Hydrogen storage alloy
By adjusting the composition and mechanical properties of the hydrogen storage alloy, and controlling the amount of Co and the crystal structure, the problem of reduced lifetime characteristics caused by reduced Co was solved, and a balance between improved output characteristics and lifetime characteristics was achieved.
Patent Information
- Application Number
- CN202280062331.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-10-22
- Filing Date
- 2022-06-16
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2042-06-16
AI Technical Summary
Reducing the amount of Co in existing hydrogen storage alloys leads to a decrease in battery life characteristics and an increase in output characteristics, making it difficult to maintain a balance between the two.
By adjusting the composition and mechanical properties of the hydrogen storage alloy, controlling the molar ratio of Co (d) to be above 0.00 and below 0.15, ensuring the H/E ratio to be above 0.08 and below 0.15, the C/B ratio to be above 0.30 and below 0.85, and the segregation rate to be above 0.01% and below 1.60%, and rationally controlling the crystal structure parameters, the cross-section of the hydrogen storage alloy was observed using nanoindentation and scanning electron microscopy.
This approach achieves a balance between the lifetime and output characteristics of the hydrogen storage alloy while reducing the amount of Co used, avoiding a decrease in lifetime characteristics due to reduced Co content and improving output characteristics.
Smart Images

Figure GDA0004740931580000231 
Figure GDA0004740931580000241 
Figure GDA0004740931580000242
Abstract
Description
Technical Field
[0001] This invention relates to hydrogen storage alloys. Background Technology
[0002] For AB5-type hydrogen storage alloys with a CaCu5-type crystal structure, such as alloys with Mm (mixed rare earth metals) as a rare earth element mixture at site A and Ni, Al, Mn, Co, etc. at site B (hereinafter referred to as "Mm-Ni-Mn-Al-Co alloy"), compared with alloys with other compositions, they have the following characteristics: they can be used to form negative electrodes at a relatively low cost, and can form closed nickel-metal hydride batteries with long cycle life and less internal pressure rise caused by gas generated during overcharging.
[0003] However, in the constituent elements of Mm-Ni-Mn-Al-Co alloys, Co is a crucial element that inhibits micronization and improves lifespan characteristics. However, Co is a very expensive metal; therefore, reducing the amount of Co used is desirable. From this perspective, Patent Document 1 proposes a method for manufacturing a hydrogen storage alloy with low Co content, using the general formula MmNi... a Mn b Al c Co d (where Mm is a mixed rare earth metal, 4.0≤a≤4.7, 0.3≤b≤0.65, 0.2≤c≤0.5, 0<d≤0.35, 5.2≤a+b+c+d≤5.5) represents a hydrogen storage alloy with a CaCu5 type crystal structure.
[0004] Patent document 2 proposes a hydrogen storage alloy with a parent phase having an AB5 type crystal structure. Site A is composed of rare earth elements containing La, while site B does not contain Co but contains Ni, Al and Mn. The molar ratio of Mn to Al is greater than 0.60 and less than 1.56, and the molar ratio of La to the sum of the molar ratios of Al and Mn, La / (Mn+Al), is greater than 0.92.
[0005] Existing technical documents
[0006] Patent documents
[0007] Patent Document 1: US2006 / 188385A1
[0008] Patent Document 2: US2019 / 348671A1 Summary of the Invention
[0009] However, reducing the amount of Co in hydrogen storage alloys with a CaCu5-type crystal structure tends to decrease battery life characteristics while increasing output characteristics. Therefore, it is desirable to reduce the amount of Co while maintaining both output and life characteristics. To this end, the objective of this invention is to provide a hydrogen storage alloy that overcomes the various drawbacks of the prior art described above.
[0010] [1]
[0011] This invention provides a hydrogen storage alloy containing Mm (Mm represents mixed rare earth metals), Ni, Mn, Al, and Co, and having a parent phase with a CaCu5 type crystal structure.
[0012] The total content of La and Ce in Mm is over 95% by mass.
[0013] When the molar numbers of Ni, Mn, Al, and Co relative to 1 mole of Mm are set as a, b, c, and d, respectively,
[0014] d is greater than 0.00 and less than 0.15.
[0015] d / b is above 0.00 and below 0.35.
[0016] The sum of a+b+c+d is greater than 5.22 and less than 5.44.
[0017] The ratio of hardness H (GPa) to composite modulus E (GPa) determined by nanoindentation is greater than 0.08 and less than 0.15.
[0018] [2]
[0019] The present invention provides a hydrogen storage alloy according to [1], wherein the hardness H is 1 GPa or more and 11 GPa or less.
[0020] [3]
[0021] The present invention provides a hydrogen storage alloy according to [1] or [2], wherein the ratio of the c-axis length to the a-axis length in the CaCu5 type crystal structure is 0.8080 or more and 0.8110 or less.
[0022] [4]
[0023] The present invention provides a hydrogen storage alloy according to any one of [1] to [3], wherein the c / b ratio is 0.30 or more and 0.85 or less.
[0024] [5]
[0025] The present invention provides a hydrogen storage alloy according to any one of [1] to [4], wherein, when the cross section of the hydrogen storage alloy is observed with a scanning electron microscope, the ratio of the area of the segregated phase to the area of the cross section is more than 0.01% and less than 1.60%. Detailed Implementation
[0026] The present invention will now be described based on its preferred embodiments.
[0027] The hydrogen storage alloy of the present invention has a parent phase of a CaCu5 type crystal structure, i.e., an AB5 type crystal structure, with space group number 191 (P6 / mmm).
[0028] The hydrogen storage alloy of the present invention contains Mm (Mm represents a mixture of rare earth metals), Ni, Mn, Al, and Co as its constituent elements. Preferably, in the hydrogen storage alloy, the A sites in the above-mentioned ABx composition are composed of Mm, while the B sites are composed of Ni, Mn, Al, and Co. Therefore, in a preferred embodiment of the hydrogen storage alloy, the hydrogen storage alloy is, for example, an AB5 type hydrogen storage alloy represented by the general formula: MmNiaMnbAlcCod. In the formula, a, b, c, and d represent the molar ratios of Ni, Mn, Al, and Co relative to 1 mole of Mm, respectively.
[0029] Various rare earth metal elements are known as Mm, but from the viewpoint of the output characteristics of the hydrogen storage alloy, it is preferable to use at least La and Ce as Mm in this invention. From this viewpoint, the total percentage of La and Ce in Mm is preferably 95% by mass or more, more preferably 96% by mass or more, and even more preferably 97% by mass or more. The total percentage of La and Ce in Mm can be 100% by mass.
[0030] From the viewpoint of the lifetime characteristics of the hydrogen storage alloy, the Ce content in Mm is preferably 13% by mass or more, more preferably 15% by mass or more, and more preferably 16% by mass or more. On the other hand, from the viewpoint of the output characteristics of a battery equipped with a hydrogen storage alloy, the Ce content in Mm is preferably 24% by mass or less, more preferably 22% by mass or less, and more preferably 21% by mass or less.
[0031] When a hydrogen storage alloy contains a rare earth metal element other than La and Ce as Mm, such rare earth metal element may be selected from the group consisting of Nd, Pr and Sm.
[0032] For the metallic elements other than Mm constituting the hydrogen storage alloy, namely Ni, Mn, Al, and Co, firstly, regarding Co, from the viewpoint of reducing costs, the molar ratio of Co when the molar ratio of Mm is set to 1, i.e., the molar ratio of Co d in the general formula, is preferably less than 0.15. Preferably, it is 0.14 or less, more preferably 0.13 or less, even more preferably 0.125 or less, and even more preferably 0.12 or less. From the viewpoint of reducing costs, a molar ratio of Co d of 0 is most preferred, but from the viewpoint of the performance of the hydrogen storage alloy, it is desirable to contain a small amount of Co. From this viewpoint, the molar ratio of Co d is preferably 0.01 or more, more preferably 0.025 or more, and even more preferably 0.05 or more. When the amount of Co contained in the hydrogen storage alloy is low, the lifetime characteristics of the alloy tend to decrease. However, in this invention, by appropriately controlling the alloy composition and the mechanical properties of the alloy (described later), even with a low amount of Co, the decrease in lifetime characteristics can be suppressed, and the output characteristics can be improved.
[0033] The inventors' research indicates that the relationship between the molar ratio of Co (d) and the molar ratio of Mn (b) affects the performance of the hydrogen storage alloy. Specifically, from the perspective of reducing the amount of Co used while enabling the hydrogen storage alloy to exhibit sufficient lifetime and output characteristics, a Co molar ratio d to Mn molar ratio b (d / b) of 0.35 or less is preferred. From the viewpoint of making this advantage even more significant, a d / b value of 0.34 or less is further preferred, and even more preferably 0.33 or less.
[0034] From the perspective of cost reduction, a d / b value of 0 is most preferred, but from the perspective of the performance of the hydrogen storage alloy, a d / b value slightly greater than 0 is desirable. From this perspective, a d / b value of 0.04 or higher is preferred, more preferably 0.06 or higher, and even more preferably 0.08 or higher.
[0035] In the hydrogen storage alloy of the present invention, from the viewpoint of suppressing excessive cracking of the hydrogen storage alloy accompanied by repeated hydrogen absorption and release, when the molar ratio of Mm constituting site A in the ABx composition is set to 1, the total molar ratio of the elements constituting site B (i.e., the sum of a+b+c+d in the above general formula) is preferably 5.22 or more. From the viewpoint of making this advantage more significant, the sum of a+b+c+d is further preferably 5.24 or more, and even more preferably 5.26 or more. On the other hand, from the viewpoint of the output characteristics of the battery when the hydrogen storage alloy is used as the electrode material of the battery, the sum of a+b+c+d is preferably 5.44 or less. From the viewpoint of making this advantage more significant, the sum of a+b+c+d is further preferably 5.42 or less, and even more preferably 5.40 or less.
[0036] When using the hydrogen storage alloy of the present invention as the negative electrode active material of a nickel-metal hydride battery, one solution to prevent a decrease in battery life characteristics is to suppress corrosion of the hydrogen storage alloy when it comes into contact with the alkaline aqueous solution used as the electrolyte. Therefore, the inventors' research results indicate that for a hydrogen storage alloy with a sufficiently low Co content and using Mn containing La and Ce, it is advantageous to adjust the ratio (c / b) of the molar ratio of Al (c) to the molar ratio of Mn (b) to a specified range. From this viewpoint, in the hydrogen storage alloy of the present invention, the value of c / b is preferably 0.30 or more, more preferably 0.31 or more, even more preferably 0.32 or more, even more preferably 0.33 or more, and even more preferably 0.34 or more. Furthermore, the value of c / b is preferably 0.85 or less, even more preferably 0.845 or less, even more preferably 0.840 or less, and even more preferably 0.835 or less.
[0037] In the hydrogen storage alloy of the present invention, from the viewpoint of solving the problems of the present invention, the molar ratios a, b, and c of Ni, Mn, and Al are not particularly limited. In particular, from the viewpoint of using the hydrogen storage alloy of the present invention as the negative electrode active material of Ni-MH batteries mounted in EVs and HEVs, the following considerations can be made.
[0038] For Ni, when the molar ratio of Mm constituting the A site in the ABx composition is set to 1, the molar ratio a of Ni is preferably 4.20 or more and 4.80 or less, more preferably 4.30 or more or 4.70 or less, and particularly preferably 4.35 or more or 4.60 or less.
[0039] For the molar ratio b of Mn, it is preferably 0.30 or more and 0.66 or less, more preferably 0.34 or more or 0.64 or less, and particularly preferably 0.38 or more or 0.62 or less.
[0040] The molar ratio c of Al is preferably 0.15 or more and 0.40 or less, more preferably 0.17 or more or 0.39 or less, and even more preferably 0.19 or more or 0.38 or less.
[0041] The hydrogen storage alloy of the present invention may contain impurities within a range that does not affect the effectiveness of the invention. For example, it may contain one or more of the elements selected from Fe, Cu, Ti, Mo, W, Si, Ca, Pb, Cd, Mg and Zr, each at a mass percentage of less than 0.05%.
[0042] The content and composition ratio of each element in the hydrogen storage alloy of the present invention can be determined by chemical composition analysis. It should be noted that when using the hydrogen storage alloy of the present invention as the negative electrode active material of Ni-MH batteries mounted in EVs and HEVs, the molar ratio of Al and Mn may sometimes change slightly during the battery manufacturing process and during battery use. However, the inventors' research results show that the amount of change, expressed as a molar ratio, is within approximately 0.03. Therefore, by analyzing the negative electrode active material collected from the Ni-MH battery in use, the elemental molar ratio of the hydrogen storage alloy in its initial state before use in the battery can be estimated.
[0043] The inventors' research results indicate that by adjusting the mechanical properties of the hydrogen storage alloy of the present invention, a balance between the lifetime and output characteristics of the hydrogen storage alloy can be achieved. Specifically, it is preferable to set the ratio of the hardness H (GPa) to the composite modulus E (GPa) of the hydrogen storage alloy, as measured by nanoindentation, to a value of 0.08 or higher and 0.15 or lower. The value of H / E is a quantity proportional to the yield strain and is a mechanical property value that can determine whether a material is easily damaged. It can be considered that a material that is easily damaged is fragile, meaning it is prone to brittle fracture. Therefore, it can be inferred that in the hydrogen storage alloy, this is a measure of the ease of fracture during repeated hydrogen absorption and release. It can be considered that by setting this value within the above range, the hydrogen storage alloy fractures to a degree that can maintain its lifetime characteristics during repeated hydrogen absorption and release, thereby improving the output characteristics. From this perspective, the value of H / E is further preferably 0.08 or higher and 0.148 or lower, even more preferably 0.08 or higher and 0.146 or lower, and even more preferably 0.08 or higher and 0.14 or lower.
[0044] To set the H / E value within the aforementioned range, a hydrogen storage alloy can be manufactured, for example, according to the manufacturing method described later. Furthermore, the methods for measuring the composite modulus E and hardness H will be explained in the embodiments described later.
[0045] The H / E value is preferably within the above-mentioned range. However, from the perspective of more easily achieving a balance between lifetime characteristics and output characteristics, the composite modulus E is preferably 4.0 GPa or more and 138.5 GPa or less, particularly preferably 4.1 GPa or more and 138.0 GPa or less, particularly preferably 4.2 GPa or more and 137.5 GPa or less, and even more preferably 35 GPa or more and 137.0 GPa or less.
[0046] From the same point of view, the value of hardness H is preferably 1.0 GPa or higher and 11.0 GPa or lower, particularly preferably 1.1 GPa or higher and 11.0 GPa or lower, particularly preferably 1.2 GPa or higher and 10.98 GPa or lower, and even more preferably 4.0 GPa or higher and 10.96 GPa or lower.
[0047] As described above, the hydrogen storage alloy of the present invention is preferably controlled to produce cracks to a moderate degree under repeated hydrogen absorption and release. Therefore, it is preferable to control the crystal structure of the hydrogen storage alloy in a manner capable of withstanding volume changes caused by hydrogen absorption and release. From this viewpoint, in the hydrogen storage alloy of the present invention, the ratio of the c-axis length to the a-axis length in the CaCu5 type crystal structure is preferably 0.8080 or more, more preferably 0.8084 or more, and more preferably 0.8088 or more. Furthermore, the ratio of the c-axis length to the a-axis length is preferably 0.8110 or less, more preferably 0.8109 or less, and more preferably 0.8107 or less.
[0048] The ratio of the c-axis length to the a-axis length is as described above, with the a-axis length itself being preferably within the range specified above. The above and The following are further preferred options. The above and The following is a further preferred option. The above and the following.
[0049] On the other hand, the value of the c-axis length itself is preferably conditional on the c-axis length / a-axis length being within the above-mentioned range. The above and The following are further preferred options. The above and The following is a further preferred option. The above and the following.
[0050] In the hydrogen storage alloy of the present invention, methods for adjusting the ratio of the c-axis length to the a-axis length include, for example, changing the composition ratio of the alloy, changing the cooling method and conditions after casting, or changing the heat treatment conditions. However, these methods are not limited to.
[0051] In this invention, the a-axis and c-axis lengths of the hydrogen storage alloy can be obtained by powder X-ray diffraction. In this case, the powder used for powder X-ray diffraction is sieved from -500 μm powder, and the undersize powder (-20 μm) obtained by sieving with a 20 μm sieve is used as the sample for measurement. It should be noted that if the sample size is insufficient after sieving alone, the -500 μm powder can be pulverized to obtain the required amount of powder for measurement. In the case of pulverization, it is necessary to perform pulverization under conditions that do not alter the crystal structure of the hydrogen storage alloy. Therefore, it is preferable to measure the a-axis length, c-axis length, and lattice volume under both pulverized and non-pulverized conditions, and compare the two measurements to confirm that the pulverization conditions are equivalent. The a-axis and c-axis lengths are determined by X-ray diffraction as described in the examples described later. For analysis, the Pawley method is used with the Fundamental Parameter as described in the examples described later.
[0052] In addition to adjusting the mechanical properties of the hydrogen storage alloy as described above, it is clarified that if a small amount of segregated phase is observed in the hydrogen storage alloy, the alloy further possesses both sufficient lifetime and output characteristics. The segregated phase refers to the phase generated during the manufacture of the hydrogen storage alloy of this invention, and is a phase with a different crystal structure from the parent phase, CaCu5. The inventors believe that the composition of the segregated phase, as a heterogeneous phase, is not necessarily defined, but it is mainly composed of Mn and Al, and also contains Ni and Co. Furthermore, the segregated phase does not possess hydrogen storage capacity. The presence or absence of the segregated phase can be confirmed by observing the cross-section of the hydrogen storage alloy of this invention using scanning electron microscopy backscattered electron (SEM-BSE) images. In the presence of the segregated phase, it is observed in the SEM-BSE image with a different contrast than the parent phase, thus making its presence or absence easily determined.
[0053] As mentioned above, the segregated phase does not possess hydrogen storage capacity. Therefore, when the hydrogen storage alloy absorbs and releases hydrogen, the segregated phase will not exhibit the volume change caused by the hydrogen absorption and release. Consequently, due to repeated hydrogen absorption and release, the segregated phase can easily become the initiation point for cracks in the hydrogen storage alloy. From the viewpoint of the lifetime characteristics of the hydrogen storage alloy, crack formation should be avoided. Therefore, from this perspective, it is desirable that the hydrogen storage alloy be free of segregated phases.
[0054] On the other hand, cracking in the hydrogen storage alloy leads to an increase in its surface area. An increased surface area means that in batteries using this alloy as an electrode material, the alloy has more opportunities to come into contact with the electrolyte; in other words, the battery's output characteristics improve. From this perspective, it is desirable to introduce segregated phases into the hydrogen storage alloy to induce cracking. However, from the perspective of battery lifespan, an excessively large surface area can exacerbate corrosion of the hydrogen storage alloy; therefore, an excessively large surface area should be avoided.
[0055] Considering the above advantages and disadvantages, in addition to adjusting the mechanical properties of the hydrogen storage alloy, this invention also compensates for the reduction in lifetime characteristics caused by reducing the amount of Co by controlling the segregated phase that may exist in the hydrogen storage alloy, thereby achieving a further balance between lifetime characteristics and output characteristics.
[0056] Based on the above viewpoints, in the hydrogen storage alloy of the present invention, when observing the cross-section of the hydrogen storage alloy with SEM-BSE images, the ratio of the area of the segregated phase to the area of the cross-section (hereinafter also referred to as the "segregation rate") is preferably set to 0.01% or more and 1.60% or less, more preferably 0.10% or more and 1.40% or less, more preferably 0.20% or more and 1.20% or less, and even more preferably 0.20% or more and 1.10% or less.
[0057] To set the segregation rate of the hydrogen storage alloy within the aforementioned range, the hydrogen storage alloy can be manufactured, for example, according to the manufacturing method described later. Furthermore, the method for determining the segregation rate will be explained in the examples described later.
[0058] Next, a suitable manufacturing method for the hydrogen storage alloy of the present invention will be described.
[0059] In this manufacturing method, raw materials of a hydrogen storage alloy, in which the ratio of each element is adjusted to form a specified alloy composition, are weighed and mixed. For example, the raw materials are melted into a molten liquid using a high-frequency furnace with induction heating. The molten liquid yields an alloy ingot, which is then crushed to obtain powder of the hydrogen storage alloy.
[0060] When melting the raw materials of the hydrogen storage alloy to form a molten liquid, the temperature of the molten liquid is preferably 1300 to 1600°C, more preferably 1350°C or higher or 1590°C or lower, and more preferably 1400°C or higher or 1580°C or lower.
[0061] The molten metal is then cooled to obtain an alloy ingot. For example, the molten metal can be poured into a mold to obtain an alloy ingot. A water-cooled mold can be used as the mold, for example. Since the cooling of the molten metal using a water-cooled mold is relatively slow, the resulting alloy ingot contains inhomogeneities in terms of crystallinity, such as crystallization strain, grain size, axial length, and lattice volume. To appropriately control these inhomogeneities and thus the mechanical properties of the alloy, it is preferable to perform a first heat treatment on the alloy ingot before crushing it. By performing heat treatment, some of the aforementioned inhomogeneities in the alloy ingot can be homogenized. For this purpose, the heat treatment is preferably performed under a vacuum or an inert gas atmosphere. There are no particular limitations on the type of inert gas; argon, neon, helium, nitrogen, etc., can be used. The temperature and time of the heat treatment can be appropriately set to moderately homogenize the aforementioned inhomogeneities in the alloy ingot. The inventors' research results show that satisfactory results can be obtained by performing heat treatment at a temperature of 900°C or higher and 1098°C, more preferably 1000°C or higher and 1096°C, and even more preferably 1050°C or higher and 1095°C for a time of preferably 1 hour or higher and 10 hours or lower, more preferably 2 hours or higher and 8 hours or lower, and even more preferably 2 hours or higher and 6 hours or lower.
[0062] Next, the alloy ingot, whose non-uniform crystallinity was homogenized by the first heat treatment, is subjected to a pulverization process to obtain powder. The degree of pulverization is preferably, for example, to a particle size (-500 μm) that passes through a 500 μm sieve. In particular, the degree of pulverization can be, as needed, up to a particle size (-1000 μm) that passes through a 1000 μm sieve, or up to a particle size (-850 μm) that passes through an 850 μm sieve. If over-pulverization occurs at this stage, magnetic separation efficiency may decrease; therefore, in the case of micronization, pulverization is preferably performed with a particle size (+150 μm) containing at least 50% by mass of particles with a size of 150 μm on a sieve.
[0063] Preferably, the powder obtained in this way is subjected to a second heat treatment. The purpose of this heat treatment is to further homogenize the residual crystalline inhomogeneities in the alloy, thereby accurately controlling the mechanical properties of the alloy within the target range. Since there are many crystalline inhomogeneities in the alloy ingot, it is not easy to accurately control the mechanical properties of the alloy within the target range by performing only a first heat treatment. Therefore, in this manufacturing method, the heat treatment is performed in two stages to homogenize the aforementioned crystalline inhomogeneities in stages, thereby accurately controlling the mechanical properties of the alloy within the target range.
[0064] The atmosphere for the second heat treatment can be the same as that for the first. The temperature and time of the heat treatment can be appropriately set in a way that makes the mechanical properties of the alloy within the target range. The inventors' research results show that satisfactory results can be obtained by performing heat treatment at a temperature of 900°C or higher and 1098°C or lower, more preferably 1000°C or higher and 1096°C or lower, and even more preferably 1050°C or higher and 1095°C or lower for a time of preferably 1 hour or higher and 10 hours or lower, more preferably 2 hours or higher and 8 hours or lower, and even more preferably 2 hours or higher and 6 hours or lower.
[0065] In this way, alloy powder with the target mechanical properties can be obtained. The alloy powder can then be crushed and sieved as needed to obtain the hydrogen storage alloy powder of the present invention.
[0066] In the above manufacturing method, molten hydrogen storage alloy is poured into a water-cooled mold to obtain an alloy ingot. However, alternatively, the molten alloy can be supplied to the circumference of a rotating water-cooled roller to obtain a thin strip. From the viewpoint of the cooling rate of the molten alloy and the thickness of the thin strip, the rotation speed of the roller is preferably 50 to 200 rpm, more preferably 55 rpm or more or 190 rpm or less, and more preferably 60 rpm or more or 180 rpm or less.
[0067] Cooling using a water-cooled roller results in a faster cooling rate for the molten metal compared to cooling using a water-cooled mold. This means that the cooled alloy contains fewer inhomogeneous crystal regions. Therefore, when cooling the molten metal using a water-cooled mold, the alloy requires two heat treatments, whereas when cooling the molten metal using a water-cooled roller, only one heat treatment is necessary. Thus, when cooling the molten metal using a water-cooled roller, only heat treatment of the resulting strip is required to reduce the aforementioned inhomogeneous crystal regions and adjust the alloy's mechanical properties to the target range. The powder obtained by pulverizing the heat-treated strip does not require further heat treatment.
[0068] Heat treatment is preferably performed under vacuum or inert gas atmosphere. The type of inert gas is not particularly limited; argon, neon, helium, nitrogen, etc., can be used. The temperature and time of heat treatment can be appropriately set in a way that makes the mechanical properties of the alloy within the target range. The inventors' research results show that satisfactory results can be obtained by performing heat treatment at a temperature preferably above 900°C and below 1098°C, more preferably above 1000°C and below 1096°C, and even more preferably above 1050°C and below 1095°C for a time preferably more than 1 hour and less than 10 hours, more preferably more than 2 hours and less than 8 hours, and even more preferably more than 2 hours and less than 6 hours.
[0069] After the above-mentioned crushing process is carried out, the heat-treated strip can be used to obtain the powder of the target hydrogen storage alloy without further heat treatment.
[0070] The resulting hydrogen storage alloy powder is suitable for use as a negative electrode material in batteries. In this case, it is preferable to perform magnetic separation treatment on the hydrogen storage alloy powder as needed. By performing magnetic separation treatment, impurities that could cause short circuits in the battery can be removed. After performing magnetic separation treatment as needed, a negative electrode for batteries can be prepared, for example, by a known method. Specifically, a hydrogen storage alloy negative electrode can be obtained by mixing a binder and conductive additives into the hydrogen storage alloy powder using a known method and shaping it into a predetermined shape.
[0071] The hydrogen storage alloy negative electrode obtained in this way can be used in primary batteries (including fuel cells) in addition to secondary batteries. For example, it can be used to construct a Ni-MH battery with a positive electrode using nickel hydroxide as the active material, an electrolyte composed of an alkaline aqueous solution, and a separator. In particular, the hydrogen storage alloy of the present invention can reduce the amount of Co used and has both sufficient lifespan and output characteristics, so it is particularly suitable for use as a Ni-MH battery in EVs, HEVs, etc., which require these characteristics.
[0072] Example
[0073] The present invention will be described in more detail below through embodiments. However, the scope of the present invention is not limited to these embodiments.
[0074] [Examples 1 to 5]
[0075] The raw materials were weighed to obtain the mixture, with the mass ratios of each element as shown in Table 1 below. It should be noted that Mm is actually made using La and Ce single metals.
[0076] The resulting mixture was placed in a crucible and fixed on a high-frequency furnace, and the pressure was reduced to 10. -4 ~10 -5After torsion, argon gas is introduced, and the mixture is heated to 1450°C in an argon atmosphere to form a molten liquid.
[0077] The molten metal was poured into a water-cooled copper mold for cooling to obtain an alloy ingot. The resulting alloy ingot was placed in a stainless steel container and placed in a vacuum heat treatment apparatus for a first heat treatment in an argon atmosphere. The heat treatment was carried out at a temperature of 1078°C for 4 hours and 45 minutes.
[0078] The heat-treated alloy ingots were pulverized in an argon atmosphere using a jaw crusher (Fuji Paudal, model 1021-B) and a mill (Yoshida, model 1025-HBG). The pulverization continued until the particles were reduced to a size of -500 μm that could pass through a 500 μm sieve.
[0079] The resulting alloy powder was placed in a stainless steel container and placed in a vacuum heat treatment apparatus for a second heat treatment in an argon atmosphere. The heat treatment was carried out at a temperature of 1078°C for 4 hours and 45 minutes.
[0080] The heat-treated alloy powder was crushed and passed through a sieve with a mesh size of 500 μm to obtain the hydrogen storage alloy powder of each embodiment.
[0081] [Example 6]
[0082] The raw materials were weighed to obtain the mixture, with the mass ratios of each element as shown in Table 1 below. It should be noted that Mm is actually made using La and Ce single metals.
[0083] The resulting mixture was placed in a crucible and fixed on a high-frequency furnace, and the pressure was reduced to 10. -4 ~10 -5 After torsion, argon gas is introduced, and the mixture is heated to 1500°C in an argon atmosphere to form a molten liquid.
[0084] The molten metal is cooled by casting on a rotating, water-cooled copper roller to obtain a thin strip of hydrogen storage alloy.
[0085] The obtained strip was placed in a stainless steel container and placed in a vacuum heat treatment apparatus for heat treatment in an argon atmosphere. The heat treatment was carried out at a temperature of 1078°C for 4 hours and 45 minutes.
[0086] The heat-treated strip was pulverized using a grinder (Yoshida Manufacturing Co., Ltd., model: 1025-HBG) in an argon atmosphere. Pulverization continued until the particles reached a size (-500μm) that could pass through a 500μm sieve, thus obtaining the hydrogen storage alloy powder of this embodiment.
[0087] [Examples 7 to 9]
[0088] The raw materials were weighed to obtain a mixture in the manner shown in Table 1 below, with the mass ratios of each element being equal. In addition, the hydrogen storage alloy powders of each embodiment were obtained in the same manner as in Example 1.
[0089] [Example 10]
[0090] The raw materials were weighed to obtain a mixture in the manner shown in Table 1 below, with the mass ratios of each element being equal. In addition, the hydrogen storage alloy powder of Example 10 was obtained in the same manner as in Example 6.
[0091] [Comparative Examples 1 to 5]
[0092] The raw materials were weighed to obtain the mixture, with the mass ratios of each element as shown in Table 1 below. It should be noted that Mm is actually made using La and Ce single metals.
[0093] The resulting mixture was placed in a crucible and fixed on a high-frequency furnace, and the pressure was reduced to 10. -4 ~10 -5 After torsion, argon gas is introduced, and the mixture is heated to 1450°C in an argon atmosphere to form a molten liquid.
[0094] The molten metal was poured into a water-cooled copper mold for cooling to obtain an alloy ingot. The resulting alloy ingot was placed in a stainless steel container and placed in a vacuum heat treatment apparatus for heat treatment in an argon atmosphere. The heat treatment was carried out at a temperature of 1078°C for 4 hours and 45 minutes.
[0095] The heat-treated alloy ingots were pulverized in an argon atmosphere using a jaw crusher (Fuji Paudal, model: 1021-B) and a mill (Yoshida Manufacturing Co., Ltd., model: 1025-HBG). Pulverization continued until the particles were reduced to a size of -500 μm that could pass through a 500 μm sieve, yielding powders of the hydrogen storage alloys for each comparative example.
[0096] 〔evaluate〕
[0097] The composite modulus E and hardness H were measured for Examples 1 to 10 and Comparative Examples 1 to 5. Furthermore, the a-axis length, c-axis length, and segregation ratio of the hydrogen storage alloy powders obtained in each example and comparative example were measured using the following methods. The results are shown in Table 2 below. Further, the micronization residual rate index, specific surface area increase ΔCS, and magnetization intensity after alkali treatment were measured for the hydrogen storage alloy powders obtained in each example and comparative example using the following methods. The results are shown in Table 3 below.
[0098] [Composite modulus E, hardness H, and H / E]
[0099] After resin coating, the alloy powders of each embodiment and comparative example were mirror-polished to expose the precise cross-section of each particle. Next, measurements were performed using a SEM-Indenter system (Femto Tools, model: FT-NMT04). The SEM used was a SUPRA 55VP (Carl Zeiss), and the sensor used was an FT S200000 (diamond indenter, Berkovich (65.3°)). The measurement conditions were set as follows.
[0100] Measurement mode: Indentation CSM (Frequency = 200MHz)
[0101] • Indentation load: Maximum 200,000 μN
[0102] • Indentation offset: arbitrary
[0103] • Number of measurement points: 5 or more (valid) / 3 particles per sample; Measurement interval: 15μ (4 × 4 points = 16 points)
[0104] • Hardness calibration: Fused silica (Reduced Modulus: 69.6 GPa)
[0105] It should be noted that during the measurement process, measurement points with abnormal behavior on the stress-strain curve due to particle cracks or abnormal surface shapes (such as abrasions, foreign objects, etc.) were excluded from the measurement data and were not referenced.
[0106] Calculate the average value of the data obtained from each measurement, and use it as the value of H and E respectively. Additionally, the value of H / E is calculated by dividing H by E.
[0107] [Segregation Phase Ratio]
[0108] Hydrogen storage alloy powder was placed inside an acrylic cylindrical ring, followed by the flow of epoxy resin, and left to cure overnight. The cured material was cut to an appropriate height, and then surface-polished using a Struers KK (S5629, Laboforce-3) mill to make the alloy cross-section visible in the resin. Next, gold was deposited using an ion sputtering apparatus (Eikoh Co., Ltd., IB-3) with the alloy cross-section as the upper surface, yielding a sample for SEM measurement.
[0109] The obtained samples were placed in a scanning electron microscope (Hitachi High-Technologies Corporation, model: SU8220) and the alloy cross-sections were observed under the following conditions. It should be noted that the semiconductor backscattered electron detector included with this instrument was also used for SEM-BSE image-based observation of the alloy cross-sections.
[0110] [Observation Conditions]
[0111] Detector: BSE(PD)
[0112] Specimen height (z): 8.0
[0113] Accelerating voltage: 10.0kV
[0114] Probe current: High
[0115] Number of particles observed: 100
[0116] Magnification Observation: Any (choose any magnification level at which the entire particle is visible)
[0117] Next, the captured images were analyzed using image analysis software for particle size distribution determination (Mountech Co., Ltd., Mac-View version 4). The analysis steps are shown below.
[0118] [Analysis Steps]
[0119] • Use a stylus to trace the entire circumference of the photographed particles to define them.
[0120] • In the presence of a segregated phase, trace the circumference of the segregated phase with a stylus pen to identify it.
[0121] • Specify the scale based on the scale bar within the SEM image.
[0122] • If the above operations are completed and confirmed, the total area of the particles and the area of the segregated phase will be calculated.
[0123] Next, using the methods described above to analyze the area of each particle and the segregated phase, the segregation rate is calculated using the following formula.
[0124] Segregation rate = (sum of segregated phase areas) / (sum of total particle area) × 100
[0125] [Length of a-axis and length of c-axis]
[0126] The hydrogen storage alloy powder was graded using a sieve with 20 μm openings to obtain a sample of -20 μm (particles passing through the 20 μm sieve openings). The obtained sample was filled into a sample holder and measured using an X-ray diffractometer (Bruker AXS Co., Ltd., D8 ADVANCE) to determine the a-axis length, c-axis length, and lattice volume. The n-number was measured three times for the similarly prepared hydrogen storage alloy powder, and the average value was calculated. The specifications and conditions of the X-ray diffractometer used are described below.
[0127] (Equipment Specifications)
[0128] Lamp: CuKα rays
[0129] Incident beam path
[0130] [Tubemount]
[0131] Voltage: 40 kV
[0132] Current: 40mA
[0133] Element: Cu
[0134] [Optics_Primary_MortorizedSlit]
[0135] Opening: 0.30 [°]
[0136] [SlitMount]
[0137] NoSlit 10.5 [mm] 10.5 [mm]
[0138] Width: 18 [mm]
[0139] Height: 10.5 mm
[0140] Deflection: 0 [°]
[0141] [SollerMount]
[0142] AxialSoller 2.5 [°] 2.5 [°]
[0143] Axial Divergence: 2.5 [°]
[0144] EquatorilDivergence: 0 [°]
[0145] Deflection: 0 [°]
[0146] • Beam path on the receiving side
[0147] Detector: LYNXEYE XE
[0148] [LYNXEYE_XE]
[0149] Mode: LYNXEYE_XE(1D mode)
[0150] Deflection: 0[°]
[0151] ActivationLimit: 200000[1 / s]
[0152] DeactivationLimit: 150000[1 / s]
[0153] LowerDiscriminator: 0.212[V]
[0154] Binning: 1Counter1D: 0[counts]
[0155] ScanCounter: 0[counts]
[0156] Counter0D: 0[counts]
[0157] UpperDiscriminator: 0.230[V]
[0158] Orientation: 0[°]
[0159] [DetectorOpticsMount2]
[0160] Soller_25 2.5[°]2.5[°]
[0161] AxialDivergence: 2.5[°]
[0162] EquatorialDivergence: 0[°]
[0163] Deflection: 0[°]
[0164] [DetectorOpticsMount1]
[0165] Slit_Open_1 0[mm]0[mm]
[0166] Width: 14[mm]
[0167] Height: 0[mm]
[0168] Deflection: 0 [°]
[0169] [SollerMount]
[0170] Deflection: 0 [°]
[0171] [SlitMount]
[0172] NoSlit 10.5 [mm] 10.5 [mm]
[0173] Width: 18 [mm]
[0174] Height: 10.5 mm
[0175] Deflection: 0 [°]
[0176] (Measurement conditions)
[0177] Measurement mode: TwoTheta / Theta
[0178] Mode: PSD high-speed scan
[0179] Time / Stroke: 0.280 [s]
[0180] Start: 20.0000 [°]
[0181] Stop: 120.0046 [°]
[0182] Step size: 0.007175469952
[0183] The X-ray diffraction patterns obtained by measurement (diffraction angle 2θ = 20–120°) were analyzed using analytical software (Software name: TopasVersion5).
[0184] In the analysis, FundamentalParameter was used, Spacegroup: P6 / mmm was selected, and refinement based on the Pawley method was performed with the a-axis length, c-axis length and Crystalsize-L set as variables.
[0185] The peaks of the X-ray diffraction pattern used in the analysis are as follows.
[0186] • The peak of the index located near 20.5° is marked with the Miller index (010).
[0187] • The peak of the index, located near 21.9°, is marked with the Miller index (001).
[0188] • Peaks near 30.1° are marked with the Miller index (011). • Peaks near 35.8° are marked with the Miller index (110). • Peaks near 41.6° are marked with the Miller index (020). • Peaks near 42.4° are marked with the Miller index (111). • Peaks near 44.6° are marked with the Miller index (002). • Peaks near 47.5° are marked with the Miller index (021). • Peaks near 49.5° are marked with the Miller index (012). • The peak of the index near 56.1° was marked with the Miller index (210). • The peak of the index near 58.5° was marked with the Miller index (112). • The peak of the index near 60.9° was marked with the Miller index (211). • The peak of the index near 62.6° was marked with the Miller index (022). • The peak of the index near 64.4° was marked with the Miller index (030). • The peak of the index near 68.9° was marked with the Miller index (031). • The peak of the index near 69.4° was marked with the Miller index (003). • The peak of the index near 73.2° was marked with the Miller index (013). • The peak of the index near 74.3° was marked with the Miller index (212). • The peak of the index near 76.0° was marked with the Miller index (220). • The peak of the index near 79.7° was marked with the Miller index (310). • The peak of the index near 80.2° was marked with the Miller index (221). • The peak of the index near 80.7° was marked with the Miller index (113). • The peak of the index near 81.8° was marked with the Miller index (032). • The peak of the index near 83.9° was marked with the Miller index (311). • The peak of the index near 84.3° was marked with the Miller index (023). • The peak of the index near 90.6° was marked with the Miller index (040). • The peak of the index near 92.7° was marked with the Miller index (222). • The peak of the index near 94.7° was marked with the Miller index (041). • The peak of the index near 95.2° was marked with the Miller index (213). • The peak of the index near 96.3° was marked with the Miller index (312).
[0189] • The peak of the index, located near 98.8°, is marked with the Miller index (004).
[0190] • The peak of the index, located near 101.5°, is marked with the Miller index (320).
[0191] • The peak of the index, located near 102.5°, is marked with the Miller index (014).
[0192] • The peak of the index, located near 102.6°, is marked with the Miller index (033).
[0193] The peak of the index, located near 105.8°, was marked with the Miller index (321).
[0194] • The peak of the index, located near 107.4°, is marked with the Miller index (042).
[0195] The peak of the index, located near 109.0°, is marked with the Miller index (410).
[0196] • The peak of the index located near 110.0° is marked with the Miller index (114).
[0197] • The peak of the index, located near 113.4°, is marked with the Miller index (411).
[0198] • The peak of the index, located near 113.9°, is marked with the Miller index (024).
[0199] The peak of the index, located near 114.0°, was marked with the Miller index (223).
[0200] • The peak of the index, located near 118.0°, is marked with the Miller index (313).
[0201] • The peak of the index, located near 119.2°, is marked with the Miller index (322).
[0202] [Micronization residual index and increase in specific surface area ΔCS]
[0203] 20g of hydrogen storage alloy powder was pulverized for 30 seconds using a cyclone mill (Yoshida Manufacturing Co., Ltd., model: 1033-200). The powder was then sieved between two sieves with 20μm and 53μm apertures, and the powder was adjusted to D. 50 =45μm±0.5μm, and the sample for measurement is obtained. At this time, with D 50 Value (D before loop) 50 The CS value (specific surface area, "CS value before cycling") is also measured. The CS value is the specific surface area calculated based on the measured particle size, assuming the particles are spherical.
[0204] D 50 The CS value was measured using a particle size distribution measuring device (Microtrac, manufactured by Nikkiso Co., Ltd., model: HRA9320-X100) under the following conditions, and the value was determined based on the obtained volumetric standard particle size distribution chart.
[0205] (SetZero time): 30 seconds
[0206] (Measurement time): 30 seconds
[0207] (Number of measurements): 1
[0208] (Solvent and refractive index): Water, 1.33
[0209] (Particle-conditional transmissivity): Reflection
[0210] (Flow rate): 60 ml / sec
[0211] The obtained 2g sample was placed in the PCT holder and activated using an activation device.
[0212] Activation treatment: In a jacketed resistance heater (300°C), a vacuum was applied for 1 hour while the PCT holder was heated. Then, hydrogen at 1.75 MPa was introduced, and after standing for 30 minutes, a vacuum was applied again. This series of operations was performed twice.
[0213] Next, the PCT holder was removed from the jacketed resistance heater and connected to the PCT characteristic measuring device (manufactured by Suzuki Shokan Co., Ltd.). The PCT holder was then placed in a 45°C constant temperature bath for 45 minutes to induce a vacuum in the PCT holder. Then, PCT measurements were performed under the following conditions.
[0214] (Convergence time) 1 min
[0215] (Convergence pressure difference) 0.0001MPa
[0216] (Convergence judgment time) 1 minute
[0217] (End of absorption / storage pressure) 1.7 MPa
[0218] (Release pressure at the end) 0.01 MPa
[0219] (Number of cycles) 10 cycles
[0220] After 10 cycles, the PCT holder was evacuated for 30 minutes, and the sample was removed from the PCT holder to obtain the sample after 10 cycles.
[0221] The D of the sample after 10 cycles 50 Value (after loop D) 50 The values (values), CS values (CS values after cycling), and the D values of the powder obtained by pulverizing the hydrogen storage alloys obtained in the Examples and Comparative Examples using a cyclone mill are compared. 50 Value (D before loop) 50 The micronization residual rate and the increase in specific surface area ΔCS were also measured in the same way, and the CS value (CS value before cycling) were calculated by the following formula.
[0222] Micronization Residual Index = (D after cycling) 50 Value / D before loop 50 (value) × 100
[0223] Increase in specific surface area ΔCS = (CS value after cycle - CS value before cycle)
[0224] The micronization residual rate index listed in Table 3 represents the values obtained by setting the micronization residual rate of Example 1, measured using the above method, to 100, and indexing Examples 2 to 10 and Comparative Examples 1 to 5. The micronization residual rate index is an indicator of the battery's output characteristics; a smaller value indicates better output characteristics.
[0225] [Magnetic intensity after alkali treatment]
[0226] 20g of hydrogen storage alloy powder was pulverized for 1 minute using a cyclone mill (Yoshida Manufacturing Co., Ltd., model: 1033-200), and then classified using a sieve with an aperture of 32μm to obtain D. 50 Samples for processing with a diameter of 21 μm ± 2 μm. D 50 The particle size distribution was measured using a particle size distribution measuring device (Microtrac, manufactured by Nikkiso Co., Ltd., model: HRA9320-X100) under the following conditions, and the result was obtained from the volumetric reference particle size distribution chart.
[0227] (SetZero time): 30 seconds
[0228] (Measurement time): 30 seconds
[0229] (Number of measurements): 1
[0230] (Solvent and refractive index): Water, 1.33
[0231] (Particle-conditional transmissivity): Reflection
[0232] (Flow rate): 60 ml / sec
[0233] Add 3g of the obtained sample to 30ml of a 31% KOH aqueous solution at 120℃, and shake for 3 hours to perform alkali treatment. Then, wash with water, filter, and dry to obtain the sample for testing.
[0234] The magnetic hysteresis loop of the sample was measured using a VSM (Vibration Sample Magnetometer, manufactured by Tamagawa Corporation, model: TM-VSM1014-MRO-M, electromagnet: TM-WTF51.406-101.5FA, sample holder: TM-VSMSH-21-3, sample container: TM-VSMPCA-C). The magnetization intensity was measured.
[0235] It should be noted that before measuring the magnetization intensity, a calibration procedure was performed using a standard sample (99.998% pure Ni) to calibrate the apparatus and confirm that it was functioning correctly. Then, the aforementioned magnetization intensity measurement was conducted.
[0236] (Measurement conditions for a vibrating sample type magnetometer)
[0237] ·maxmagnetic field···10(kOe)
[0238] ·time constant lock-in amp···100(msec)
[0239] ·measuring method···sweep{speed1:5sec / 1kOe speed2:10sec / 1kOe(1~-1[kOe])}
[0240] ·angle···fix 0[°]
[0241] • Gap of pole chips • 14mm
[0242] ·measuringloop···half
[0243] The magnetization intensity can be calculated based on the obtained hysteresis loop.
[0244] Magnetization (emu / g) = {M(10) - 2{M(10) - M(5)}} / measured alloy weight
[0245] In the formula, M(10) is the magnetization intensity when the X-axis is 10 [kOe], and M(5) is the magnetization intensity when the X-axis is 5 [kOe].
[0246] [Increase in specific surface area (ΔCS) × Magnetization intensity after alkali treatment]
[0247] For the hydrogen storage alloy powder, the product of the "specific surface area increase ΔCS" and the "magnetization intensity after alkali treatment" obtained as described above is used to calculate the value of the product.
[0248] The decrease in battery life characteristics is due to the increase in specific surface area caused by the particle fracture of the hydrogen storage alloy during repeated charge-discharge cycles, as well as corrosion initiating on the alloy surface. Thus, particle cracking and corrosion occur simultaneously, degrading battery characteristics. Therefore, as a method for evaluating battery life to assess the impact of their synergistic effect, the product of the increase in specific surface area ΔCS and the magnetization after alkaline treatment is used. If the value of ΔCS × magnetization after alkaline treatment is low, the battery life characteristics can be considered less prone to deterioration.
[0249] [Table 1]
[0250]
[0251] [Table 2]
[0252]
[0253] [Table 3]
[0254]
[0255] As clearly shown in Table 3, the hydrogen storage alloys obtained in each example have a small micronization residual rate index and a small value of specific surface area increase (ΔCS) × magnetization intensity after alkali treatment. That is, the lifetime and output characteristics of the hydrogen storage alloys obtained in each example are balanced. In particular, Examples 1 to 3 show a very good balance between lifetime and output characteristics compared to the other examples. In contrast, the hydrogen storage alloys obtained in the comparative examples either have good lifetime characteristics but poor output characteristics, or good output characteristics but poor lifetime characteristics.
[0256] Industrial availability
[0257] As detailed above, according to the present invention, it is possible to provide a hydrogen storage alloy that reduces the amount of Co used and has both sufficient lifetime and output characteristics.
Claims
1. A hydrogen storage alloy containing Mm, Ni, Mn, Al, and Co, and having a parent phase with a CaCu5-type crystal structure, where Mm represents a mixed rare earth metal. The total proportion of La and Ce in Mm is over 95% by mass. When the molar ratios of Ni, Mn, Al, and Co relative to 1 mole of Mm are set as a, b, c, and d, respectively, d is greater than 0.00 and less than 0.
15. d / b is above 0.00 and below 0.
35. The sum of a+b+c+d is greater than 5.22 and less than 5.
44. The ratio of hardness H to composite modulus E, as determined by nanoindentation, is H / E, which is greater than 0.08 and less than 0.
15. The units for both composite modulus E and hardness H are GPa. When the cross-section of the hydrogen storage alloy is observed using a scanning electron microscope, the ratio of the area of the segregated phase to the area of the cross-section is more than 0.20% and less than 1.10%.
2. The hydrogen storage alloy according to claim 1, wherein The hardness H is above 1 GPa and below 11 GPa.
3. The hydrogen storage alloy according to claim 1, wherein In the CaCu5 type crystal structure, the ratio of the c-axis length to the a-axis length is greater than 0.8080 and less than 0.8110.
4. The hydrogen storage alloy according to claim 1, wherein The c / b ratio is above 0.30 and below 0.85.
Citation Information
Patent Citations
Low co hydrogen occlusion alloy
US20060188385A1
Hydrogen storage alloy
US20190348671A1
Low co hydrogen storage alloys
CN1833039A
Low Co hydrogen storage alloy powder
JP6948441B1