A CNT-FeCoNi / C aerogel composite microwave absorbing material and its preparation method
By synthesizing FeCoNi-MOF precursors via a solvothermal method and mixing them with nanocellulose and carbon nanotubes to form porous aerogels, the problems of high loading and insufficient microwave absorption in existing trimetallic MOF composite materials are solved, achieving lightweight, thin, and wide-bandwidth microwave absorption effects.
Patent Information
- Application Number
- CN202311738857.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-18
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-12-18
AI Technical Summary
Existing trimetallic MOF composite materials mainly exist in powder form, with high loading levels and insufficient microwave absorption performance, making it difficult to achieve lightweight, thin, and wide-band microwave absorption.
FeCoNi-MOF precursor powder was synthesized by solvothermal method, mixed with nanocellulose and carbon nanotubes to form an aerogel, and then freeze-dried and calcined at high temperature to generate a three-dimensional carbon framework-supported FeCoNi alloy/carbon composite, forming a porous structure to enhance electromagnetic wave reflection and scattering.
The prepared CNT-FeCoNi/C aerogel composite material exhibits high microwave absorption performance at low filling amounts. It is thin, has low filling amount, wide effective absorption bandwidth, and strong reflection loss, making it suitable for microwave absorption applications.
Smart Images

Figure CN117960056B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of microwave absorbing materials technology, specifically designing a CNT-FeCoNi / C aerogel composite microwave absorbing material and its preparation method. Background Technology
[0002] Ideal microwave absorbing (MWA) materials need to be lightweight, thin, highly absorbent, and have an effective absorption bandwidth. To explore novel MWA materials for practical applications, structural design and multi-component composite materials are often required to achieve synergistic effects.
[0003] Metal-organic frameworks (MOFs) are porous framework compounds formed through the self-assembly of metal ions and organic ligands. Due to their high porosity and high specific surface area, they can be retained even after high-temperature treatment, making them suitable as novel MWA materials. Organic ligands containing heteroatoms can be easily doped with heteroatoms, thereby enhancing their dipole polarization performance. Among these, porous carbon-based composites derived from magnetic transition metals (such as Fe, Co, and Ni) effectively overcome the limitations of traditional magnetic metal particles, such as high density, insufficient dispersibility, and susceptibility to corrosion and oxidation.
[0004] Researchers have proposed a technical solution to integrate trimetallic MOFs with carbon nanotubes (CNTs), graphene, and other materials into composite materials. However, most of the trimetallic MOFs in these composite materials exist mainly in powder form, which requires high loading levels and suffers from insufficient microwave absorption performance. Summary of the Invention
[0005] In view of this, one of the objectives of the present invention is to provide a method for preparing CNT-FeCoNi / C aerogel composite microwave absorbing material. The composite material prepared by this method has good impedance matching through the effective combination of multiple loss mechanisms, and has the characteristics of thinness, light weight, low filling amount, effective absorption bandwidth and strong absorption performance.
[0006] To achieve the above objectives, the present invention employs the following technical solution: a method for preparing a CNT-FeCoNi / C aerogel composite microwave absorbing material, comprising the following steps:
[0007] Step 1: Mix dimethylformamide (DMF), deionized water and ethanol as a mixed solvent. First add cobalt salt, nickel salt and iron salt to the mixed solvent, then add 2-aminoterephthalic acid and disperse evenly to obtain a mixed solution.
[0008] The mixed solution was transferred to a high-pressure reactor and reacted at 100-140℃ for 10-30 h. After the reaction, it was centrifuged at high speed, washed and dried to obtain FeCoNi-MOF precursor powder.
[0009] Step 2: Dissolve carbon nanotube powder in deionized water, add polyvinylpyrrolidone first, then add nanocellulose and hydrolyzed methyltrimethoxysilane in sequence and disperse them separately, and then add the FeCoNi-MOF precursor powder prepared in Step 1 to obtain a mixed dispersion of carbon nanotubes, nanocellulose and FeCoNi-MOF precursor powder.
[0010] Step 3: The mixed dispersion from Step 2 is rapidly frozen in liquid nitrogen and then freeze-dried to obtain an aerogel containing carbon nanotubes, nanocellulose and FeCoNi-MOF.
[0011] Step 4: Place the aerogel in an argon atmosphere and calcine it at 700-900℃ for 1-3 hours. The resulting aerogel product includes a three-dimensional carbon skeleton and a trimetallic FeCoNi alloy / carbon composite loaded on the pore walls of the skeleton, referred to as CNT-FeCoNi / C aerogel composite microwave absorbing material.
[0012] Further improvements to the preparation method of CNT-FeCoNi / C aerogel composite microwave absorbing materials:
[0013] Preferably, in the mixed solvent described in step 1, DMF, deionized water and ethanol are mixed in a volume ratio of 100:6:6.
[0014] Preferably, the cobalt salt, nickel salt, and iron salt mentioned in step 1 are cobalt nitrate hexahydrate, nickel nitrate hexahydrate, and ferrous chloride tetrahydrate, respectively.
[0015] Preferably, the molar ratio of the cobalt salt, nickel salt, and iron salt is 2:1:1, 1:2:1, or 1.5:1.5:1, and the molar ratio of the total molar amount of the cobalt salt, nickel salt, and iron salt to 2-aminoterephthalic acid is (3-3.2):1.
[0016] Preferably, the drying temperature in step 1 is 55-60℃ and the drying time is 20-24h.
[0017] Preferably, the mass ratio of carbon nanotube powder, polyvinylpyrrolidone, nanocellulose and FeCoNi-MOF precursor powder in step 2 is 100:30:2:100.
[0018] Preferably, in step 2, the concentration of carbon nanotube powder dissolved in deionized water is 0.03-0.1 g / ml.
[0019] Preferably, the preparation method of the hydrolyzed methyltrimethoxysilane is as follows: methyltrimethoxysilane and deionized water are mixed at a volume ratio of 1:1, and then a 5wt% hydrochloric acid solution is added. The amount of hydrochloric acid solution added accounts for 10% of the total volume of methyltrimethoxysilane and deionized water. The mixture is stirred thoroughly under an ice bath to obtain the hydrolyzed methyltrimethoxysilane. In step 2, the amount of hydrolyzed methyltrimethoxysilane added is 10wt%-20wt% of the total mass of the mixed dispersion system.
[0020] Preferably, in step 3, the temperature of liquid nitrogen is -210℃ to -196℃, the rapid freezing time is 3-5 min, the freeze-drying temperature is -80℃ to -30℃, the vacuum degree is below 20 Pa, and the time is 36-48 h; in step 4, the temperature is increased to the calcination temperature at a rate of 2-5℃ / min.
[0021] The second objective of this invention is to provide a CNT-FeCoNi / C aerogel composite microwave absorbing material prepared by any of the above-mentioned methods.
[0022] The advantages of this invention compared to the prior art are as follows:
[0023] 1) This invention provides a method for preparing CNT-FeCoNi / C aerogel composite microwave absorbing material. First, cobalt salt, nickel salt, and iron salt are added to a mixed solvent of DMF, deionized water, and ethanol. Then, 2-aminoterephthalic acid is added, and a spindle-shaped FeCoNi-MOF precursor powder is generated through a solvothermal reaction. Then, the FeCoNi-MOF precursor powder is mixed with nanocellulose and multi-walled carbon nanotubes. Under the crosslinking of silane coupling agent, the solvent is evaporated by directional freeze-drying to form a highly porous aerogel. The spindle-shaped trimetallic MOF is uniformly loaded on the pore walls of the carbon skeleton. Then, a high-temperature carbonization reaction is carried out to generate a trimetallic FeCoNi alloy / carbon aerogel composite material. In this composite material, FeCoNi / C is loaded on the pore walls of the three-dimensional carbon skeleton. The carbon aerogel skeleton helps to reflect and scatter electromagnetic waves (EMW) multiple times. Among them, renewable nanocellulose establishes a three-dimensional network through cross-linking, and multi-walled carbon nanotubes are introduced to enhance the conductivity of the network. They are also cross-linked with nanocellulose through hydrogen bonds to strengthen the carbon framework. The introduction of carbon nanotubes helps to optimize impedance matching by minimizing dielectric loss. The introduced trimetallic MOF solves the inherent limitations of single carbon materials. The resulting aerogel composite material has the properties of being lightweight, thin, low infill content, having a wide effective absorption bandwidth, and high reflection loss. The microwave absorption performance of the composite material can be controlled by adjusting the carbonization temperature, and high microwave absorption performance at low infill content is finally achieved, which has great potential in the field of microwave absorption.
[0024] 2) This invention provides a composite aerogel microwave absorbing material comprising a three-dimensional carbon framework and FeCoNi / C loaded on the pore walls of the three-dimensional carbon framework. The macropores of the three-dimensional porous aerogel allow more electromagnetic waves to enter, while the mesopores and micropores within promote multiple reflections and scattering of electromagnetic waves. This layered porous structure design is beneficial for the absorption and dissipation of electromagnetic waves. This complex porous structure significantly elongates the path of the incident wave, leading to multiple reflections and scattering, thereby promoting the attenuation of EMW. Simultaneously, the aerogel with its directional growth structure provides a considerable surface area for anchoring MOF-derived nanoparticles. Furthermore, the difference in conductivity between CNTs and FeCoNi / C leads to interfacial polarization. The three-dimensional network composed of multi-walled carbon nanotubes and the carbon framework enhances electron migration, thereby promoting conduction loss. In addition, the presence of defective functional groups and negatively charged sites in the multi-walled carbon nanotubes leads to defective polarization and dipole polarization. Adding alloys with different magnetic atoms to the composite material can produce efficient electron transfer and higher spin polarizability, thus surpassing the performance properties of single metals. The polarization relaxation was further amplified by introducing nitrogen (N) elements internally through doping. The unique spindle morphology of FeCoNi / C plays a crucial role in electromagnetic wave dissipation. Under the influence of an applied electric field, the high aspect ratio helps generate a strong local electric field at the tips. Simultaneously, the finite conductivity of the electrodes ensures a fast response, with each needle acting as a dipole to resonate with the incident electromagnetic wave, thus promoting energy dissipation. Finally, thanks to the MOF template, the carbon framework encapsulates the FeCoNi alloy, thereby enhancing the magnetic response of the composite material. In the frequency range of 2–18 GHz, the magnetic losses of CNT-FeCoNi / C are mainly caused by natural resonance, eddy current losses, and exchange resonance phenomena.
[0025] 3) The CNT-FeCoNi / C aerogel composite microwave absorbing material prepared by this invention, after being mixed with paraffin at a low filling amount of 5wt%, exhibits the following microwave absorption performance: at a frequency of 17.44GHz, the minimum reflection loss (RL) is -61.55dB when the thickness is 2.42mm; furthermore, when the thickness reaches 2.82mm, the effective absorption bandwidth extends to 7.2GHz, and it has more than 90% effective absorption of electromagnetic waves in the 10.8GHz to 18GHz frequency band. Attached Figure Description
[0026] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on the provided drawings without creative effort.
[0027] Figure 1The diagram shows the reflection loss of the CNT-FeCoNi / C aerogel composite absorbing material at different thicknesses in Example 1 of the present invention.
[0028] Figure 2 The diagram shows the reflection loss of the CNT-FeCoNi / C aerogel composite absorbing material at different thicknesses in Example 2 of this invention.
[0029] Figure 3 The diagram shows the reflection loss of the CNT-FeCoNi / C aerogel composite absorbing material at different thicknesses in Example 3 of this invention.
[0030] Figure 4 (a, b, c) are SEM images of CNF-CNT-FeCoNi MOFs aerogel obtained in step 3 of Example 2; Figure 4 (d, e, f) are SEM images of the CNT-FeCoNi / C aerogel composite microwave absorbing material prepared in step 4 of Example 2. Detailed Implementation
[0031] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of this invention without creative effort are within the scope of protection of this invention.
[0032] Example 1
[0033] This embodiment provides a method for preparing a CNT-FeCoNi / C aerogel composite microwave absorbing material, which specifically includes the following steps:
[0034] Step 1: Mix 60 mL DMF, 3.6 mL H2O and 3.6 mL ethanol, then add Co(NO3)2·6H2O (419.1 mg), Ni(NO3)2·6H2O (209.4 mg), FeCl2·4H2O (143.1 mg), and then add 2-aminoterephthalic acid (164.6 mg). The molar ratio of cobalt salt, nickel salt, iron salt and 2-aminoterephthalic acid is 1.44:0.72:0.72:0.91. Disperse by sonication for 10 min and stir magnetically for 25 min to obtain a mixed solution.
[0035] The mixed solution was transferred to a 100 mL stainless steel autoclave and kept at 120 °C for 24 hours. After the reaction, it was centrifuged at high speed, washed, and vacuum dried at 55 °C for 20 hours to obtain FeCoNi-MOF precursor powder.
[0036] Step 2, mix methyltrimethoxysilane and deionized water at a volume ratio of 1:1, then add 5 wt% hydrochloric acid solution with an added volume fraction of 10%, place the mixture in an ice bath under continuous stirring for 0.5 hours, to obtain 25 ml of hydrolyzed methyltrimethoxysilane;
[0037] Disperse 6 g of carbon nanotube powder in 120 ml of deionized water, then add 1.8 g of polyvinylpyrrolidone, after uniform ultrasonic dispersion, add 0.12 g of nanocellulose, perform ultrasonic dispersion and stir overnight, add 25 ml of the hydrolyzed methyltrimethoxysilane prepared above, after stirring for dissolution, add 6 g of the FeCoNi-MOF precursor powder prepared in Step 1, to obtain a mixed dispersion of carbon nanotubes, nanocellulose and FeCoNi-MOF precursor powder;
[0038] Step 3, pour the above mixed dispersion into a square cylindrical PTFE mold with a copper plate at the bottom, quick-freeze for 5 min in an insulated bucket filled with liquid nitrogen at -200°C, then transfer to a vacuum freeze dryer at a temperature of -50°C and a vacuum degree of 10 Pa for 48 h, to obtain an aerogel containing carbon nanotubes, nanocellulose and FeCoNi-MOF, denoted as CNF-CNT-FeCoNi MOFs aerogel;
[0039] Step 4, place the aerogel containing carbon nanotubes, nanocellulose and FeCoNi-MOF in a tube furnace, heat up to 700°C at a heating rate of 5°C / min under an argon atmosphere, and calcine at this temperature for 3 h, to obtain the CNT-FeCoNi / C aerogel composite wave-absorbing material.
[0040] Figure 1 is the reflection loss diagram tested at different thicknesses of the CNT-FeCoNi / C aerogel composite wave-absorbing material prepared by calcination at 700°C in Example 1; it can be seen from Figure 1 that when the thickness is 4.27 mm, the minimum reflection loss (RL) is -57.53 dB, and when the thickness is 2.61 mm, the effective absorption bandwidth is 6.56 GHz.
[0041] Example 2
[0042] This example provides a preparation method of a CNT-FeCoNi / C aerogel composite wave-absorbing material, the specific steps refer to Example 1, the difference is that the calcination temperature in Step 4 is 800°C, to obtain the CNT-FeCoNi / C aerogel composite wave-absorbing material.
[0043] Figure 2 is the reflection loss diagram tested at different thicknesses of the CNT-FeCoNi / C aerogel composite wave-absorbing material prepared by calcination at 800°C in Example 2; it can be seen from Figure 2It can be seen that when the thickness is 2.42mm, the minimum reflection loss (RL) is -61.55dB, and when the thickness is 2.82mm, the effective absorption bandwidth is 7.2GHz.
[0044] Example 3
[0045] This embodiment provides a method for preparing CNT-FeCoNi / C aerogel composite microwave absorbing material. The specific steps are the same as in Example 1, except that the calcination temperature in step 4 is 900℃, and the CNT-FeCoNi / C aerogel composite microwave absorbing material is obtained.
[0046] Figure 3 This is a reflection loss diagram of the CNT-FeCoNi / C aerogel composite microwave absorbing material prepared by calcination at 900℃ in Example 3, tested at different thicknesses; from Figure 3 It can be seen that when the thickness is 1.9mm, the minimum reflection loss (RL) is -59.40dB, and when the thickness is 2.25mm, the effective absorption bandwidth is 6GHz.
[0047] Figure 4 (a, b, c) are SEM images of CNF-CNT-FeCoNi MOFs aerogel obtained in step 3 of Example 2; Figure 4(d, e, f) are SEM images of the CNT-FeCoNi / C aerogel composite microwave absorbing material prepared in step 4 of Example 2. (a) is a scanning electron microscope image of the CNF-CNT-FeCoNi MOFs aerogel observed axially, showing large pores caused by upward ice crystal growth during freezing. (b) is a SEM image of the CNF-CNT-FeCoNi MOFs aerogel. Scanning electron microscope (SEM) images of MOF aerogels observed radially. The composite aerogels exhibit growth orientation controlled by ice crystals. During the preparation of the composite aerogels, we used a self-made mold with a copper base in contact with liquid nitrogen to rapidly form upward-growing ice crystals. After freeze-drying, the pore walls formed by the entanglement of TOCNF and MWCNT maintain a neatly arranged tubular pore structure, while the pore structure remains anisotropic after drying. A large number of vertically growing ice crystals tend to expel the trimetallic FeCoNi-MOFs, forcing them to aggregate on the pore walls. (c) is a magnified view of (b), showing FeCoNi-MOFs encapsulated by MWCNTs; (d) is a scanning electron microscope image of CCNT-FeCoNi / C aerogel observed axially; (e) is a scanning electron microscope image of CCNT-FeCoNi / C aerogel observed radially; and (f) is a magnified view of (e), showing the convex morphology of the FeCoNi alloy encapsulated by MWCNTs. This oriented structure forms an ordered conductive pathway. The large pores of the three-dimensional porous aerogel allow more electromagnetic waves to enter, while the internal mesopores and micropores promote multiple reflections and scatterings of electromagnetic waves. This layered porous structure design is beneficial for the absorption and dissipation of electromagnetic waves. This complex porous structure greatly elongates the path of the incident wave, leading to multiple reflections and scatterings, thereby promoting the attenuation of electromagnetic waves.
[0048] Those skilled in the art should understand that the above descriptions are merely several specific embodiments of the present invention, and not all embodiments. It should be noted that many modifications and improvements can be made by those skilled in the art, and all modifications or improvements not exceeding the scope of the claims should be considered within the protection scope of the present invention.
Claims
1. A method for preparing a CNT-FeCoNi / C aerogel composite wave-absorbing material, characterized in that, Includes the following steps: Step 1: Dimethylformamide (DMF), deionized water, and ethanol are mixed as a mixed solvent. Cobalt salt, nickel salt, and iron salt are added to the mixed solvent first, followed by 2-aminoterephthalic acid, and the mixture is dispersed evenly to obtain a mixed solution. The mixed solvent contains DMF, deionized water, and ethanol in a volume ratio of 100:6:
6. The cobalt salt, nickel salt, and iron salt are cobalt nitrate hexahydrate, nickel nitrate hexahydrate, and ferrous chloride tetrahydrate, respectively, with a molar ratio of 2:1:1, 1:2:1, or 1.5:1.5:
1. The total molar amount of the cobalt salt, nickel salt, and iron salt is in a molar ratio of (3-3.2):1 to 2-aminoterephthalic acid. The mixed solution was transferred to a high-pressure reactor and reacted at 100-140℃ for 10-30 h. After the reaction, it was centrifuged at high speed, washed and dried to obtain FeCoNi-MOF precursor powder. Step 2: Dissolve carbon nanotube powder in deionized water, add polyvinylpyrrolidone first, then add nanocellulose and hydrolyzed methyltrimethoxysilane sequentially and disperse them separately, then add the FeCoNi-MOF precursor powder prepared in Step 1 to obtain a mixed dispersion of carbon nanotubes, nanocellulose and FeCoNi-MOF precursor powder; the mass ratio of carbon nanotube powder, polyvinylpyrrolidone, nanocellulose and FeCoNi-MOF precursor powder is 100:30:2:100; the amount of hydrolyzed methyltrimethoxysilane added is 10wt%-20wt% of the total mass of the mixed dispersion system; Step 3: The mixed dispersion from Step 2 is rapidly frozen in liquid nitrogen and then freeze-dried to obtain an aerogel containing carbon nanotubes, nanocellulose and FeCoNi-MOF. Step 4: Place the aerogel in an argon atmosphere and calcine it at 700-900℃ for 1-3 hours. The resulting aerogel product includes a three-dimensional carbon skeleton and a trimetallic FeCoNi alloy / carbon composite loaded on the pore walls of the skeleton, referred to as CNT-FeCoNi / C aerogel composite microwave absorbing material.
2. The preparation method of the CNT-FeCoNi / C aerogel composite wave-absorbing material according to claim 1, characterized in that, The drying temperature in step 1 is 55-60℃, and the time is 20-24h.
3. The preparation method of the CNT-FeCoNi / C aerogel composite wave-absorbing material according to claim 1, characterized in that, In step 2, the concentration of carbon nanotube powder dissolved in deionized water is 0.03-0.1 g / ml.
4. The preparation method of the CNT-FeCoNi / C aerogel composite wave-absorbing material according to claim 1, characterized in that, The preparation method of the hydrolyzed methyltrimethoxysilane is as follows: Methyltrimethoxysilane and deionized water are mixed in a volume ratio of 1:1, and then a 5wt% hydrochloric acid solution is added. The amount of hydrochloric acid solution added accounts for 10% of the total volume of methyltrimethoxysilane and deionized water. The mixture is stirred thoroughly under an ice bath to obtain hydrolyzed methyltrimethoxysilane.
5. The preparation method of the CNT-FeCoNi / C aerogel composite microwave absorbing material according to claim 1, characterized in that, In step 3, the temperature of liquid nitrogen is -210℃ to -196℃, the rapid freezing time is 3-5 min, the freeze drying temperature is -80℃ to -30℃, the vacuum degree is below 20 Pa, and the time is 36-48 h; in step 4, the temperature is increased to the calcination temperature at a rate of 2-5℃ / min.
6. A CNT-FeCoNi / C aerogel composite microwave absorbing material prepared by the preparation method of any one of claims 1-5.
Citation Information
Patent Citations
High-absorption electromagnetic shielding and heat-conducting epoxy composite material as well as preparation method and application thereof
CN115850918A