu is uniformly deposited in the current collector.
[0062] Coulombic efficiency is a key factor in evaluating battery sustainability. Its value is the ratio of the lithium metal capacity stripped from the current collector to the lithium metal capacity deposited on the current collector. The size of the coulombic efficiency directly indicates the utilization rate of lithium metal and the performance of the current collector during the battery cycle. CE is measured by electroplating a certain amount of lithium at a specific current density and then charging to 1.0V in different cycles. 2 O@Cu assembled half-cell (prepared Sn@Cu 2 O@Cu was used as the positive electrode, with the treated side close to the separator, and the lithium sheet was used as the negative electrode to assemble a button cell. The electrolyte was 1M LITFSI dissolved in DOL / DME (v:v=1:1) + 2% LiNO 3 , 40 μl on each of the positive and negative electrodes; at 1 mA cm -2 The current density is 1 mAh cm -2 The 1M LITFSI was dissolved in DOL / DME (v:v=1:1) + 2% LiNO 3 For LITFSI and LiNO 3 Dissolved in a mixture of DOL and DME to obtain an electrolyte, wherein the volume ratio of DOL to DME in the mixture of DOL and DME is 1:1, the concentration of LITFSI in the electrolyte is 1 mol / L, and LiNO3 The mass fraction is 2%), and the coulombic efficiency of the half-cell is tested. Figure 6 As shown;
[0063] Figure 6 The Sn@Cu prepared in Example 1 2 The O@Cu assembled half-cell has a current density of 1 mAh cm -2 、Li-plating capacity is 1 mAhcm -2 Coulomb efficiency under
[0064] from Figure 6 It can be seen that Sn@Cu 2 O@Cu at a current density of 1 mAh cm -2 、Li-plating capacity is 1 mAhcm -2 In the case of Sn@Cu, the average Coulombic efficiency is maintained at 98.47% over 400 cycles; this indicates that 2 O@Cu exhibits excellent reversibility and high lithium utilization.
[0065] To reveal Sn@Cu 2 The electrochemical properties of O@Cu current collectors are 2 O@Cu was used as the working electrode and lithium sheet as the counter electrode to assemble a symmetrical battery for charge and discharge tests. Figure 7 As shown; (Prepared Sn@Cu 2 O@Cu was used as the positive electrode, with the treated side close to the separator, and the lithium sheet was used as the negative electrode to assemble a button cell. The electrolyte was 1M LITFSI dissolved in DOL / DME (v:v=1:1) + 2% LiNO 3 , 40 μl on each of the positive and negative electrodes. -2 The Sn@Cu 2 The deposition capacity on O@Cu electrode is 5 mAh cm -2 After lithium, at 1mAcm -2 Current density, 1 mAh cm -2 Symmetrical battery test is performed at the surface capacity of .
[0066] Figure 7 The Sn@Cu prepared in Example 1 2 Symmetrical cells assembled from O@Cu at 1 mA cm -2 The current density is 1 mAh cm -2 Cyclic stability diagram under area capacity;
[0067] from Figure 7 It can be seen that: at 1mAcm -2 The current density is 1 mAh cm -2 Under the area capacity of Sn@Cu2 The O@Cu@Li battery can stably cycle for 1400 hours, indicating that the present invention can inhibit the growth of lithium dendrites and improve the cycle life and cycle stability of the battery.
[0068] Finally, Sn@Cu 2 O@Cu@Li and LiFePO 4 (LFP) pairing to study the electrochemical performance of the full cell. The mass loading of active material in the LFP electrode is ~4 mg cm -2 ,See Figure 8 As shown; (the Sn@Cu2O@Cu@Li electrode prepared in Example 2 is used as the negative electrode, so that the treated side is close to the diaphragm, LiFePO 4 (LFP) was used as the positive electrode to assemble button cells, 1M LITFSI was dissolved in DOL / DME (v:v=1:1) + 2% LiNO 3 , 50 microliters on each of the positive and negative electrode surfaces. Full battery charge and discharge tests were performed at a current density of 5C;)
[0069] The 1M LITFSI is dissolved in DOL / DME (v:v=1:1) + 2% LiNO 3 For LITFSI and LiNO 3 Dissolved in a mixture of DOL and DME to obtain an electrolyte, wherein the volume ratio of DOL to DME in the mixture of DOL and DME is 1:1, the concentration of LITFSI in the electrolyte is 1 mol / L, and LiNO 3 The mass fraction is 2%.
[0070] Figure 8 The Sn@Cu prepared in Example 1 2 O@Cu and LiFePO 4 (LFP) Sn@Cu paired assembly 2 Coulombic efficiency and discharge capacity of O@Cu@Li||LFP full cell at 5C.
[0071] Figure 8 It can be seen that: lithium-containing deposited anode (capacity: 5 mAh cm -2 ) 2 O@Cu@Li||LFP full cell has 96 mAh g at 5C -1 The initial discharge capacity is 93 mAhg after 1000 cycles. -1 , with a high capacity retention rate of 96.87%. These results show that the lithium metal battery anode material provided by the present invention can provide excellent discharge specific capacity and cycle life.
Claims
1. A method for preparing a tin-modified cuprous oxide nanowire three-dimensional copper-based current collector, Features The preparation method is specifically completed according to the following steps:
1. Preparation of CuO@Cu: The copper foam was used as the working electrode, the platinum sheet was used as the counter electrode, and the sodium hydroxide solution was used as the electrolyte. -2 ~20mAcm -2 Electrodepositing for a period of time at a current density of 1000 nm to generate copper hydroxide nanowires to obtain a reaction product I; washing the reaction product I, vacuum drying it, and then placing it in a muffle furnace for heat treatment for a period of time, and taking it out after the temperature drops to room temperature to obtain a copper oxide nanowire / foam copper composite material; The concentration of the sodium hydroxide solution described in step 1 is 1 mol / L to 2 mol / L; The electrodeposition time in step 1 is 5 to 20 minutes; 2. Preparation of Sn@Cu 2 O@Cu: ① Immerse the copper oxide nanowire / foam copper composite material in a mixed solution of NaCl and anhydrous ethanol, and then add SnCl 4 ·5H 2 O ethanol solution, continue to stir and react for 1h~2h after the addition is completed, then let it stand for 1h~2h, then wash and vacuum dry to obtain reaction product II; The mixed solution of NaCl and anhydrous ethanol described in step 2① is prepared by mixing a NaCl solution with a concentration of 100 g / L to 200 g / L and anhydrous ethanol, wherein the volume ratio of the NaCl solution to the anhydrous ethanol is 0.2:20; the SnCl described in step 2① 4 ·5H 2 The concentration of O ethanol solution is 0.7g / L~1g / L; SnCl described in step 2① 4 ·5H 2 The volume ratio of O ethanol solution to the mixed solution of NaCl and anhydrous ethanol is 10:(20-25); ②, placing the reaction product II in a plasma reaction chamber, raising the temperature to 200°C to 300°C, introducing hydrogen into the plasma reaction chamber, maintaining the pressure of the reaction chamber at 10Pa to 20Pa during the glow discharge process, and the power of the radio frequency plasma at 250W to 300W. The reaction product II is continuously treated for 120 seconds to 240 seconds, and then taken out after the temperature drops to room temperature to obtain a tin-modified cuprous oxide nanowire three-dimensional copper-based current collector; In step 2②, the flow rate of hydrogen gas introduced into the plasma reaction chamber is 15 sccm to 20 sccm.
2. The method for preparing a tin-modified cuprous oxide nanowire three-dimensional copper-based current collector according to claim 1, Features In step 1, the reaction product I is washed 3 to 5 times with deionized water and anhydrous ethanol respectively; the vacuum drying temperature in step 1 is 60° C. to 100° C., and the vacuum drying time is 12 h to 24 h.
3. The method for preparing a tin-modified cuprous oxide nanowire three-dimensional copper-based current collector according to claim 1, Features The temperature of the heat treatment in step 1 is 250° C. to 300° C., and the time of the heat treatment is 2 h to 5 h.
4. The method for preparing a tin-modified cuprous oxide nanowire three-dimensional copper-based current collector according to claim 1, Features The cleaning described in step 2① is to use deionized water and anhydrous ethanol to clean for 3 to 5 times respectively; the vacuum drying temperature is 40°C to 65°C, and the vacuum drying time is 5h to 20h.
5. Application of a tin-modified cuprous oxide nanowire three-dimensional copper-based current collector prepared by the preparation method according to claim 1, Features A tin-modified cuprous oxide nanowire three-dimensional copper-based current collector is used as an anode for lithium metal batteries.