Method for measuring surface parameters of copper foil, method for screening copper foil, and method for producing surface-treated copper foil
By setting the L filter cutoff value and calculating ISO25178 surface parameters, copper foils that meet a specific range are screened out, which solves the problem of insufficient correlation between copper foil surface roughness measurement and high-frequency characteristics in the existing technology, and improves the quality of printed circuit boards. high frequency performance.
Patent Information
- Application Number
- CN202180101984.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-22
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-12-22
AI Technical Summary
The existing copper foil surface roughness measurement method cannot fully reflect the high-frequency characteristics, resulting in the problem of high-frequency signal transmission loss not being reduced.
By setting the cutoff value of the L filter, the corrugated component of the surface profile of the untreated copper foil is removed, the surface parameters specified by ISO25178 are calculated, and the copper foil whose parameters such as Sa, Sq, Sz, Sdr, Vmc and Sk meet the specific range are screened out. Used in the manufacture of printed circuit boards for high frequencies.
It effectively removes the corrugation component and retains the rough component for high-frequency characteristics, improves the measurement accuracy of the correlation between surface parameters and high-frequency characteristics, and improves the high-frequency performance of the printed circuit board.
Smart Images

Figure CN117916553B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for measuring surface parameters of copper foil, a method for screening copper foil and a method for producing surface-treated copper foil. Background Art
[0002] In the manufacturing process of printed circuit boards, copper foil is widely used in the form of a copper-clad laminate bonded to an insulating resin substrate. In this regard, in order to prevent the stripping of wiring during the manufacture of printed circuit boards, it is desired that the copper foil and the insulating resin substrate have a high adhesion. For this reason, in the conventional copper foil for printed circuit board manufacturing, the bonding surface of the copper foil is subjected to surface treatment such as roughening treatment to form concavo-convex surfaces composed of fine copper particles, and the concavo-convex surfaces are engaged into the interior of the insulating resin substrate by stamping to exert an anchoring effect, thereby improving adhesion.
[0003] In recent years, with the high functionality of portable electronic devices, the high frequency of signals is developing in order to process a large amount of information at high speed, and printed circuit boards suitable for high-frequency applications are required. For such high-frequency printed circuit boards, in order to be able to transmit without reducing the quality of high-frequency signals, it is expected to reduce transmission losses. The printed circuit board has a copper foil processed into a wiring pattern and an insulating substrate. As the main losses in transmission loss, conductor loss caused by the copper foil and dielectric loss caused by the insulating substrate can be listed.
[0004] As a copper foil used in a high-frequency printed circuit board, for example, Patent Document 1 (Japanese Patent Publication No. 2020-50954) discloses a micro-roughened electrolytic copper foil having a micro-roughened surface including multiple peaks, multiple grooves, and multiple microcrystalline clusters, and according to this copper foil, the loss in signal transmission can be effectively suppressed. In addition, Patent Document 1 also records the measurement of the Rlr value of the copper foil under the conditions of λs=2.5μm and λc=0.003mm using a laser microscope.
[0005] However, it is known that the high-frequency characteristics (frequency dependence of transmission loss) of a printed circuit board are related to the surface roughness of the copper foil. Generally, the lower the roughness of the copper foil, the better the high-frequency characteristics tend to be. As a method for measuring the surface roughness of copper foil, for example, non-patent document 1 (Guide to the Test Method for High-Speed Transmission Lines of Flexible Printed Circuit Boards, 1st Edition) discloses a three-dimensional test method based on the surface profile of the copper foil for high-frequency transmission lines. Non-patent document 1 records that in this test method, the arithmetic mean height Sa is calculated by using a measuring device (confocal microscope) based on ISO25178 and using a specified S filter (0.5μm or 0.8μm) and an L filter (25μm, 50μm or 80μm) for processing.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application Publication No. 2020-50954
[0009] Patent Document 2: Japanese Patent Application Laid-Open No. 9-241882
[0010] Patent Document 3: WO2008 / 041706A1
[0011] Non-patent literature
[0012] Non-patent document 1: Guidelines for testing methods of high-speed transmission lines for flexible printed circuit boards, 1st edition, Japan Electronics and Circuits Association, published on June 5, 2019 Summary of the invention
[0013] However, the correlation between the surface parameters calculated by the conventional surface roughness measurement method of copper foil and the high-frequency characteristics is not necessarily sufficient.
[0014] The present inventors have obtained the following findings: the cutoff value of the L filter is set based on the surface profile of the untreated copper foil, and then the surface profile of the surface treated copper foil derived from the untreated copper foil is processed using the L filter with the pre-set cutoff value, and the surface parameters specified in ISO25178 are calculated. The surface parameter expression obtained in this way is highly correlated with the high-frequency characteristics.
[0015] Therefore, an object of the present invention is to provide a method for measuring a surface parameter of a copper foil which is highly correlated with high-frequency characteristics.
[0016] According to one embodiment of the present invention, a method for measuring surface parameters of a copper foil is provided, comprising the following steps:
[0017] Step (a), a step of obtaining a surface profile of at least one surface of an untreated copper foil;
[0018] Step (b), a step of setting a cutoff value of the L filter based on the surface profile;
[0019] Step (c), a step of obtaining a surface profile of at least one surface of the surface-treated copper foil derived from the untreated copper foil;
[0020] Step (d), a step of filtering the surface profile of the surface treated copper foil, including the step of using an L filter with the cutoff value for processing; and
[0021] The step (e) is a step of calculating at least one of the surface parameters specified in ISO 25178 of the surface of the surface-treated copper foil based on the surface profile after the filtering process.
[0022] According to another aspect of the present invention, a method for screening copper foil is provided, comprising the following steps:
[0023] The step of measuring the surface parameters of the copper foil using the method, wherein the surface parameters are at least one selected from the group consisting of the arithmetic mean height Sa, the root mean square height Sq, the maximum height Sz, the interface expansion area ratio Sdr, the solid volume Vmc of the center part, and the level difference Sk of the center part specified in ISO25178; and
[0024] The following samples were selected: Sa was less than 1.2 μm, Sq was less than 2.5 μm, Sz was less than 14 μm, Sdr was less than 60%, Vmc was less than 1.5 μm. 3 The following and / or the above-mentioned process of preparing a copper foil having a surface with an Sk of 4 μm or less as a copper foil suitable for a printed wiring board for high-frequency applications.
[0025] According to another aspect of the present invention, there is provided a method for producing a surface-treated copper foil, comprising the following steps:
[0026] The process of preparing untreated copper foil;
[0027] A step of performing surface treatment on at least one surface of the untreated copper foil to produce a surface-treated copper foil;
[0028] A step of measuring the surface parameters of the surface-treated copper foil using the method; and
[0029] The process of providing the surface-treated copper foil for shipment or recognizing it as a product for shipment only when the surface parameters meet the prescribed conditions,
[0030] The surface profile obtained in the step (a) is obtained on at least one surface of the untreated copper foil, and the surface profile obtained in the step (c) is obtained on the surface of the surface-treated copper foil subjected to the surface treatment.
[0031] According to still another aspect of the present invention, there is provided a method for producing a printed wiring board for high-frequency applications, the method comprising the step of producing the printed wiring board for high-frequency applications using the copper foil obtained by the method. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 This is a diagram for explaining the load curve and load area ratio determined according to ISO25178.
[0033] Figure 2This is a diagram for explaining the load area ratio Smr1 separating the protruding peak portion from the center portion, the load area ratio Smr2 separating the protruding valley portion from the center portion, and the level difference Sk of the center portion, which are determined based on ISO25178.
[0034] Figure 3 This is a diagram for explaining the substantial volume Vmc of the center portion determined in accordance with ISO25178.
[0035] Figure 4 This is a schematic diagram of a copper foil surface having a plurality of bumps, and is a diagram for explaining the α value.
[0036] Figure 5 This is a process flow chart for explaining the method for measuring the surface parameters of the copper foil of the present invention.
[0037] Fig. 6A This is a diagram showing the Sdr of the deposition surface of the untreated copper foil I subjected to the L filter process based on each cutoff value in Example A1.
[0038] Figure 6B This is a diagram showing the α value of the precipitation surface of the untreated copper foil I subjected to the L filter process based on each cutoff value in Example A1.
[0039] Figure 7 This is a diagram showing the second-order differential of Sdr before and after the L filter treatment on the deposition surface of the untreated copper foil I.
[0040] Fig. 8A This is a diagram showing the Sdr of the electrode surface of the untreated copper foil I subjected to the L filter process based on each cutoff value in Example A1.
[0041] Figure 8B This is a diagram showing the α value of the electrode surface of the untreated copper foil I subjected to the L filter process based on each cutoff value in Example A1.
[0042] Fig. 9 1 is a diagram showing the second-order differential of Sdr before and after the L filter treatment on the electrode surface of the untreated copper foil I.
[0043] Fig. 10A This is a diagram showing the Sdr of the deposition surface of the untreated copper foil II subjected to the L filter process based on each cutoff value in Example A1.
[0044] Fig. 10B This is a diagram showing the α value of the deposition surface of the untreated copper foil II subjected to the L filter process based on each cutoff value in Example A1.
[0045] Fig.11 This is a diagram showing the second-order differential of Sdr before and after the L filter treatment on the deposition surface of the untreated copper foil II.
[0046] Fig.12 The coefficient of determination R of the regression equation between the surface parameters of the copper foil and the transmission loss in Examples A1 to A3 is 2 A diagram for comparison.
[0047] Fig.13 This is a diagram showing the correlation between the arithmetic mean height Sa of the copper foils a to d in Example B1 and the high frequency characteristics.
[0048] Fig.14 The correlation between the change rate of Sdr of the untreated copper foils I and II in Examples B2 to B5 and the high frequency characteristics of the copper foils a to d (determination coefficient R 2 )’s picture.
[0049] Fig.15 The correlation between the change rate of the α value of the untreated copper foils I and II in Examples B2 to B5 and the high-frequency characteristics of the copper foils a to d (determination coefficient R 2 )’s picture.
[0050] Fig.16 This is a diagram showing the correlation between the arithmetic mean height Sa of the copper foils a to d in Example B3 and the high frequency characteristics. DETAILED DESCRIPTION
[0051] definition
[0052] Definitions of terms and parameters used to define the present invention are as follows.
[0053] In this specification, "arithmetic mean height Sa" or "Sa" is a parameter indicating the average of the absolute values of the height differences of each point relative to the average plane of the surface specified in ISO 25178. That is, Sa corresponds to a parameter obtained by extending the arithmetic mean height Ra of the profile curve to the surface.
[0054] In this specification, "root mean square height Sq" or "Sq" is a parameter corresponding to the standard deviation of the distance from the mean plane specified by ISO25178, and corresponds to the standard deviation of the height.
[0055] In this specification, "maximum height Sz" or "Sz" means the distance from the highest point to the lowest point of a surface as specified in ISO25178.
[0056] In this specification, "interface expansion area ratio Sdr" or "Sdr" refers to: a parameter indicating how much the expansion area (surface area) of a defined area increases relative to the area of the defined area as specified in ISO25178. It should be noted that in this specification, the interface expansion area ratio Sdr is expressed as the increase in the surface area (%). The smaller the value, the closer the surface shape is to being flat, and the Sdr of a completely flat surface is 0%. On the other hand, the larger the value, the more uneven the surface shape is. For example, when the Sdr of a surface is 40%, it means that the surface area of the surface has increased by 40% from a completely flat surface.
[0057] In this specification, the "surface load curve" (hereinafter referred to as "load curve") refers to a curve indicating the height of the load area ratio from 0% to 100% as specified in ISO25178. Figure 1 The following are parameters that represent the area of the area above a certain height c. The load area ratio at height c is equivalent to Figure 1 Smr(c) in Figure 2 As shown in FIG. 1 , a secant line of the load curve is drawn from the load area rate of 0% with the load area rate difference set to 40%, and the secant line of the load curve is moved from the load area rate of 0%. The position where the slope of the secant line is the most gentle is called the central part of the load curve. With respect to the central part, the straight line with the smallest sum of the squares of the deviations from the vertical axis direction is called the equivalent straight line. The portion of the equivalent straight line included in the range of the height of the load area rate of 0% to 100% is called the central part. The portion higher than the central part is called the protruding peak, and the portion lower than the central part is called the protruding valley.
[0058] In this specification, the "center level difference Sk" is the value obtained by subtracting the minimum height from the maximum height of the center according to ISO25178. Figure 2 The figure shows the parameters calculated by the height difference between the load area ratio of 0% and 100% passing through the equivalent straight line.
[0059] In this specification, the “central volume Vmc” or “Vmc” is Figure 3 Parameters indicating the volume of the center portion are specified in accordance with ISO 25178. In this specification, Vmc is calculated by specifying the load area ratio Smr1 separating the center portion and the protruding peak portion to be 10% and the load area ratio Smr2 separating the center portion and the protruding valley portion to be 80%.
[0060] In this specification, the "α value" refers to a parameter obtained by dividing the solid volume Vmc of the center by the level difference Sk of the center and multiplying it by the interface expansion area ratio Sdr, that is, by the formula (Vmc / Sk)×Sdr. Here, a schematic diagram of the copper foil surface for explaining the α value is shown in Figure 4 . In Figure 4 In the copper foil surface having a plurality of bumps N shown in (i), Vmc corresponds to the volume of the center portion of the bump N excluding the protruding portion, and Sk corresponds to the height of the center portion (see Figure 4 (ii)). Therefore, it can be considered that Vmc divided by Sk, that is, Vmc / Sk, corresponds to the area of the central part (see Figure 4 (iii)), the α value obtained by multiplying Vmc / Sk by Sdr is a parameter reflecting the Sdr of the center (see Figure 4 (iv)).
[0061] In this specification, "untreated copper foil" refers to copper foil that has not been subjected to surface treatment such as roughening treatment or rustproofing treatment. The copper foil referred to here may be copper foil having a support layer, a release layer, and an ultra-thin copper layer (so-called copper foil with carrier).
[0062] In this specification, "surface-treated copper foil derived from untreated copper foil" refers to copper foil obtained by subjecting untreated copper foil to surface treatment such as roughening treatment and rust-proofing treatment.
[0063] In this specification, the "electrode surface" of the electrolytic copper foil refers to the surface on the side in contact with the cathode during production.
[0064] In this specification, the "deposition surface" of the electrolytic copper foil refers to the surface on the side where the electrolytic copper is deposited during production, that is, the surface on the side not in contact with the cathode.
[0065] In this specification, "L filter" is a filter that removes relatively large wavelength components, and is also referred to as "λc" in the profile method measurement (line roughness measurement). That is, the L filter is a filter that removes large-scale wavelength components such as copper foil waviness.
[0066] In this specification, "S filter" refers to a filter that removes smaller wavelength components, and is also referred to as "λs" in the profile method measurement (line roughness). That is, the S filter is a filter that removes small-scale wavelength components in the roughening process of copper foil, etc.
[0067] Method for measuring surface parameters of copper foil
[0068] The method of the present invention is a method for measuring the surface parameters of copper foil. The method includes the steps of (1) obtaining the surface profile of untreated copper foil, (2) setting the cutoff value of the L filter, (3) obtaining the surface profile of the surface treated copper foil, (4) filtering the surface profile of the surface treated copper foil, and (5) calculating the surface parameters of the surface treated copper foil.
[0069] Hereinafter, steps (1) to (5) will be described respectively with reference to the drawings.
[0070] (1) Obtaining the surface profile of untreated copper foil
[0071] An example of a method for measuring the surface parameters of the copper foil according to the present invention is shown below. Figure 5 First, if Figure 5 As shown in (i), the surface profile of at least one surface of the untreated copper foil 10 is obtained. The surface profile can be obtained for one surface of the untreated copper foil 10, or for both surfaces of the untreated copper foil 10.
[0072] The surface profile of the untreated copper foil 10 can be preferably obtained by measuring the surface of the untreated copper foil 10 using a non-contact surface roughness measuring instrument, such as a commercially available laser microscope. When the laser microscope is used for measurement, the measurement area is preferably set to 90 μm 2 Above and 103000μm 2 Below, more preferably 1000 μm 2 Above and 26000μm 2 Below, it is more preferably set to 1000 μm 2 Above and 17000μm 2 In addition, the measurement magnification of the laser microscope is preferably 50 times or more and 500 times or less, and more preferably 100 times or more and 400 times or less.
[0073] The untreated copper foil 10 may be manufactured according to a known method and conditions, or may be a commercial product. In addition, the untreated copper foil 10 may be any one of an electrolytic copper foil and a rolled copper foil, preferably an electrolytic copper foil. When the untreated copper foil 10 is an electrolytic copper foil, the surface profile may be obtained for the surface of any one of the electrode surface and the precipitation surface of the electrolytic copper foil, preferably for the surface of the side subjected to surface treatment.
[0074] (2) Setting the cutoff value of the L filter
[0075] The cutoff value of the L filter is set based on the obtained surface profile of the untreated copper foil 10. Thus, in the process described later, a surface parameter indicating a high correlation with high frequency characteristics can be calculated.
[0076] As mentioned above, in the copper foil for the common printed circuit board manufacturing, the bonding surface of the copper foil is subjected to surface treatment such as roughening treatment to improve the adhesion with the insulating resin substrate. In this regard, in the existing measurement method, in order to evaluate the performance of the copper foil product, the surface profile of the surface-treated copper foil (surface-treated copper foil) is measured. However, the correlation between the surface parameters calculated by this method and the high-frequency characteristics is not necessarily sufficient.
[0077] The reason is not clear yet, but it is considered as follows. That is, the unevenness of the treated surface of the surface-treated copper foil is composed of a roughness component caused by bumps (roughened particles, etc.) and a corrugation component caused by the corrugation of the copper foil. At this point, the transmission loss of the printed circuit board increases due to the skin effect of the copper foil, and the skin effect of the copper foil is more obvious at higher frequencies, but the corrugation component hardly affects the transmission loss, and the roughness component mainly affects the transmission loss. Therefore, if the corrugation component can be selectively removed by filtering the surface profile of the surface-treated copper foil, it can be considered that the surface parameters derived from the roughness component that is highly correlated with the high-frequency characteristics can be calculated. However, if Figure 5 As shown in (ii), the surface treated copper foil 14 forms bumps 12 (e.g., roughened particles) on the corrugations of the untreated copper foil 10 through surface treatment. Therefore, when determining filtering conditions based on the surface profile of the surface treated copper foil, it is affected by the roughness components generated by the surface treatment (such as the roughness components generated by the bumps 12, etc.), and it is difficult to determine the conditions for selectively removing the corrugation components. Therefore, the correlation between the surface parameters of the surface treated copper foil calculated by the conventional method and the high frequency characteristics is not necessarily sufficient.
[0078] In contrast, in the method of the present invention, before measuring the surface profile of the surface treated copper foil, the surface profile of the untreated copper foil before the surface treatment is measured and the cutoff value of the L filter is set. As a result, the conditions of the L filter that can selectively remove the ripple component can be set without being affected by the roughness component generated by the surface treatment. Therefore, by adopting the conditions of the L filter as the filter treatment conditions of the surface treated copper foil, the surface parameters of the surface treated copper foil that are highly correlated with the high frequency characteristics can be calculated.
[0079] According to a preferred embodiment of the present invention, the cutoff value of the L filter is set as follows: (i) Sa1, which is Sa after the L filter treatment, satisfies 0.5 μm or less, and (ii) the change rate of Sdr before and after the L filter treatment: (|Sdr0-Sdr1| / Sdr0)×100 satisfies 80% or less (wherein Sdr0 is Sdr before the L filter treatment, and Sdr1 is Sdr after the L filter treatment). The cutoff value of the L filter is more preferably set such that Sa1 is 0.3 μm or less and the change rate of Sdr is 70% or less, further preferably such that Sa1 is 0.001 μm or more and 0.3 μm or less and the change rate of Sdr is 0.1% or more and 60% or less, and particularly preferably such that Sa1 is 0.005 μm or more and 0.2 μm or less and the change rate of Sdr is 1% or more and 40% or less. That is, Sa1 is preferably 0.5 μm or less, more preferably 0.3 μm or less, further preferably 0.001 μm or more and 0.3 μm or less, and particularly preferably 0.005 μm or more and 0.2 μm or less. When Sa1 is within the above range, the ripple component that is difficult to affect the high-frequency characteristics can be more effectively removed. In addition, the rate of change of Sdr is preferably 80% or less, more preferably 70% or less, further preferably 0.1% or more and 60% or less, and particularly preferably 1% or more and 40% or less. When the rate of change of Sdr is within the above range, the roughness component (bump component) that has a large influence on the high-frequency characteristics can be more reliably retained. That is, when the cutoff value for removing the roughness component is used based on the L filter for processing, the rate of change of Sdr will increase. Therefore, by controlling the rate of change of Sdr within the above range, the removal of the roughness component required for evaluating the high-frequency characteristics can be effectively suppressed. Therefore, by setting the cutoff value of the L filter to meet the above conditions, the surface parameters of the surface-treated copper foil that are more highly correlated with the high-frequency characteristics can be calculated in the process described later.
[0080] According to another preferred embodiment of the present invention, the cutoff value of the L filter is set as follows: (i) Sa1, which is Sa after the L filter treatment, satisfies 0.5 μm or less, and (ii') the change rate of the α value before and after the L filter treatment: (|α0-α1| / α0)×100 satisfies 80% or less (wherein α0 is the α value before the L filter treatment, and α1 is the α value after the L filter treatment). The cutoff value of the L filter is more preferably set in a manner such that Sa1 is 0.3 μm or less and the change rate of the α value is 70% or less, further preferably in a manner such that Sa1 is 0.001 μm or more and 0.3 μm or less and the change rate of the α value is 0.1% or more and 60% or less, and particularly preferably in a manner such that Sa1 is 0.005 μm or more and 0.2 μm or less and the change rate of the α value is 1% or more and 40% or less. That is, Sa1 is preferably 0.5 μm or less, more preferably 0.3 μm or less, further preferably 0.001 μm or more and 0.3 μm or less, and particularly preferably 0.005 μm or more and 0.2 μm or less. When Sa1 is within the above range, the ripple component that is difficult to affect the high-frequency characteristics can be more effectively removed. In addition, the rate of change of the α value is preferably 80% or less, more preferably 70% or less, further preferably 0.1% or more and 60% or less, and particularly preferably 1% or more and 40% or less. When the rate of change of the α value is within the above range, the rough components (bump components) that have a large impact on the high-frequency characteristics can be more reliably retained. That is, when filtering is performed with a cutoff value for removing the rough components, the rate of change of the α value becomes larger. Therefore, by controlling the rate of change of the α value within the above range, the removal of the rough components required for evaluating the high-frequency characteristics can be more effectively suppressed. Therefore, by setting the cutoff value of the L filter to meet the above conditions, the surface parameters of the surface-treated copper foil that are more highly correlated with the high-frequency characteristics can be calculated in the process described later.
[0081] The cutoff value of the L filter can be set as follows. First, the surface profile of the untreated copper foil 10 is preliminarily analyzed using multiple cutoff values of the L filter, and the surface parameters of each cutoff value are calculated. Then, based on the calculated surface parameters, a preferred cutoff value is determined from the above multiple cutoff values. For example, such a cutoff value can be preferably determined by finding a change point according to each condition described in the embodiment of this specification.
[0082] (3) Obtaining the surface profile of surface-treated copper foil
[0083] like Figure 5As shown in (ii), the surface profile of at least one surface of the surface-treated copper foil 14 originating from the untreated copper foil 10 is obtained. The surface-treated copper foil 14 is obtained by subjecting the untreated copper foil 10 to any surface treatment. Examples of such surface treatments include roughening treatment, rust-proof treatment, coupling agent treatment, and any combination thereof. For example, the surface-treated copper foil 14 is preferably provided with roughened particles (bumps) by subjecting the untreated copper foil 10 to at least roughening treatment, or may be subjected to only rust-proof treatment without roughening treatment.
[0084] The surface of the surface-treated copper foil 14 on which the surface profile is obtained is preferably the surface on which the surface treatment is applied to the untreated copper foil 10. In addition, typically, the surface of the surface-treated copper foil 14 on which the surface profile is obtained is on the same side as the surface of the untreated copper foil 10 on which the surface profile is obtained. However, in the case where both sides of the untreated copper foil 10 have similar surface profiles (for example, in the case of rolled copper foil), the surface of the untreated copper foil 10 on which the surface profile is obtained and the surface of the surface-treated copper foil 14 on which the surface profile is obtained may be on opposite sides to each other.
[0085] The surface profile of the surface-treated copper foil 14 can be obtained using various known devices such as AFM (atomic force microscope), contact surface roughness measuring instrument, non-contact surface roughness measuring instrument, etc. For example, it is preferable to use a commercially available laser microscope as a non-contact surface roughness measuring instrument to measure the surface of the surface-treated copper foil 14. The measurement conditions using the laser microscope can be, for example, the above-mentioned conditions for obtaining the surface profile of the untreated copper foil 10.
[0086] (4) Filtering treatment of the surface profile of surface treated copper foil
[0087] The surface profile of the obtained surface-treated copper foil 14 is subjected to filtering. The filtering process includes processing using an L filter having a cutoff value set based on the surface profile of the untreated copper foil 10. As a result, the ripple component of the copper foil that is unlikely to affect the high-frequency characteristics can be selectively removed as described above, and the surface parameters reflecting the roughness component that has a large influence on the high-frequency characteristics can be calculated.
[0088] The filtering process is preferably performed without using an S filter. When the S filter is used for processing, the concavities and convexities smaller than the cutoff value of the S filter are averaged (removed). Therefore, by performing the filtering process without using an S filter, small bumps (roughened particles, etc.) present in the surface-treated copper foil 14 can be reliably detected, and as a result, surface parameters that are more highly correlated with high-frequency characteristics can be calculated.
[0089] (5) Calculation of surface parameters of surface treated copper foil
[0090] Based on the surface profile after filtering, at least one of the surface parameters specified in ISO 25178 of the surface of the surface-treated copper foil 14 is calculated. The surface parameters calculated through the above process are parameters that fully exclude the influence of the ripple component and accurately reflect the roughness component of the surface-treated copper foil 14, and therefore are highly correlated with high-frequency characteristics.
[0091] Preferred examples of the calculated surface parameters include Sa, Sq, Sz, Sdr, Vmc, Sk, and combinations thereof (e.g., α value), more preferably Sa, Sq, Sdr, Vmc, Sk, and combinations thereof, further preferably Sa, Sdr, Vmc, Sk, and combinations thereof, and particularly preferably Sa, Sdr, and combinations thereof. These surface parameters are more highly correlated with high-frequency characteristics.
[0092] Copper foil screening method
[0093] According to a preferred embodiment of the present invention, there is provided a method for selecting copper foil, comprising the steps of measuring the surface parameters of the copper foil according to the above method, and selecting the copper foil having the predetermined surface parameters as the copper foil suitable for printed wiring boards for high frequency applications.
[0094] The surface parameter of the copper foil measured in this method is at least one selected from the group consisting of Sa, Sq, Sz, Sdr, Vmc and Sk. In addition, the copper foil having a surface with Sa, Sdr, Vmc and / or Sk within the range shown in Table 1 is selected as the copper foil suitable for printed circuit boards for high-frequency applications.
[0095] [Table 1]
[0096]
[0097] As described above, the surface parameters of the copper foil measured by the method of the present invention are highly correlated with the high-frequency characteristics, and thus can be used as an indicator to replace the high-frequency characteristics. In this regard, the copper foil having a surface that satisfies the surface parameters within the above range can be judged to have particularly excellent high-frequency characteristics, and thus can be said to be a copper foil suitable for printed circuit boards for high-frequency applications.
[0098] Method for producing surface treated copper foil
[0099] The method for measuring the surface parameters of the copper foil according to the present invention can be preferably used for product management, quality assurance, etc. According to a preferred embodiment of the present invention, a method for manufacturing a surface-treated copper foil is improved. The method for manufacturing the surface-treated copper foil includes the following steps: a step of preparing an untreated copper foil; a step of performing a surface treatment on at least one surface of the untreated copper foil to manufacture a surface-treated copper foil; a step of measuring the surface parameters of the surface-treated copper foil using the above method; and a step of supplying the surface-treated copper foil to the factory or identifying it as a product supplied to the factory only when the surface parameters meet the specified conditions.
[0100] That is, in the method for manufacturing the surface-treated copper foil, for at least one surface of the prepared untreated copper foil, (1) a surface profile is obtained, and (2) the untreated copper foil is subjected to surface treatment after the cutoff value of the L filter is set to manufacture the surface-treated copper foil. Then, for the surface of the surface-treated copper foil that has been subjected to surface treatment, (3) a surface profile is obtained, (4) the surface profile of the surface-treated copper foil is subjected to filtering, and (5) surface parameters are calculated. By utilizing the surface parameters calculated through such a process, high-quality products can be easily and reliably screened and shipped. The measurement of the surface profile of the surface-treated copper foil and the calculation of the surface parameters can be performed immediately after the manufacture of the surface-treated copper foil, or can be performed during the inspection before shipment.
[0101] The conditions that the surface parameters of the surface-treated copper foil should satisfy can directly adopt the above-mentioned conditions for the screening method of copper foil. In addition, the preferred forms of untreated copper foil and surface-treated copper foil are as described above. The thickness of the surface-treated copper foil (in the case of a carrier copper foil, the thickness of the ultra-thin copper layer) is preferably 0.5 μm or more and 210 μm or less, and more preferably 0.5 μm or more and 70 μm or less.
[0102] The surface-treated copper foil is preferably used for a printed wiring board for high-frequency applications of 1 GHz or higher, more preferably 3 GHz or higher, and further preferably 20 GHz or higher and 300 GHz or lower.
[0103] Method for manufacturing printed circuit board
[0104] According to a preferred embodiment of the present invention, a method for manufacturing a printed circuit board for high-frequency applications is provided. The method for manufacturing a printed circuit board includes a step of manufacturing a printed circuit board for high-frequency applications using the copper foil obtained by the above method. The printed circuit board can adopt a known layer structure. That is, in addition to using the copper foil or surface-treated copper foil screened or manufactured by the method of the present invention, the manufacture of the printed circuit board can also adopt known methods and conditions, and is not particularly limited.
[0105] Example
[0106] The present invention is further described in detail by the following examples.
[0107] [Examples A1~A3]
[0108] According to the method of the present invention, the cutoff value of the L filter is set based on the surface profile of the untreated copper foil, and the correlation between the surface parameters of the copper foil and the high-frequency characteristics is confirmed. The details are as follows.
[0109] Example A1
[0110] The cutoff value of the L filter was set according to the method of the present invention, and then the correlation between the surface parameters of the copper foil and the high-frequency characteristics was confirmed.
[0111] (1) Preparation of untreated copper foil
[0112] As untreated copper foils, two types of copper foils (separated foils) were prepared as they were in the form of electrolytic foils.
[0113] - Untreated copper foil I: 18 μm or 35 μm thick, manufactured by the method disclosed in Patent Document 2 (Japanese Patent Application Laid-Open No. 9-241882)
[0114] - Untreated copper foil II: 18 μm thick, manufactured by the method disclosed in Patent Document 3 (WO2008 / 041706A1)
[0115] (2) Obtaining the surface profile of untreated copper foil
[0116] A laser microscope (OLS-5000 manufactured by Olympus Corporation) was used to measure the area of 4096 μm 2 The surfaces of the untreated copper foils I and II were measured at a magnification of 200 times to obtain the surface profile. The measurement was performed on both the electrode surface and the precipitation surface of the untreated copper foil I, and only on the precipitation surface of the untreated copper foil II.
[0117] (3) Setting the cutoff value of the L filter
[0118] Sdr, Vmc and Sk are calculated by analyzing the surface profile of the untreated copper foil. Specifically, the cutoff value of the L filter is changed to 0.3μm, 0.5μm, 1.0μm, 1.5μm, 2.0μm, 2.5μm, 3.0μm, 3.5μm, 4.0μm, 4.5μm, 5.0μm, 6.0μm, 7.0μm, 8.0μm, 9.0μm, 10μm and 64μm for analysis, and Sdr, Vmc and Sk after L filtering using each cutoff value are calculated. In addition, Sdr, Vmc and Sk are calculated in the same way without the cutoff condition based on the L filter. The α value (= (Vmc / Sk) × Sdr) is calculated based on the calculated Sdr, Vmc and Sk, and the second-order differential of Sdr before and after the L filtering and the second-order differential of the α value are calculated. The Sdr and α values of the deposited surface of the untreated copper foil I after L filtering based on each cutoff value are shown in FIG. Fig. 6A and 6B , and the second-order differential of Sdr before and after L filtering is shown in Figure 7 In addition, the Sdr and α values of the electrode surface of the untreated copper foil I after L filtering based on each cutoff value are shown in Fig. 8A and 8B , and the second-order differential of Sdr before and after L filtering is shown in Fig. 9 In addition, the Sdr and α values of the precipitation surface of the untreated copper foil II after L filtering based on each cutoff value are shown in Fig. 10A and 10B , and the second-order differential of Sdr before and after L filtering is shown in Fig.11 .
[0119] Regarding the deposition surface of the untreated copper foil I, it was confirmed that when the cutoff value based on the L filter was 5.0 μm, the Sdr and α values reached the change point (see Fig. 6A , 6B On the other hand, regarding the electrode surface of the untreated copper foil I, it was confirmed that the Sdr and α values reached a change point when the cutoff value based on the L filter was 3.5 μm (see Fig. 8A , 8B In addition, regarding the precipitation surface of the untreated copper foil II, it was confirmed that the Sdr value and the α value reached a change point when the cutoff value based on the L filter was 3.0 μm (see Fig. 10A , 10Band 11). According to the above results, respectively, for the precipitation surface of untreated copper foil I, the cutoff value of the L filter is set to 5.0μm; for the electrode surface of untreated copper foil I, the cutoff value of the L filter is set to 3.5μm; for the precipitation surface of untreated copper foil II, the cutoff value of the L filter is set to 3.0μm. It should be noted that the "change point" mentioned here refers to the point where the slope of the graph in the figure showing the relationship between the cutoff value and the surface parameter (here Sdr and α value) changes greatly. When the cutoff value is set to a value less than the change point, it means that the area where the small bumps on the surface are actually averaged (removed) falls. However, since it is difficult to strictly and clearly define the "change point", it is a concept that allows a certain degree of width. When the second-order differential in the relationship between the cutoff value and the surface parameter is used, the accuracy of determining the "change point" becomes higher, which helps to set a more preferred cutoff value. In this embodiment, the "change point" is obtained by second-order differentials of the Sdr and α values of the deposition surface and electrode surface of the untreated copper foil I and the deposition surface of the untreated copper foil II. When calculating the second-order differential, a three-region moving average is used to reduce the error.
[0120] (4) Surface treatment of untreated copper foil
[0121] As shown in Table 2, by surface treating (roughening) the electrode surface or precipitation surface of untreated copper foil I or II under known conditions, four kinds of surface treated copper foils (copper foils a to d) with different surface roughness were prepared. It should be noted that the prepared copper foils a to d all have the same properties (surface roughness and high frequency characteristics, etc.) as commercial products. In addition, the copper foil that was not surface treated on untreated copper foil II was directly used as copper foil e.
[0122] (5) Obtaining the surface profile of copper foil
[0123] A laser microscope (OLS-5000 manufactured by Olympus Corporation) was used to measure the area of 4096 μm 2 The surface treated surfaces of the copper foils a to d and the precipitation surface of the copper foil e were measured at a magnification of 200 times to obtain the surface profile.
[0124] (6) Filtering and calculation of surface parameters
[0125] The surface profile of each copper foil is filtered. At this time, as shown in Table 2, the cutoff value of the L filter is set to the value set in (3) above, that is, 5.0 μm for copper foil a and copper foil b, 3.5 μm for copper foil c, and 3.0 μm for copper foil d and copper foil e. Regarding this filtering process, only the processing based on the L filter is performed, and the processing based on the S filter is not performed. Based on the surface profile after filtering, Sa, Sdr, Vmc and Sk are calculated, and the α value is calculated. The results are shown in Table 2.
[0126] (7) Evaluation of high-frequency characteristics
[0127] Prepare a high-frequency substrate (MEGTRON6N manufactured by Panasonic) as an insulating resin substrate. The surface-treated copper foil is laminated on both sides of the insulating resin substrate in such a way that its surface-treated surface is in contact with the insulating resin substrate, and is laminated using a vacuum press at a temperature of 190°C and a pressing time of 120 minutes to obtain a copper-clad laminate with an insulation thickness of 136 μm. Then, the copper-clad laminate is etched to obtain a substrate for measuring transmission loss with a microstrip line formed in a manner with a characteristic impedance of 50Ω. The transmission loss (dB / cm) of the obtained transmission loss measurement substrate at 50 GHz was measured using a network analyzer (N5225B manufactured by Keysight Technologies). The results are shown in Table 2.
[0128] (8) Correlation between surface parameters and high-frequency characteristics
[0129] The evaluation results of each copper foil were plotted with transmission loss as the horizontal axis and surface parameter (Sdr or α value) as the vertical axis. Based on the plotted data, the regression equation was determined by linear approximation (least squares method) and the determination coefficient R was calculated. 2 As a result, the coefficient of determination R in the regression equation with Sdr as the vertical axis is 2 The coefficient of determination R in the regression equation when α is the vertical axis is 0.9202. 2 It is 0.9363.
[0130] [Table 2]
[0131]
[0132] Example A2
[0133] The correlation between the surface parameters and the high-frequency characteristics was confirmed in the same manner as in Example A1 except that the cutoff value of the L filter was set to 5.0 μm for the precipitation surface and electrode surface of the untreated copper foil I and the precipitation surface of the untreated copper foil II, that is, the surface profile of the copper foils a to e was filtered with the cutoff value of the L filter set to 5.0 μm. As a result, the determination coefficient R in the regression equation with Sdr as the vertical axis was 2 The coefficient of determination R in the regression equation when α is the vertical axis is 0.9092. 2 It should be noted that in Example A1, although the change points of Sdr and α values of the electrode surface of untreated copper foil I and the precipitation surface of untreated copper foil II are considered to be 3.5μm and 3.0μm, respectively, this is different from the set value of the cutoff value (5.0μm) in Example A2. Fig. 8A , 8BAs shown in FIGS. 10A and 10B , in the range of the cutoff value being 3.0 μm or more and 5.0 μm or less, the changes in the Sdr and α values are small, and therefore the above cutoff setting value can be used as a change point.
[0134] Example A3
[0135] In the step of setting the cutoff value of the L filter using the untreated copper foil, the cutoff value of the L filter on the deposition surface and electrode surface of the untreated copper foil I and the deposition surface of the untreated copper foil II was set to 2.0 μm, that is, the cutoff value of the L filter was set to 2.0 μm to perform the filtering process on the surface profile of the copper foils a to e. In addition, the correlation between the surface parameters and the high-frequency characteristics was confirmed in the same manner as in Example A1. As a result, the determination coefficient R in the regression equation when Sdr is the vertical axis is 2 The coefficient of determination R in the regression equation when α is the vertical axis is 0.8548. 2 It should be noted that in Example A1, although the change points of Sdr and α values of the deposition surface and electrode surface of the untreated copper foil I and the deposition surface of the untreated copper foil II are considered to be 5.0μm, 3.5μm and 3.0μm, respectively, this is different from the set value of the cutoff value (2.0μm) in Example A3. Fig. 6A , 6B As shown in FIGS. 8A, 8B, 10A and 10B, in the range of the cutoff value being 2.0 μm or more and 5.0 μm or less, the changes in Sdr and α value are small, so the above cutoff setting value can be used as a change point.
[0136] The coefficient of determination R of the regression equation between the surface parameter (Sdr or α value) of the copper foil and the transmission loss in Examples A1 to A3 is 2 The comparison diagram is shown in Fig.12 .like Fig.12 As shown, the correlation between the surface parameters and high-frequency characteristics of Examples A1 to A3 is good. That is, it was confirmed that the surface parameters of the copper foil accurately reflect the high-frequency characteristics by presetting the cutoff value of the L filter using the untreated copper foil. In addition, the surface parameters calculated by setting the cutoff value based on the surface parameters of the untreated copper foil alone (the surface parameters calculated in Example A1) are more correlated with the high-frequency characteristics than the surface parameters calculated by fixing the cutoff value of the L filter (the surface parameters calculated in Examples A2 and A3).
[0137] [Example B1~B5]
[0138] In the process of setting the cutoff value of the L filter according to the surface profile of the untreated copper foil, it was confirmed that by setting the cutoff value to satisfy the specified conditions, the surface parameters of the copper foil more accurately reflected the high frequency characteristics.
[0139] Example B1
[0140] (1) Preparation of untreated copper foil
[0141] Untreated copper foils I and II were prepared similarly to those in Example A1.
[0142] (2) Obtaining the surface profile of untreated copper foil
[0143] The surface profiles of the electrode surface and the deposition surface of the untreated copper foil I and the deposition surface of the untreated copper foil II were obtained in the same manner as in Example A1.
[0144] (3) Setting the cutoff value of the L filter
[0145] For each surface profile of the obtained untreated copper foil, Sa, Sdr, Vmc and Sk were calculated by setting the cutoff value of the L filter to 32μm. As a result, it was confirmed that the Sa (i.e., Sa1) of the precipitation surface of the untreated copper foil I after the L filter treatment was a value exceeding 0.5μm (=1.16μm). In addition, Sdr, Vmc and Sk were calculated under the condition of no cutoff based on the L filter. Based on the calculated Sdr, Vmc and Sk, the α value (=(Vmc / Sk)×Sdr) was calculated, and the change rate of Sdr before and after the L filter treatment and the change rate of α value were calculated. As a result, the change rate of Sdr and the change rate of α value of the untreated copper foils I and I were both less than 80%.
[0146] (4) Surface treatment of untreated copper foil
[0147] Four types of surface-treated copper foils (copper foils a to d) having different surface roughness were prepared in the same manner as in Example A1.
[0148] (5) Obtaining the surface profile of copper foil
[0149] The surface treated surfaces of the copper foils a to d were measured using a laser microscope in the same manner as in Example A1 to obtain the surface profiles.
[0150] (6) Filtering and calculation of surface parameters
[0151] The surface profile of each copper foil was filtered. At this time, the cutoff value of the L filter was set to 32 μm. Regarding this filtering process, only the processing based on the L filter was performed, and the processing based on the S filter was not performed. Based on the surface profile after the filtering process, Sa, Sq, Sz, Sdr, Vmc and Sk were calculated, and the α value was calculated.
[0152] (7) Evaluation of high-frequency characteristics
[0153] In the same manner as in Example A1, copper foils a to d were used to prepare substrates for measuring transmission loss, and the transmission loss at 50 GHz was measured.
[0154] (8) Correlation between surface parameters and high-frequency characteristics
[0155] The evaluation results of each copper foil are plotted with transmission loss as the horizontal axis and surface parameters (Sa, Sq, Sz, Sdr, Vmc, Sk or α value) as the vertical axis. Based on the data graph, the regression equation is determined by linear approximation (least squares method) and the determination coefficient R is calculated. 2 The results are shown in Table 3. It should be noted that the graph showing the correlation between Sa and high frequency characteristics in copper foils a to d is shown in Fig.13 .
[0156] Example B2
[0157] The correlation between the surface parameters and the high frequency characteristics was confirmed in the same manner as in Example B1 except that the cutoff value of the L filter using the untreated copper foil and the cutoff value of the L filter treatment of the surface profile of the copper foils a to d was set to 10 μm. The results are shown in Table 3.
[0158] The correlation between the change rate of Sdr in untreated copper foil I and II and the high frequency characteristics (determination coefficient R 2 ) is shown in Fig.14 , and the correlation between the change rate of the α value in the untreated copper foil I and II and the high-frequency characteristics (determination coefficient R 2 ) is shown in Fig.15 .like Fig.14 and 15 As shown, when the cutoff value of the L filter is set to 10 μm, the change rate of Sdr and the change rate of α value of the electrode surface and the precipitation surface of the untreated copper foil I and the precipitation surface of the untreated copper foil II are both 80% or less. In addition, when the cutoff value of the L filter is set to 10 μm, the value of Sa of the electrode surface and the precipitation surface of the untreated copper foil I and the precipitation surface of the untreated copper foil II is both 0.5 μm or less.
[0159] Example B3
[0160] The correlation between the surface parameters and the high-frequency characteristics was confirmed in the same manner as in Example B1, except that the cutoff value of the L filter using the untreated copper foil and the cutoff value in the L filter treatment of the surface profile of the copper foils a to d was set to 5.0 μm. The results are shown in Table 3. It should be noted that the graph showing the correlation between Sa and the high-frequency characteristics of the copper foils a to d is shown in Fig.16 .
[0161] like Fig.14 and 15As shown, when the cutoff value of the L filter is set to 5.0 μm, the change rate of Sdr and the change rate of α value of the electrode surface and the precipitation surface of the untreated copper foil I and the precipitation surface of the untreated copper foil II are both 80% or less. In addition, when the cutoff value of the L filter is set to 5 μm, the value of Sa of the electrode surface and the precipitation surface of the untreated copper foil I and the precipitation surface of the untreated copper foil II is both 0.5 μm or less.
[0162] Example B4
[0163] The correlation between the surface parameters and the high frequency characteristics was confirmed in the same manner as in Example B1 except that the cutoff value of the L filter using the untreated copper foil and the L filter treatment of the surface profiles of the copper foils a to d was set to 2.0 μm. The results are shown in Table 3.
[0164] like Fig.14 and 15 As shown, when the cutoff value of the L filter is set to 2.0 μm, the change rate of Sdr and the change rate of α value of the electrode surface and the precipitation surface of the untreated copper foil I and the precipitation surface of the untreated copper foil II are both 80% or less. In addition, when the cutoff value of the L filter is set to 10 μm, the value of Sa of the electrode surface and the precipitation surface of the untreated copper foil I and the precipitation surface of the untreated copper foil II is both 0.5 μm or less.
[0165] Example B5
[0166] The correlation between the surface parameters and the high frequency characteristics was confirmed in the same manner as in Example B1 except that the cutoff value of the L filter using the untreated copper foil and the L filter treatment of the surface profiles of the copper foils a to d was set to 0.5 μm. The results are shown in Table 3.
[0167] like Fig.14 and 15 As shown, when the cutoff value of the L filter is set to 0.5 μm, the change rate of Sdr and the change rate of α value on the electrode surface and precipitation surface of the untreated copper foil I and the precipitation surface of the untreated copper foil II are both greater than 80%. In addition, when the cutoff value of the L filter is set to 0.5 μm, the values of Sa on the electrode surface and precipitation surface of the untreated copper foil I and the precipitation surface of the untreated copper foil II are all less than 0.5 μm.
[0168] [Table 3]
[0169] Table 3
[0170]
Claims
1. A method for measuring surface parameters of a copper foil, comprising the following steps: Step (a), a step of obtaining a surface profile of at least one surface of an untreated copper foil; Step (b), a step of setting a cutoff value of the L filter based on the surface profile; The L filter is a filter that removes large-scale wavelength components. Step (c), a step of obtaining a surface profile of at least one surface of the surface-treated copper foil derived from the untreated copper foil; Step (d), a step of filtering the surface profile of the surface treated copper foil, including the step of using the L filter with the cutoff value for processing; and The step (e) is a step of calculating at least one of the surface parameters specified in ISO 25178 of the surface of the surface-treated copper foil based on the surface profile after the filtering process.
2. The method for measuring the surface parameters of the copper foil according to claim 1, wherein: In the step (d), the filtering process is performed without using an S filter which is a filter for removing a small-scale wavelength component.
3. The method for measuring the surface parameters of the copper foil according to claim 1 or 2, wherein: In the step (b), the cutoff value of the L filter is set as follows: (i) Sa1, which is the arithmetic mean height Sa after processing using the L filter, satisfies 0.5 μm or less, and (ii) The change rate of the interface expansion area ratio Sdr before and after the L filter treatment: (|Sdr0-Sdr1| / Sdr0)×100 satisfies 80% or less, where Sdr0 is the Sdr before the L filter treatment, Sdr1 is the Sdr after the L filter treatment, Sa and Sdr are surface parameters specified in ISO25178.
4. The method for measuring the surface parameters of the copper foil according to claim 3, wherein: The Sa1 is 0.3 μm or less and the change rate of the Sdr is 70% or less.
5. The method for measuring the surface parameters of copper foil according to claim 1 or 2, wherein: In the step (b), the cutoff value of the L filter is set as follows: (i) Sa1, which is the arithmetic mean height Sa after processing using the L filter, satisfies 0.5 μm or less, and (ii') The change rate of the α value obtained by dividing the solid volume Vmc of the center by the level difference Sk of the center and multiplying it by the interface expansion area ratio Sdr before and after the L filter processing, that is, by the formula (Vmc / Sk)×Sdr: (|α0-α1| / α0)×100 satisfies less than 80%, where α0 is the α value before the L filter processing and α1 is the α value after the L filter processing. Sa, Sdr, Vmc and Sk are surface parameters specified in ISO25178.
6. The method for measuring the surface parameters of the copper foil according to claim 5, wherein: The Sa1 is 0.3 μm or less and the rate of change of the α value is 70% or less.
7. A method for screening copper foil, comprising the following steps: A step of measuring a surface parameter of the copper foil using the method according to any one of claims 1 to 6, wherein the surface parameter is at least one selected from the group consisting of an arithmetic mean height Sa, a root mean square height Sq, a maximum height Sz, an interface expansion area ratio Sdr, a solid volume Vmc of the center portion, and a level difference Sk of the center portion specified in ISO25178; and The following samples were selected: Sa was 1.2 μm or less, Sq was 2.5 μm or less, Sz was 14 μm or less, Sdr was 60% or less, Vmc was 1.5 μm or less. 3 The following and / or the above-mentioned process of preparing a copper foil having a surface with an Sk of 4 μm or less as a copper foil suitable for a printed wiring board for high-frequency applications.
8. A method for manufacturing a surface-treated copper foil, comprising the following steps: The process of preparing untreated copper foil; A step of performing surface treatment on at least one surface of the untreated copper foil to produce a surface-treated copper foil; A step of measuring the surface parameters of the surface-treated copper foil using the method according to any one of claims 1 to 6; and A process of providing the surface-treated copper foil for shipment or identifying it as a product for shipment only when the surface parameters meet the prescribed conditions; The surface profile obtained in the step (a) is obtained on at least one surface of the untreated copper foil, and the surface profile obtained in the step (c) is obtained on the surface of the surface-treated copper foil subjected to the surface treatment.
9. The method for producing a surface-treated copper foil according to claim 8, wherein: The surface-treated copper foil is used for printed circuit boards for high-frequency applications above 1 GHz. 10 . A method for producing a printed wiring board for high-frequency applications, comprising the step of producing a printed wiring board for high-frequency applications using the copper foil obtained by the method according to claim 7 .
Citation Information
Patent Citations
Production of copper foil for printed circuit board
JP1997241882A
Fine roughened electrolytic copper foil and copper foil substrate
JP2020050954A
Method of preparing electrolytic copper solution acidified with sulfuric acid, sulfuric-acid-acidified electrolytic copper solution prepared by the preparation method, and electrodeposited copper film
WO2008041706A1
Novel methods for establishing contour outline reference surface in three-dimensional surface roughness assessment
CN101158573A
Roughened copper foil, copper-clad laminate and printed wiring board
CN107614760A