A magnesium tailings admixture and its preparation method and application
By mixing magnesium tailings powder with other additives in proportion and preparing admixtures, and adding them to concrete, the problem of volume expansion and strength decrease caused by excessive dosage of magnesium tailings in concrete has been solved, and a large amount of magnesium tailings has been achieved. Resource utilization and environmentally friendly resource utilization.
Patent Information
- Application Number
- CN202410162991.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-05
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-02-05
AI Technical Summary
Excessive dosage of dolomite magnesium tailings in concrete leads to volume expansion and reduced strength. Existing technology makes it difficult to realize large-scale resource utilization of magnesium tailings and causes environmental pollution problems.
Mix magnesium tailings powder with borax, coal gangue powder, zeolite powder, sodium silicate and xanthan gum in a certain proportion. After high temperature insulation and grinding, the magnesium tailings admixture is prepared and added to concrete to control the reaction of magnesium oxide. Speed and volume expansion improve the mechanical properties and volume stability of concrete.
It realizes the use of high dosage of dolomite magnesium tailings in cement concrete, improves the mechanical properties, volume stability and durability of concrete, and solves the problems of resource waste and environmental pollution.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_4
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of comprehensive utilization of solid waste resources, and in particular to a magnesium tailings admixture and a preparation method and application thereof. Background Art
[0002] When using dolomite magnesium ore to smelt magnesium-based products, a large amount of unusable tailings with a particle size of less than 10 mm are produced while mining dolomite magnesium ore. The main component of dolomite magnesium tailings is magnesium-calcium carbonate compounds, of which the content of magnesium compounds accounts for more than 30%. The accumulation of these dolomite magnesium tailings not only occupies land, but also affects the surrounding environment. Moreover, the stock of dolomite tailings is huge. If a large amount of resource utilization is not carried out, it will inevitably have a lasting adverse impact on the environment. Therefore, the resource utilization of dolomite magnesium tailings is imminent.
[0003] At present, there are a lot of studies on the use of magnesium ore in the field of building materials, but it is mainly to use magnesium ore to prepare magnesium oxide and then prepare concrete expansion agent based on magnesium oxide, or to prepare micro-expansion cement, which can effectively inhibit the volume shrinkage of concrete. The use of magnesium ore to make expansion agent is not only low in usage, but also cannot be used on a large scale in concrete, and it is mainly to use magnesium ore, and the use of tailings is less, and there are fewer studies. But for now, based on magnesium ore tailings, it has been studied that it is used as an admixture in building products and concrete, and it is mainly to use it to generate magnesium hydroxide in cement to produce micro-expansion, thereby inhibiting cracking caused by volume shrinkage. However, when the tailings dosage is too high, due to the large amount of magnesium hydroxide (brucite) generated, the internal volume expansion of concrete increases, resulting in damage to the internal structure, thereby causing the concrete strength to decrease. At present, when magnesium tailings are added to concrete for use, the amount of magnesium tailings added generally accounts for about 5% of the total weight of cementitious materials in concrete, otherwise it will have a greater adverse effect on the volume stability of mortar and concrete. However, the low dosage of magnesium tailings cannot realize the large-scale use of magnesium tailings, and the large-scale resource utilization of magnesium tailings is limited. Summary of the invention
[0004] In view of the problems and shortcomings in the prior art, the purpose of the present invention is to provide a magnesium tailings admixture and a preparation method and application thereof.
[0005] The first aspect of the present invention provides a method for preparing a magnesium tailings admixture, comprising the following steps:
[0006] (1) mixing magnesium tailing powder and borax uniformly to obtain a mixture, heating the mixture to 850-950° C. and then performing heat preservation treatment; after the heat preservation is completed, adding coal gangue powder to the mixture, stirring uniformly, and cooling to room temperature to obtain product A;
[0007] (2) Add zeolite powder, sodium silicate, grinding aid and xanthan gum to the product A, mix well and grind to obtain magnesium tailings admixture.
[0008] According to the above preparation method, preferably, the mass ratio of the magnesium tailings powder to borax is 1:(0.05-0.1).
[0009] According to the above preparation method, preferably, the mass ratio of the coal gangue powder to the dolomite magnesium tailings powder is (0.2-0.3):1.
[0010] According to the above preparation method, preferably, the mass ratio of the zeolite powder to the product A is (0.1-0.2):1.
[0011] According to the above preparation method, preferably, the mass ratio of the sodium silicate to the product A is (0.02-0.04):1.
[0012] According to the above preparation method, preferably, the mass ratio of the xanthan gum to the product A is (0.005-0.01):1.
[0013] According to the above preparation method, preferably, the mass ratio of the grinding aid to the product A is (0.01-0.02):1.
[0014] According to the above preparation method, preferably, in step (1), the insulation time is 10 to 20 minutes.
[0015] According to the above preparation method, preferably, in step (1), the heating rate of the heating process is ≤30°C / min.
[0016] According to the above preparation method, preferably, in step (1), before adding the coal gangue powder to the mixture, the mixture is stirred to make it uniformly mixed.
[0017] According to the above preparation method, preferably, the specific surface area of the magnesium tailings powder is 300 to 600 m 2 / kg; the specific surface area of the magnesium tailings admixture is 600-800m 2 / kg.
[0018] According to the above preparation method, preferably, the specific surface area of the coal gangue powder is 300-600m 2 More preferably, the coal gangue powder is non-spontaneous combustion coal gangue powder.
[0019] According to the above preparation method, preferably, the magnesium tailings powder is dolomite magnesium tailings powder.
[0020] The second aspect of the present invention provides a magnesium tailings admixture product prepared by the preparation method described in the first aspect.
[0021] The third aspect of the present invention provides the use of the magnesium tailings admixture product described in the second aspect in concrete.
[0022] A fourth aspect of the present invention provides concrete, wherein the concrete contains the magnesium tailings admixture product described in the second aspect.
[0023] According to the above concrete, preferably, the concrete is prepared from aggregate, cement, water reducing agent, water and magnesium tailings admixture.
[0024] The fifth aspect of the present invention provides a method for preparing concrete, which comprises: first mixing other powders in the concrete raw materials except water and the magnesium tailings admixture product to obtain a dry mix; then uniformly mixing the magnesium tailings admixture product with water to obtain a wet mix; and uniformly mixing the dry mix with the wet mix to obtain the concrete.
[0025] According to the above-mentioned method for preparing concrete, preferably, the aggregate, cement and water reducing agent in the concrete are first mixed to obtain a dry mix; then the magnesium tailings admixture product is evenly mixed with water to obtain a wet mix; and the dry mix and the wet mix are evenly mixed to obtain the concrete.
[0026] Compared with the prior art, the present invention has the following positive and beneficial effects:
[0027] (1) The present invention mixes magnesium tailing powder and borax in a certain proportion and then heat-treats them at 850-950°C, so that the magnesium tailing decomposes to generate magnesium oxide, which is further dissolved by the molten material of borax at high temperature, so that the two can be effectively fused, and then the speed and content of magnesium oxide participating in the reaction are controlled by the molten material of borax, and its volume expansion after the reaction is restricted, so as to avoid the adverse effect on the volume stability of concrete. In addition, the coal gangue contains a certain amount of carbon, which is added to the above-mentioned substances in a powder state at high temperature, so that the combustion and activity of carbon can be increased, so that a loose structure is formed on the surface of the coal gangue, which can provide a certain volume space for magnesium oxide to expand after the reaction with water, which is beneficial to the volume stability of concrete, and the coal gangue after combustion has strong water absorption and water constraint, which can consume a large amount of water, reduce the formation of magnesium hydroxide expansion products when magnesium oxide meets water, and its loose structure can increase the grindability of the admixture, and also realize the resource utilization of coal gangue.
[0028] (2) Zeolite powder has the function of ion exchange. Zeolite powder can participate in the ion exchange and effectively replace free magnesium ions, realize structural constraints on magnesium ions, reduce the generation of magnesium hydroxide expansion products, and improve volume stability. In addition, sodium silicate can be quickly dissolved in the slurry. At the same time, its viscosity is relatively high. It can react with magnesium ions to form magnesium silicate, which can improve the tensile strength and toughness of concrete, enhance the crack resistance of concrete, reduce the generation of magnesium hydroxide, and reduce expansion. Xanthan gum has good water absorption and water retention. After adding water to moisten, the admixture retains sufficient moisture, accelerates the exchange between zeolite powder and magnesium ions, promotes the reaction of boric acid and calcium ions to form calcium borate, effectively assists in controlling the movement of magnesium ions, and reduces the adverse expansion effect of the formation of magnesium hydroxide on concrete.
[0029] (3) The magnesium tailings admixture prepared by the present invention can be added to concrete as a cementitious material, which not only enables the high-dosage use of dolomite magnesium tailings in cement concrete, but also greatly improves the mechanical properties, volume stability and durability of concrete, realizes the resource utilization of dolomite magnesium tailings, and solves the resource waste and environmental pollution problems existing in the accumulation of existing dolomite magnesium tailings. DETAILED DESCRIPTION
[0030] In order to enable those skilled in the art to more clearly understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below in conjunction with specific embodiments.
[0031] The following detailed description is exemplary and is intended to provide further description of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those of ordinary skill in the art to which the present invention belongs. It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention.
[0032] The experimental methods in the following examples without specifying specific conditions all adopt conventional techniques in the art or follow the conditions recommended by the manufacturers; the reagents or instruments used without specifying the manufacturers are all conventional products that can be obtained commercially.
[0033] Example 1: Borax dosage study experiment
[0034] In order to study the effect of borax dosage on the performance of the prepared magnesium tailings admixture, the present invention carried out Examples 1-1 to 1-3 and Comparative Examples 1-1 to Comparative Example 1-3. The specific contents of Examples 1-1 to 1-3 and Comparative Examples 1-1 to Comparative Example 1-3 are as follows:
[0035] Example 1-1:
[0036] A method for preparing a magnesium tailings admixture, comprising the following specific steps:
[0037] (1) 100 parts by weight of dolomite magnesium tailings powder and borax were mixed uniformly at a mass ratio of 1:0.05 to obtain a mixture; the mixture was heated to 880°C at a heating rate of 20°C / min and kept warm for 12 minutes; after the insulation, the mixture was stirred for 160 seconds to make it uniformly mixed, and then non-spontaneous combustion coal gangue powder was added to the mixture, stirred and mixed for 40 seconds, and immediately cooled by blowing at room temperature to obtain product A. The specific surface area of the dolomite magnesium tailings powder is 410m 2 / kg, the specific surface area of the coal gangue powder is 305m 2 / kg, the mass ratio of the coal gangue powder to the dolomite magnesium tailings powder is 0.25:1.
[0038] (2) Add zeolite powder, sodium silicate, grinding aid and xanthan gum to 100 parts by weight of product A, mix well and grind until the specific surface area reaches 700 m 2 / kg, and the magnesium tailings admixture is obtained. The mass ratio of the zeolite powder to the product A is 0.15:1, the mass ratio of the sodium silicate to the product A is 0.03:1, the mass ratio of the xanthan gum to the product A is 0.008:1, and the mass ratio of the grinding aid to the product A is 0.015:1.
[0039] Embodiment 1-2:
[0040] The content of Example 1-2 is substantially the same as that of Example 1-1, except that in step (1), the mass ratio of dolomite magnesium tailings powder to borax is 1:0.08.
[0041] Embodiment 1-3:
[0042] The content of Example 1-3 is substantially the same as that of Example 1-1, except that in step (1), the mass ratio of dolomite magnesium tailings powder to borax is 1:0.1.
[0043] Comparative Example 1-1:
[0044] The content of Comparative Example 1-1 is substantially the same as that of Example 1-1, except that in step (1), the mass ratio of dolomite magnesium tailings powder to borax is 1:0.12.
[0045] Comparative Example 1-2:
[0046] The content of Comparative Example 1-2 is substantially the same as that of Example 1-1, except that in step (1), the mass ratio of dolomite magnesium tailings powder to borax is 1:0.02.
[0047] Comparative Examples 1-3:
[0048] The content of Comparative Example 1-3 is substantially the same as that of Example 1-1, except that in step (1), the mass ratio of dolomite magnesium tailings powder to borax is 1:0.
[0049] In order to verify the performance of the magnesium tailings admixture prepared in Examples 1-1 to 1-3 and Comparative Examples 1-1 to 1-3, the mixture of product A, zeolite powder, sodium silicate, grinding aid and xanthan gum in the detection step (2) was ground to a specific surface area of 700 m 2 / kg required grinding time; at the same time, the magnesium tailings admixtures prepared in Examples 1-1 to 1-3 and Comparative Examples 1-1 to 1-3 were added to the concrete respectively to prepare six kinds of concrete. Among them, the components of the concrete are, by weight: 280 parts of PO.42.5 cement, 70 parts of magnesium tailings admixture, 860 parts of river sand (medium sand), 940 parts of crushed stone (5-25mm continuous grading), 7 parts of polycarboxylic acid water reducer, and 157 parts of water. The preparation method of the above concrete is: first, the river sand (medium sand), crushed stone, PO.42.5 cement and water reducer in the concrete are evenly mixed to obtain a dry mix; then the magnesium tailings admixture is evenly mixed with water to obtain a wet mix; the dry mix and the wet mix are evenly mixed to obtain the concrete. According to GB / T50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Concrete", the 28d compressive strength of concrete was tested, and GB / T50082-2009 "Standard for Test Methods for Long-term Properties and Durability of Ordinary Concrete" was used to test the 180d shrinkage rate of concrete. The test results are shown in Table 1.
[0050] Table 1 Effect of magnesium tailings admixtures prepared in Examples 1-1 to 1-3 and Comparative Examples 1-1 to 1-3 on concrete performance
[0051]
[0052] As shown in Table 1, when borax is not added or the amount of borax added is low, the grindability of the prepared admixture becomes worse, the grinding time is prolonged, the compressive strength of the concrete is low after being added to the concrete, and the volume stability decreases, and a large expansion occurs; the reason is that when borax is not added or the amount of borax used is small, it is impossible to form a good encapsulation of the magnesium oxide in the dolomite tailings, and the encapsulation and adhesion are uneven. After calcium oxide becomes calcium hydroxide in the later stage, it reacts with borax to form calcium borate, which cannot have a good covering effect on magnesium oxide. More magnesium oxide participates in the cement hydration reaction to form expansion, which makes the volume stability of concrete decrease. With the increase of borax addition, the grindability of the prepared admixture remains unchanged, and the compressive strength of the concrete gradually increases after the admixture is added to the concrete, and the volume stability also gradually increases; but when the amount of borax added is too high, the mechanical properties of the concrete are decreased after the prepared admixture is added to the concrete. This is because under the condition of high borax addition, there is too much borax, which causes serious slow setting of the concrete, affects the normal hydration of cement, and causes the mechanical properties of the concrete to decrease. Therefore, the mass ratio of dolomite magnesium tailings to borax is preferably 1: (0.05-0.1).
[0053] Example 2: Experimental study on the amount of coal gangue
[0054] In order to study the effect of the amount of coal gangue on the performance of the prepared magnesium tailings admixture, the present invention carried out Examples 2-1 to 2-2 and Comparative Examples 2-1 to 2-3. The specific contents of Examples 2-1 to 2-2 and Comparative Examples 2-1 to 2-3 are as follows:
[0055] Example 2-1:
[0056] The content of Example 2-1 is basically the same as that of Example 1-1, except that in step (1), the mass ratio of coal gangue powder to dolomite magnesium tailings powder is 0.2:1.
[0057] Example 2-2:
[0058] The content of Example 2-2 is basically the same as that of Example 1-1, except that in step (1), the mass ratio of coal gangue powder to dolomite magnesium tailings powder is 0.3:1.
[0059] Comparative Example 2-1:
[0060] The content of Comparative Example 2-1 is substantially the same as that of Example 1-1, except that in step (1), the mass ratio of the coal gangue powder to the dolomite magnesium tailings powder is 0.4:1.
[0061] Comparative Example 2-2:
[0062] The content of Comparative Example 2-2 is substantially the same as that of Example 1-1, except that in step (1), the mass ratio of the coal gangue powder to the dolomite magnesium tailings powder is 0.1:1.
[0063] Comparative Example 2-3:
[0064] The content of Comparative Example 2-3 is substantially the same as that of Example 1-1, except that in step (1), the mass ratio of the coal gangue powder to the dolomite magnesium tailings powder is 0:1.
[0065] In order to verify the performance of the magnesium tailings admixture prepared in Examples 2-1 to 2-2 and Comparative Examples 2-1 to 2-3, the mixture of product A and zeolite powder, sodium silicate, grinding aid and xanthan gum in the detection step (2) was ground to a specific surface area of 700 m 2 / kg required grinding time; At the same time, the magnesium tailings admixtures prepared in Examples 2-1 to 2-2 and Comparative Examples 2-1 to 2-3 were added to the concrete respectively to prepare five kinds of concrete. Among them, the components of the concrete are as follows by weight: 280 parts of PO.42.5 cement, 70 parts of magnesium tailings admixture, 860 parts of river sand (medium sand), 940 parts of crushed stone (5-25mm continuous grading), 7 parts of polycarboxylic acid water reducer, and 157 parts of water. According to GB / T 50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Concrete", the 28d compressive strength of concrete and GB / T50082-2009 "Standard for Test Methods for Long-term Performance and Durability of Ordinary Concrete" were tested for the 180d shrinkage of concrete, and the test results are shown in Table 2.
[0066] Table 2 shows the effects of magnesium tailings admixtures prepared in Examples 2-1 to 2-2 and Comparative Examples 2-1 to 2-3 on concrete performance
[0067]
[0068]
[0069] As shown in Table 2, when no gangue is added or the amount of gangue is small, the grindability of the admixture is poor, the prepared concrete has low compressive strength and large expansion; with the increase of the amount of gangue added, the grindability of the prepared admixture increases, because the carbon in the gangue powder burns under high temperature conditions, which increases the porosity of the gangue surface structure and improves the grindability; moreover, with the increase of the amount of gangue added, the compressive strength and volume stability of the concrete both show a trend of first increasing and then decreasing. After the high-temperature activation of the gangue, the active substances are increased, mainly silicon dioxide, which increases the silicon-calcium ratio and improves its activity, which is beneficial to the improvement of concrete strength and the formation of calcium silicate, and is beneficial to the increase of volume stability; when the amount of gangue added is too high, its structural pores increase, the water absorption rate is high, resulting in an increase in the shrinkage rate of the concrete and a decrease in volume stability. Therefore, the mass ratio of gangue to dolomite magnesium tailings is preferably (0.2-0.3):1.
[0070] Example 3: Experimental study on the dosage of zeolite powder
[0071] In order to study the effect of zeolite powder dosage on the performance of the prepared magnesium tailings admixture, the present invention carried out Examples 3-1 to 3-2 and Comparative Examples 3-1 to 3-3. The specific contents of Examples 3-1 to 3-2 and Comparative Examples 3-1 to 3-3 are as follows:
[0072] Example 3-1:
[0073] The content of Example 3-1 is basically the same as that of Example 1-1, except that in step (2), the mass ratio of zeolite powder to product A is 0.1:1.
[0074] Example 3-2:
[0075] The content of Example 3-2 is basically the same as that of Example 1-1, except that in step (2), the mass ratio of zeolite powder to product A is 0.2:1.
[0076] Comparative Example 3-1:
[0077] The content of Comparative Example 3-1 is substantially the same as that of Example 1-1, except that in step (2), the mass ratio of zeolite powder to product A is 0.3:1.
[0078] Comparative Example 3-2:
[0079] The content of Comparative Example 3-2 is substantially the same as that of Example 1-1, except that in step (2), the mass ratio of zeolite powder to product A is 0.05:1.
[0080] Comparative Example 3-3:
[0081] The content of Comparative Example 3-3 is substantially the same as that of Example 1-1, except that in step (2), the mass ratio of zeolite powder to product A is 0:1.
[0082] In order to verify the performance of the magnesium tailings admixture prepared in Examples 3-1 to 3-2 and Comparative Examples 3-1 to 3-3, the mixture of product A, zeolite powder, sodium silicate, grinding aid and xanthan gum in the detection step (2) was ground to a specific surface area of 700 m 2 / kg required grinding time; At the same time, the magnesium tailings admixtures prepared in Examples 3-1 to 3-2 and Comparative Examples 3-1 to 3-3 were added to the concrete to prepare five kinds of concrete. Among them, the components of the concrete are as follows by weight: 280 parts of PO.42.5 cement, 70 parts of magnesium tailings admixture, 860 parts of river sand (medium sand), 940 parts of crushed stone (5-25mm continuous grading), 7 parts of polycarboxylic acid water reducer, and 157 parts of water. According to GB / T 50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Concrete", the 28d compressive strength of concrete and GB / T50082-2009 "Standard for Test Methods for Long-term Performance and Durability of Ordinary Concrete" were tested for the 180d shrinkage of concrete, and the test results are shown in Table 3.
[0083] Table 3 shows the effects of magnesium tailings admixtures prepared in Examples 3-1 to 3-2 and Comparative Examples 3-1 to 3-3 on concrete performance
[0084]
[0085] It can be seen from Table 3 that zeolite powder has little effect on the grindability of admixtures, but has a greater effect on the strength and shrinkage of concrete. When the amount of zeolite powder added is low, the prepared concrete has the lowest compressive strength and poor volume stability. This is because the lack of zeolite powder's adsorption and ion exchange effect on magnesium ions in the reaction causes magnesium ions to participate in the reaction, increasing their expansibility, resulting in increased expansion of concrete and decreased strength. With the increase in the amount of zeolite powder used, the compressive strength and volume stability of concrete both show a trend of first increasing and then decreasing. Therefore, the mass ratio of zeolite powder to product A is preferably (0.1-0.2):1.
[0086] Example 4: Sodium silicate dosage study experiment
[0087] In order to study the effect of sodium silicate dosage on the performance of the prepared magnesium tailings admixture, the present invention carried out Examples 4-1 to 4-2 and Comparative Examples 4-1 to 4-3. The specific contents of Examples 4-1 to 4-2 and Comparative Examples 4-1 to 4-3 are as follows:
[0088] Example 4-1:
[0089] The content of Example 4-1 is basically the same as that of Example 1-1, except that in step (2), the mass ratio of sodium silicate to product A is 0.01:1.
[0090] Example 4-2:
[0091] The content of Example 4-2 is basically the same as that of Example 1-1, except that in step (2), the mass ratio of sodium silicate to product A is 0.04:1.
[0092] Comparative Example 4-1:
[0093] The content of Comparative Example 4-1 is substantially the same as that of Example 1-1, except that in step (2), the mass ratio of sodium silicate to product A is 0.05:1.
[0094] Comparative Example 4-2:
[0095] The content of Comparative Example 4-2 is substantially the same as that of Example 1-1, except that in step (2), the mass ratio of sodium silicate to product A is 0.01:1.
[0096] Comparative Example 4-3:
[0097] The content of Comparative Example 4-3 is substantially the same as that of Example 1-1, except that in step (2), the mass ratio of sodium silicate to product A is 0:1.
[0098] In order to verify the performance of the magnesium tailings admixture prepared in Examples 4-1 to 4-2 and Comparative Examples 4-1 to 4-3, the mixture of product A and zeolite powder, sodium silicate, grinding aid and xanthan gum in the detection step (2) was ground to a specific surface area of 700 m 2 / kg required grinding time; At the same time, the magnesium tailings admixtures prepared in Examples 4-1 to 4-2 and Comparative Examples 4-1 to Comparative Examples 4-3 were added to the concrete to prepare five kinds of concrete. Among them, the components of the concrete are as follows by weight: 280 parts of PO.42.5 cement, 70 parts of magnesium tailings admixture, 860 parts of river sand (medium sand), 940 parts of crushed stone (5-25mm continuous grading), 7 parts of polycarboxylic acid water reducer, and 157 parts of water. According to GB / T 50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Concrete", the 28d compressive strength of concrete and GB / T50082-2009 "Standard for Test Methods for Long-term Performance and Durability of Ordinary Concrete" were tested for the 180d shrinkage of concrete, and the test results are shown in Table 4.
[0099] Table 4 shows the effects of magnesium tailings admixtures prepared in Examples 4-1 to 4-2 and Comparative Examples 4-1 to 4-3 on concrete performance
[0100]
[0101] It can be seen from Table 4 that when sodium silicate is not added, the prepared concrete has low compressive strength and poor volume stability; with the increase of sodium silicate addition, the concrete compressive strength and volume stability gradually increase, but when the mass ratio of sodium silicate to product A exceeds 0.04:1, the compressive strength of the concrete decreases and the volume stability also begins to deteriorate. This is because when the amount of sodium silicate added is too little, the reaction is incomplete, the expansibility of the concrete increases, and the performance decreases; when the amount of sodium silicate added is too much, the excess sodium silicate reacts with magnesium ions, which will further exchange with calcium silicate, causing the concrete structure system to be destroyed and the strength to decrease rapidly. Therefore, the mass ratio of sodium silicate to product A is preferably (0.02-0.04):1.
[0102] Example 5: Experiment on the dosage of xanthan gum
[0103] In order to study the effect of xanthan gum dosage on the performance of the prepared magnesium tailings admixture, the present invention carried out Examples 5-1 to 5-2 and Comparative Examples 5-1 to 5-3. The specific contents of Examples 5-1 to 5-2 and Comparative Examples 5-1 to 5-3 are as follows:
[0104] Example 5-1:
[0105] The content of Example 5-1 is basically the same as that of Example 1-1, except that in step (2), the mass ratio of xanthan gum to product A is 0.005:1.
[0106] Example 5-2:
[0107] The content of Example 5-2 is basically the same as that of Example 1-1, except that in step (2), the mass ratio of xanthan gum to product A is 0.01:1.
[0108] Comparative Example 5-1:
[0109] The content of Comparative Example 5-1 is substantially the same as that of Example 1-1, except that in step (2), the mass ratio of xanthan gum to product A is 0.015:1.
[0110] Comparative Example 5-2:
[0111] The content of Comparative Example 5-2 is substantially the same as that of Example 1-1, except that in step (2), the mass ratio of xanthan gum to product A is 0.001:1.
[0112] Comparative Example 5-3:
[0113] The content of Comparative Example 5-3 is basically the same as that of Example 1-1, except that in step (2), the mass ratio of xanthan gum to product A is 0:1.
[0114] In order to verify the performance of the magnesium tailings admixture prepared in Examples 5-1 to 5-2 and Comparative Examples 5-1 to 5-3, the mixture of product A, zeolite powder, sodium silicate, grinding aid and xanthan gum in the detection step (2) was ground to a specific surface area of 700 m 2 / kg required grinding time; At the same time, the magnesium tailings admixtures prepared in Examples 5-1 to 5-2 and Comparative Examples 5-1 to 5-3 were added to the concrete respectively to prepare five kinds of concrete. Among them, the components of the concrete are as follows by weight: 280 parts of PO.42.5 cement, 70 parts of magnesium tailings admixture, 860 parts of river sand (medium sand), 940 parts of crushed stone (5-25mm continuous grading), 7 parts of polycarboxylic acid water reducer, and 157 parts of water. According to GB / T 50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Concrete", the 28d compressive strength of concrete and GB / T50082-2009 "Standard for Test Methods for Long-term Performance and Durability of Ordinary Concrete" were tested for the 180d shrinkage of concrete, and the test results are shown in Table 5.
[0115] Table 5 shows the effects of magnesium tailings admixtures prepared in Examples 5-1 to 5-2 and Comparative Examples 5-1 to 5-3 on concrete performance
[0116]
[0117] As shown in Table 5, when xanthan gum is not added, the prepared concrete has low compressive strength and poor volume stability; with the increase of xanthan gum addition, the compressive strength and volume stability of the concrete both show a trend of first increasing and then decreasing. This is because xanthan gum has good water absorption and water retention. After adding water to moisten, the admixture retains sufficient moisture, accelerates the exchange between zeolite powder and magnesium ions, promotes the reaction of boric acid and calcium ions to form calcium borate, effectively assists in controlling the movement of magnesium ions, and reduces the adverse expansion effect of magnesium hydroxide on concrete; but when the xanthan gum dosage is too high, the xanthan gum absorbs excessive water, causing the viscosity of the concrete to increase, the performance of the mixture to decrease, and the internal defects to increase, resulting in a decrease in the performance of the concrete. Therefore, the mass ratio of xanthan gum to product A is preferably (0.005-0.01):1.
[0118] Example 6: Insulation temperature study experiment
[0119] In order to study the influence of the insulation temperature on the performance of the prepared magnesium tailings admixture, the present invention carried out Examples 6-1 to 6-2 and Comparative Examples 6-1 to 6-3. The specific contents of Examples 6-1 to 6-2 and Comparative Examples 6-1 to 6-3 are as follows:
[0120] Example 6-1:
[0121] The content of Example 6-1 is basically the same as that of Example 1-1, except that in step (1), the insulation temperature is 850°C.
[0122] Example 6-2:
[0123] The content of Example 6-2 is basically the same as that of Example 1-1, except that in step (1), the insulation temperature is 900°C.
[0124] Comparative Example 6-1:
[0125] The contents of Comparative Example 6-1 are substantially the same as those of Example 1-1, except that in step (1), the insulation temperature is 950°C.
[0126] Comparative Example 6-2:
[0127] The contents of Comparative Example 6-2 are substantially the same as those of Example 1-1, except that in step (1), the insulation temperature is 1000°C.
[0128] Comparative Example 6-3:
[0129] The contents of Comparative Example 6-3 are substantially the same as those of Example 1-1, except that in step (1), the insulation temperature is 800°C.
[0130] In order to verify the performance of the magnesium tailings admixture prepared in Examples 6-1 to 6-2 and Comparative Examples 6-1 to 6-3, the mixture of product A and zeolite powder, sodium silicate, grinding aid and xanthan gum in the detection step (2) was ground to a specific surface area of 700 m 2 / kg required grinding time; at the same time, the magnesium tailings admixtures prepared in Examples 6-1 to 6-2 and Comparative Examples 6-1 to 6-3 were added to the concrete to prepare concrete. Wherein, the components of the concrete are, by weight: 280 parts of PO.42.5 cement, 70 parts of magnesium tailings admixture, 860 parts of river sand (medium sand), 940 parts of crushed stone (5-25mm continuous grading), 7 parts of polycarboxylic acid water reducer, and 157 parts of water. According to GB / T 50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Concrete", the 28d compressive strength of concrete was tested, and GB / T50082-2009 "Standard for Test Methods for Long-term Performance and Durability of Ordinary Concrete" was used to test the 180d shrinkage rate of concrete. The test results are shown in Table 6. Table 6 shows the effects of magnesium tailings admixtures prepared in Examples 6-1 to 6-2 and Comparative Examples 6-1 to 6-2 on the performance of concrete
[0131]
[0132] As can be seen from Table 6, as the insulation temperature increases, the grindability of the admixture improves, but the compressive strength and volume stability of the concrete both show a trend of first increasing and then decreasing. This is because: when the insulation temperature is lower than 850°C, the temperature is too low, the borax cannot form a sufficiently fluid melt, and the absorption and dissolution of magnesium oxide is insufficient, resulting in increased expansion and decreased strength; when the insulation temperature is greater than or equal to 950°C, calcium carbonate can be completely decomposed to form calcium oxide and carbon dioxide, and the calcium carbonate wrapped in the molten state decomposes carbon dioxide, increasing the pore content of the molten state and increasing its grindability; at the same time, part of the calcium carbonate also participates in the molten state, and can quickly react with boric acid in the later stage to form calcium borate, delaying the participation of magnesium oxide in the reaction. However, excessive free calcium oxide generates calcium hydroxide, causing the concrete volume to expand and the performance to decrease. Therefore, the generation of calcium oxide should be controlled. Therefore, the insulation temperature is preferably 850-950°C.
[0133] Example 7: Heating rate study experiment
[0134] In order to study the effect of the heating rate on the performance of the prepared magnesium tailings admixture, the present invention carried out Examples 7-1 to 7-2 and Comparative Examples 7-1 to 7-2. The specific contents of Examples 7-1 to 7-2 and Comparative Examples 7-1 to 7-2 are as follows:
[0135] Example 7-1:
[0136] The content of Example 7-1 is basically the same as that of Example 1-1, except that in step (1), the heating rate is 10°C / min.
[0137] Example 7-2:
[0138] The content of Example 7-2 is basically the same as that of Example 1-1, except that in step (1), the heating rate is 30°C / min.
[0139] Comparative Example 7-1:
[0140] The content of Comparative Example 7-1 is basically the same as that of Example 1-1, except that in step (1), the heating rate is 40°C / min.
[0141] Comparative Example 7-2:
[0142] The content of Comparative Example 7-2 is basically the same as that of Example 1-1, except that in step (1), the heating rate is 50°C / min.
[0143] In order to verify the performance of the magnesium tailings admixture prepared in Examples 7-1 to 7-2 and Comparative Examples 7-1 to 7-2, the mixture of product A, zeolite powder, sodium silicate, grinding aid and xanthan gum in the detection step (2) was ground to a specific surface area of 700 m2 / kg required grinding time; at the same time, the magnesium tailings admixtures prepared in Examples 7-1 to 7-2 and Comparative Examples 7-1 to 7-2 were added to the concrete to prepare concrete. Wherein, the components of the concrete are, by weight: 280 parts of PO.42.5 cement, 70 parts of magnesium tailings admixture, 860 parts of river sand (medium sand), 940 parts of crushed stone (5-25mm continuous grading), 7 parts of polycarboxylic acid water reducer, and 157 parts of water. According to GB / T 50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Concrete", the 28d compressive strength of concrete and GB / T50082-2009 "Standard for Test Methods for Long-term Performance and Durability of Ordinary Concrete" were tested for the 180d shrinkage rate of concrete, and the test results are shown in Table 7. Table 7 shows the influence of magnesium tailings admixtures prepared in Examples 7-1 to 7-2 and Comparative Examples 7-1 to 7-2 on the performance of concrete
[0144]
[0145] It can be seen from Table 7 that when the heating rate is greater than 30°C / min, the grindability of the admixture deteriorates, the mechanical properties of the prepared concrete decrease, and the shrinkage rate is negative and increases. This is because the excessively fast heating rate causes dolomite to slowly decompose into magnesium carbonate, which further rapidly decomposes to form magnesium oxide, and calcium carbonate decomposes into calcium oxide to generate carbon dioxide. The entire process reacts violently, and the generated carbon dioxide quickly overflows and cannot be retained in the mutually molten product of magnesium oxide and borax, increasing the porosity of the mutually soluble product and reducing its grinding difficulty. At the same time, the heating rate is relatively fast, resulting in an increase in the defects of magnesium oxide crystal transformation, which is not conducive to the reduction of magnesium oxide activity. Because during the slow heating process, the magnesium oxide crystal form undergoes a change and the activity decreases, which can reduce the amount and speed of the expansion material magnesium hydroxide generated in cement, and reduce the adverse effects of the admixture on concrete under excessively high dosage conditions. Therefore, the heating rate of the heating process is preferably ≤30°C / min
[0146] Embodiment 8:
[0147] In order to study the substitution of magnesium tailings admixture prepared by the present invention for cementitious materials in concrete, the present invention carried out Examples 8-1 to 8-3 and Comparative Example 8-1. The specific contents of Examples 8-1 to 8-3 and Comparative Example 8-1 are as follows:
[0148] Example 8-1:
[0149] A concrete, wherein the components of the concrete are, by weight, 280 parts of PO.42.5 cement, 70 parts of magnesium tailings admixture, 860 parts of river sand (medium sand), 940 parts of crushed stone (5-25 mm continuous grading), 7 parts of polycarboxylic acid water reducer, and 157 parts of water; wherein the magnesium tailings admixture is the magnesium tailings admixture prepared in Example 1-2. The PO.42.5 cement and the magnesium tailings admixture are used together as cementitious materials in the concrete, and the magnesium tailings admixture accounts for 20% of the total weight of the cementitious materials.
[0150] The preparation method of the above concrete is: firstly, river sand (medium sand), crushed stone, PO.42.5 cement and water reducer in the concrete are mixed evenly to obtain a dry mix; then, the magnesium tailings admixture is mixed evenly with water to obtain a wet mix; and the dry mix and the wet mix are mixed evenly to obtain the concrete.
[0151] Example 8-2:
[0152] A concrete, wherein the components of the concrete are, by weight, 210 parts of PO.42.5 cement, 140 parts of magnesium tailings admixture, 860 parts of river sand (medium sand), 940 parts of crushed stone (5-25mm continuous grading), 7 parts of polycarboxylic acid water reducer, and 157 parts of water; wherein the magnesium tailings admixture is the magnesium tailings admixture prepared in Example 1-2. PO.42.5 cement and magnesium tailings admixture are used together as cementitious materials in concrete, and the magnesium tailings admixture accounts for 40% of the total weight of the cementitious materials. The preparation method of the above concrete is the same as that of Example 8-1.
[0153] Example 8-3:
[0154] A concrete, wherein the components of the concrete are, by weight, 140 parts of PO.42.5 cement, 210 parts of magnesium tailings admixture, 860 parts of river sand (medium sand), 940 parts of crushed stone (5-25 mm continuous grading), 7 parts of polycarboxylic acid water reducer, and 157 parts of water; wherein the magnesium tailings admixture is the magnesium tailings admixture prepared in Example 1-2. The PO.42.5 cement and the magnesium tailings admixture are used together as cementitious materials in the concrete, and the magnesium tailings admixture accounts for 60% of the total weight of the cementitious materials.
[0155] The preparation method of the above concrete is the same as that of Example 8-1.
[0156] Comparative Example 8-1:
[0157] A concrete, wherein the components of the concrete are, by weight, 350 parts of PO.42.5 cement, 860 parts of river sand (medium sand), 940 parts of crushed stone (5-25 mm continuous grading), 7 parts of polycarboxylic acid water reducer, and 157 parts of water.
[0158] The preparation method of the above concrete is: firstly, river sand (medium sand), crushed stone, cementitious material and water reducing agent in the concrete are uniformly mixed to obtain a dry mix; then, the dry mix is uniformly mixed with water to obtain the concrete.
[0159] According to GB / T 50081-2019 “Standard for Test Methods for Physical and Mechanical Properties of Concrete”, the 28d compressive strength of concrete was tested, and according to GB / T 50082-2009 “Standard for Test Methods for Long-term Properties and Durability of Ordinary Concrete”, the 180d shrinkage rate of concrete was tested. The test results are shown in Table 8.
[0160] Table 8 shows the test results of concrete properties prepared in Examples 8-1 to 8-3 and Comparative Example 8-1.
[0161]
[0162] As shown in Table 8, when the content of magnesium tailings admixture in the cementitious material increases from 20% to 60%, the compressive strength and volume stability of the concrete both show a trend of first increasing and then decreasing; when the content of magnesium tailings admixture in the cementitious material is 60%, the compressive strength of the prepared concrete can still reach 45.8MPa, which is significantly better than the concrete without magnesium tailings admixture, and although the shrinkage rate of the concrete is negative, indicating that its volume has slightly expanded, the overall volume stability is still good. It can be seen that the magnesium tailings admixture prepared by the present invention can be added to concrete as a cementitious material, realizing the high dosage of dolomite magnesium tailings in cement concrete, and also realizing the resource utilization of dolomite magnesium tailings.
[0163] Finally, it should be noted that the above embodiments are only preferred embodiments of the present invention, and are not intended to limit the present invention in other forms. Any technician familiar with the profession may use the above technical content as inspiration to make changes or modifications. This is an equivalent embodiment of equivalent changes. However, any simple modification, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the technical concept of the present invention still fall within the scope of protection of the claims of the present invention.
Claims
1. A method for preparing a magnesium tailings admixture, characterized in that: The following steps are involved: (1) mixing magnesium tailings powder and borax uniformly to obtain a mixture, heating the mixture to 850-950° C. and then performing heat preservation treatment; After the heat preservation is completed, coal gangue powder is added to the mixture, stirred evenly, and cooled to room temperature to obtain product A; the magnesium tailings powder is dolomite magnesium tailings powder, and the mass ratio of the magnesium tailings powder to borax is 1: (0.05-0.1); the mass ratio of the coal gangue powder to the magnesium tailings powder is (0.2-0.3): 1; (2) Add zeolite powder, sodium silicate, grinding aid and xanthan gum to the product A, mix well and grind to obtain magnesium tailings admixture; the mass ratio of the zeolite powder to the product A is (0.1-0.2):1, the mass ratio of the sodium silicate to the product A is (0.02-0.04):1, and the mass ratio of the xanthan gum to the product A is (0.005-0.01):
1.
2. The preparation method according to claim 1, characterized in that: In step (1), the heating rate of the heating process is ≤30°C / min; and the heat preservation treatment time is 10 to 20 minutes.
3. The preparation method according to claim 1, characterized in that: Before adding the gangue powder to the mixture in step (1), the mixture is stirred to be uniformly mixed; the specific surface area of the magnesium tailings powder is 300 to 600 m 2 / kg; the specific surface area of the magnesium tailings admixture is 600-800m 2 / kg; the magnesium tailings powder is dolomite magnesium tailings powder.
4. A magnesium tailings admixture product prepared by the preparation method according to any one of claims 1 to 3.
5. Application of the magnesium tailings admixture product according to claim 4 in concrete.
6. A concrete, characterized in that: The concrete contains the magnesium tailings admixture product according to claim 4.
7. A method for preparing the concrete according to claim 6, characterized in that: First, other powders in the concrete raw materials except water and the magnesium tailings admixture product are mixed evenly to obtain a dry mix; then the magnesium tailings admixture product is mixed evenly with water to obtain a wet mix; the dry mix and the wet mix are mixed evenly to obtain the concrete; the magnesium tailings admixture product is the magnesium tailings admixture product according to claim 4.