Composite piston based on ordered graphene modification and preparation method
By coating the surface of the piston skirt with a thermally conductive and wear-resistant layer of ordered graphene and adding materials such as copper-plated graphite powder to the aluminum alloy matrix, the problem of high-temperature and high-pressure wear of the piston material under harsh conditions has been solved, achieving high Thermal conductivity and wear resistance extend the service life of the piston.
Patent Information
- Application Number
- CN202410148036.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-01
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-02-01
AI Technical Summary
Existing piston materials are difficult to meet the requirements of high strength, high thermal conductivity, low thermal expansion and excellent wear reduction and wear resistance under conditions of high temperature, high pressure, high speed and poor lubrication, resulting in easy wear of the piston skirt and shortened working life.
The surface of the piston skirt is coated with a thermally conductive and wear-resistant layer to improve thermal conductivity by regulating the orderly arrangement of graphene. Copper-plated graphite powder and nickel-plated graphite powder are added to the aluminum alloy matrix to improve interface wettability and enhance mechanical strength. Strength and thermal conductivity.
The thermal conductivity and wear resistance of the piston skirt are significantly improved, the wear between cylinders is reduced, the working life of the piston is extended, and the mechanical properties of the aluminum alloy matrix are improved.
Smart Images

Figure CN117986974B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of metal materials, and in particular to a composite material piston modified based on orderly arranged graphene and a preparation method thereof. Background Art
[0002] As an important component of the engine, the piston has a very harsh working environment and generally works under conditions of high temperature, high pressure, high speed and poor lubrication. In order to meet the different working conditions of the piston, it is necessary to develop piston materials with high strength, high thermal conductivity, low thermal expansion and excellent wear reduction and wear resistance. At present, the industrialized piston materials include cast iron, steel and aluminum silicon alloy. Cast iron pistons and steel pistons have high thermal conductivity and mechanical strength, but their density is large and the wear on the cylinder liner is more serious. Aluminum alloy has good thermal conductivity, high strength and low density, but the thermal expansion coefficient of aluminum alloy is large and the wear resistance is poor, which can easily reduce the working life of the piston. Since the engine design widely adopts supercharging and strengthening technology, the requirements for piston performance are becoming more and more stringent. Therefore, it is urgent to study new piston materials. Summary of the invention
[0003] The inventors have found that the piston includes a top, a head and a skirt, and the main material is aluminum alloy. The piston skirt mainly plays a guiding role to withstand the pressure from the cylinder body, and at the same time withstands the high-temperature ablation caused by the combustion and explosion of gasoline in the cylinder body, which makes the piston skirt very easy to wear. The present invention coats a heat-conductive and wear-resistant layer on the surface of the piston skirt. The heat-conductive and wear-resistant layer has good thermal conductivity and can quickly dissipate heat; it also plays the role of heat conduction and wear resistance. Specifically, the graphene sheet has various anisotropies in thermal conductivity along the plane direction. The present invention regulates the orientation of graphene in the heat-conductive and wear-resistant layer material so that the graphene is arranged in an orderly manner along the orientation direction, thereby significantly improving the thermal conductivity of the piston skirt in orientation.
[0004] On one hand, the present invention provides a method for preparing a composite piston based on ordered graphene modification, comprising an aluminum alloy substrate and a heat-conducting and wear-resistant layer coated on a piston skirt, the preparation method comprising the following steps:
[0005] S1: The piston skirt surface is sandblasted to ensure that the surface roughness Ra of the piston skirt is not less than 20 μm.
[0006] S2: Ultrasonic dispersion of ferric chloride, graphene oxide and distilled water is carried out under nitrogen protection, and the mixture is heated in a water bath at 50-70° C., and the pH value is adjusted to 8-10 to obtain Fe3O4 / GO.
[0007] S3: The solid lubricating filler is ball-milled, and then a certain proportion of a binder, a solid lubricating filler, a carbon fiber, a bisphenol A epoxy resin and Fe3O4 / GO are ultrasonically treated under vacuum conditions, and then a curing agent is added and mixed to obtain a mixture.
[0008] S4: Directly inducing the mixture with an external magnetic field, first curing it at room temperature, then curing it at 100-130° C., and cooling it to obtain a heat-conductive and wear-resistant layer.
[0009] The composition comprises, by mass fraction, 5-10% of binder, 10-15% of solid lubricating filler, 10-20% of carbon fiber, 40-70% of bisphenol A epoxy resin and 10-15% of Fe3O4 / GO.
[0010] The ratio of curing agent to bisphenol A epoxy resin is 1:2-4.
[0011] Another aspect of the present invention provides a composite material piston, which is prepared by the above preparation method.
[0012] Compared with the prior art, the present invention achieves at least one of the following beneficial effects:
[0013] (1) In the preparation method of the composite piston modified by ordered graphene of the present invention, a heat-conducting and wear-resistant layer is coated on the surface of the piston skirt, which plays the role of heat conduction and wear resistance at the same time, thereby being able to quickly dissipate heat and reduce the wear between the piston skirt and the cylinder body.
[0014] (2) After being subjected to an external magnetic field, the Fe3O4 / GO of the present invention presents a certain orderly arrangement in the thermal conductive wear-resistant layer, and the heat generated by friction is quickly dissipated through the thermal conductive wear-resistant layer. At the same time, the binder, solid lubricating filler, carbon fiber, Fe3O4 / GO and bisphenol A epoxy resin in the thermal conductive wear-resistant layer are compounded, so that the mechanical properties of the thermal conductive wear-resistant layer are further improved.
[0015] (3) The present invention improves the interface wettability between the metal material and graphite by adding copper-plated graphite powder and nickel-plated graphite powder to the aluminum alloy matrix, thereby improving the mechanical strength, thermal conductivity and wear resistance of the aluminum alloy matrix. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] The drawings described herein are used to provide a further understanding of the present invention and constitute a part of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:
[0017] Figure 1 The present invention shows a process flow chart of the composite piston preparation process based on ordered graphene modification. DETAILED DESCRIPTION
[0018] In order to more clearly illustrate the overall concept of the present invention, a detailed description is given below in an exemplary manner in conjunction with the accompanying drawings.
[0019] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention can also be implemented in other ways different from those described herein, and therefore, the scope of protection of the present invention is not limited by the specific embodiments disclosed below. In the description of this specification, the description of reference terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily have to be directed to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0020] In an exemplary embodiment of the present invention, a method for preparing a composite piston based on ordered graphene modification comprises the following steps:
[0021] S1: Sandblast the surface of the piston skirt to make the surface roughness Ra of the piston skirt not less than 20μm. The piston skirt is made of aluminum alloy and has a relatively smooth surface, which is not conducive to the engagement of the piston skirt with the surface of the heat-conducting and wear-resistant layer. Therefore, the surface of the piston skirt needs to be sandblasted. The roughness of the piston skirt surface after treatment increases, and the contact area with the heat-conducting and wear-resistant layer increases, which is conducive to the combination of the heat-conducting and wear-resistant layer with the piston skirt. Specifically, dust, oil stains and other pollutants will remain on the surface of the piston skirt after sandblasting. The surface can be rinsed with flowing deionized water, and ultrasonically cleaned in ethanol and acetone solutions for 15 minutes. The piston skirt is taken out and the residual liquid on the surface is wiped with cotton wool, and then dried for use.
[0022] S2: Ultrasonic dispersion of ferric chloride, graphene oxide and distilled water under nitrogen protection, heating in a water bath at 50-70° C., adjusting the pH to 8-10, and obtaining Fe3O4 / GO. Specifically, paramagnetic ferroferric oxide / graphene oxide is obtained.
[0023] S3: ball-milling the solid lubricating filler to fully remove moisture from the filler, ultrasonically treating a certain proportion of a binder, a solid lubricating filler, carbon fiber, bisphenol A epoxy resin and Fe3O4 / GO under vacuum conditions, and then adding a curing agent and mixing to obtain a mixture.
[0024] S4: The mixture is oriented and induced by an external magnetic field, first solidified at room temperature, then solidified at 100-130°C, and cooled to obtain a heat-conducting and wear-resistant layer. The preparation process can be referred to Figure 1 shown.
[0025] Among them, by mass fraction, the binder is 5-10%, the solid lubricating filler is 10-15%, the carbon fiber is 10-20%, the bisphenol A epoxy resin is 40-70% and the Fe3O4 / GO is 10-15%;
[0026] The ratio of curing agent to bisphenol A epoxy resin is 1:2-4.
[0027] Optionally, the binder comprises 6-8%, the solid lubricating filler comprises 12-14%, the carbon fiber comprises 13-16%, the bisphenol A epoxy resin comprises 45-55% and the Fe3O4 / GO comprises 12-13%.
[0028] Optionally, the ratio of the curing agent to the bisphenol A epoxy resin is 1:3.
[0029] Optionally, the mass ratio of ferric chloride to graphene oxide is 5-7:1.
[0030] Optionally, the binder is one of polyethylene (PE for short), polyimide (PI for short), and polyamide-imide (PAI for short). Preferably, the binder is PAI.
[0031] Optionally, the solid lubricating filler is one or more of graphite, molybdenum disulfide, boron nitride, zinc oxide, titanium dioxide, barium sulfate and silicate;
[0032] Optionally, the curing agent is polyoxypropylene diamine.
[0033] Optionally, the method for preparing the aluminum alloy substrate comprises the following steps:
[0034] S01: Heat and melt pure aluminum, then add copper-plated graphite powder, nickel-plated graphite powder and fluoride salt and mix them evenly, then add refined powder and cryolite to react at 800-900℃ and perform the first casting;
[0035] S02: The alloy after the first casting is remelted, single crystal silicon is added for melting, and then aluminum-copper alloy (Al-50Cu for short) and aluminum-nickel alloy (Al-10Ni for short) are added to the melt, and then aluminum-phosphorus alloy (Al-P for short) and rare earth (40La-60Ce for short) are added for modification, and then magnesium blocks are added, and degassing agent is added for degassing, and an aluminum alloy matrix is obtained by casting.
[0036] The purity of pure aluminum is greater than 99.9%; the aluminum content in the aluminum alloy matrix is greater than 85%, the silicon content is 8-12%, the copper content is greater than 5%, the magnesium content is 0.8-1%, and the nickel content is 1-2%.
[0037] Optionally, the fluoride salt is one or more of potassium fluoroborate, potassium fluorotitanate, and potassium fluorozirconate.
[0038] Optionally, the average particle size of the copper-coated graphite powder and the galvanized graphite powder is less than 100 μm; preferably, the average particle size of the copper-coated graphite powder and the galvanized graphite powder is less than 40 μm.
[0039] Optionally, the degassing agent is C2Cl6.
[0040] Optionally, the refined powder is one or more of dehydrated zinc chloride, manganese chloride, hexachloroethane, ferric chloride, and carbon tetrachloride.
[0041] Optionally, the mass ratio of the copper-coated graphite powder to pure aluminum is 1:2-4, and the mass ratio of the galvanized graphite powder to pure aluminum is 1:5-7.
[0042] Optionally, the thickness of the heat conductive wear-resistant layer is 0.1-0.3 mm.
[0043] On the basis of the above-mentioned embodiment, the preparation method of the composite piston based on ordered graphene modification is specifically described as follows:
[0044] Example 1
[0045] Thermal conductive wear-resistant layer 1#
[0046] S2: Ultrasonic dispersion of ferric chloride, graphene oxide and distilled water under nitrogen protection, heating in a water bath at 50° C., adjusting the pH to 8, and obtaining Fe3O4 / GO. The mass ratio of ferric chloride to graphene oxide is 5:1.
[0047] S3: The solid lubricating filler boron nitride is ball-milled to fully remove the moisture in the filler, and then a certain mass fraction of 5% binder PE, 10% solid lubricating filler boron nitride, 10% carbon fiber, 65% bisphenol A epoxy resin and 10% Fe3O4 / GO are ultrasonically treated under vacuum conditions, and then a curing agent polyoxypropylene diamine is added to mix to obtain a mixture. The mass ratio of the curing agent to the bisphenol A epoxy resin is 1:2.
[0048] S4: The mixture is oriented and induced by an external magnetic field, first solidified at room temperature (25° C.), then solidified at 100° C., and cooled to obtain a heat-conductive and wear-resistant layer.
[0049] Thermal conductive wear-resistant layer 2#
[0050] S2: Ultrasonic dispersion of ferric chloride, graphene oxide and distilled water under nitrogen protection, heating in a water bath at 60° C., adjusting the pH to 9, and obtaining Fe3O4 / GO. The mass ratio of ferric chloride to graphene oxide is 6:1.
[0051] S3: Solid lubricating filler titanium dioxide is ball-milled to fully remove moisture in the filler, and then a certain mass fraction of 10% binder PI, 15% solid lubricating filler titanium dioxide, 20% carbon fiber, 40% bisphenol A epoxy resin and 15% Fe3O4 / GO are ultrasonically treated under vacuum conditions, and then a curing agent polyoxypropylene diamine is added to mix to obtain a mixture. The mass ratio of the curing agent to the bisphenol A epoxy resin is 1:4.
[0052] S4: The mixture is oriented and induced by an external magnetic field, first solidified at room temperature (25° C.), then solidified at 130° C., and cooled to obtain a heat-conductive and wear-resistant layer.
[0053] Heat conductive wear resistant layer 3#
[0054] S2: Ultrasonic dispersion of ferric chloride, graphene oxide and distilled water under nitrogen protection, heating in a water bath at 60° C., adjusting the pH to 10, and obtaining Fe3O4 / GO. The mass ratio of ferric chloride to graphene oxide is 7:1.
[0055] S3: The solid lubricating filler molybdenum disulfide is ball-milled to fully remove the moisture in the filler, and then a certain mass fraction of 8% binder PAI, 12% solid lubricating filler molybdenum disulfide, 16% carbon fiber, 52% bisphenol A epoxy resin and 12% Fe3O4 / GO are ultrasonically treated under vacuum conditions, and then a curing agent polyoxypropylene diamine is added to mix to obtain a mixture. The mass ratio of the curing agent to the bisphenol A epoxy resin is 1:3.
[0056] S4: The mixture is oriented and induced by an external magnetic field, first solidified at room temperature (25° C.), then solidified at 120° C., and cooled to obtain a heat-conductive and wear-resistant layer.
[0057] Heat conductive wear resistant layer D1
[0058] Based on the heat conductive wear resistant layer 1#, the main difference is that no external magnetic field is used for directional induction.
[0059] The performance of the heat conductive wear-resistant layers 1#-3# and D1 was tested, as shown in Table 1.
[0060] Friction performance characterization: The friction coefficient is obtained by testing the MFT-5000 friction and wear tester at room temperature. The motion mode of the tester is reciprocating mode. During the reciprocating motion, a 9.5mm diameter silicon nitride ceramic ball is used to grind the heat-conducting and wear-resistant layer. The test parameters are as follows: load is 10N, reciprocating distance is 10mm, frequency is 1Hz, and test time is 20min.
[0061] Wear rate (W), calculated as: W = V / (FL); where V is the wear volume (mm 3), F is the normal load (N), and L is the total reciprocating length of the ceramic ball (m).
[0062] Table 1
[0063]
[0064] Example 2
[0065] Aluminum alloy substrate 1#
[0066] S01: The pure aluminum powder is heated and melted at 900°C, and then copper-plated graphite powder with an average particle size of 30 μm, nickel-plated graphite powder with an average particle size of 20 μm, potassium fluoroborate and potassium fluorotitanate are added and evenly mixed, and then refined powdered ferric chloride and cryolite are added to react at 800°C for the first casting; the mass ratio of the copper-plated graphite powder to pure aluminum is 1:2, and the mass ratio of the zinc-plated graphite powder to pure aluminum is 1:5.
[0067] S02: The alloy after the first casting is remelted, single crystal silicon is added for melting, and then Al-50Cu and Al-10Ni are added to the melt, and then the temperature is raised to 800°C, Al-P and 40La-60Ce are added for modification, and then magnesium blocks are added, and degassing agent C2Cl6 is added for degassing, and an aluminum alloy matrix is obtained by casting.
[0068] According to tests, the aluminum content of the prepared aluminum alloy matrix is greater than 85%, the silicon content is 8%, the copper content is 6%, the magnesium content is 0.8%, and the nickel content is 1%.
[0069] Aluminum alloy substrate 2#
[0070] S01: Pure aluminum is heated and melted at 800°C, and then copper-plated graphite powder with an average particle size of 60 μm, nickel-plated graphite powder with an average particle size of 50 μm, potassium fluoroborate, potassium fluorotitanate and potassium fluorozirconate are added and evenly mixed, and then refined powdered carbon tetrachloride and cryolite are added to react at 700°C for the first casting; the mass ratio of copper-plated graphite powder to pure aluminum is 1:4, and the mass ratio of zinc-plated graphite powder to pure aluminum is 1:7.
[0071] S02: The alloy after the first casting is remelted, single crystal silicon is added for melting, and then Al-50Cu and Al-10Ni are added to the melt, and then the temperature is raised to 800°C, Al-P and 40La-60Ce are added for modification, and then magnesium blocks are added, and degassing agent C2Cl6 is added for degassing, and an aluminum alloy matrix is obtained by casting.
[0072] According to tests, the aluminum content of the prepared aluminum alloy matrix is greater than 85%, the silicon content is 12%, the copper content is 7%, the magnesium content is 1%, and the nickel content is 1.7%.
[0073] Aluminum alloy substrate 3#
[0074] S01: Pure aluminum is heated and melted at 950°C, and then copper-plated graphite powder with an average particle size of 20 μm, nickel-plated graphite powder with an average particle size of 30 μm, potassium fluoroborate, potassium fluorotitanate and potassium fluorozirconate are added and evenly mixed, and then refined powdered manganese chloride and cryolite are added to react at 900°C for the first casting; the mass ratio of copper-plated graphite powder to pure aluminum is 1:3, and the mass ratio of zinc-plated graphite powder to pure aluminum is 1:6.
[0075] S02: The alloy after the first casting is remelted, single crystal silicon is added for melting, and then Al-50Cu and Al-10Ni are added to the melt, and then the temperature is raised to 750°C, Al-P and 40La-60Ce are added for modification, and then magnesium blocks are added, and degassing agent C2Cl6 is added for degassing, and an aluminum alloy matrix is obtained by casting.
[0076] According to tests, the aluminum content of the prepared aluminum alloy matrix is greater than 85%, the silicon content is 10%, the copper content is 7%, the magnesium content is 0.9%, and the nickel content is 1.6%.
[0077] Aluminum alloy substrate 4#
[0078] Based on the aluminum alloy matrix 1#, the main difference is that copper-plated graphite powder and nickel-plated graphite powder are not added.
[0079] Aluminum alloy substrate 5#
[0080] Based on the aluminum alloy matrix 1#, the main difference is that the average particle size of the copper-plated graphite powder is 500μm, and the average particle size of the nickel-plated graphite powder is 800μm.
[0081] Example 3
[0082] Composite material piston 1#
[0083] S1: The piston skirt surface is sandblasted to make the piston skirt surface roughness Ra 40 μm. The composite piston 1# includes an aluminum alloy substrate 1# and a heat-conductive and wear-resistant layer 1# coated on the piston skirt.
[0084] Composite material piston 2#
[0085] S1: The piston skirt surface is sandblasted to make the piston skirt surface roughness Ra 50 μm. The composite piston 2# includes an aluminum alloy substrate 2# and a heat-conductive and wear-resistant layer 2# coated on the piston skirt.
[0086] Composite material piston 3#
[0087] S1: The piston skirt surface is sandblasted to make the piston skirt surface roughness Ra 70 μm. The composite piston 3# includes an aluminum alloy substrate 3# and a heat-conducting and wear-resistant layer 3# coated on the piston skirt.
[0088] Composite material piston 4#
[0089] Based on the composite piston 1#, the main difference is that the aluminum alloy matrix is aluminum alloy matrix 2#.
[0090] Composite material piston 5#
[0091] Based on the composite piston 1#, the main difference is that the aluminum alloy matrix is the aluminum alloy matrix 4#.
[0092] Composite material piston 6#
[0093] Based on the composite piston 1#, the main difference is that the aluminum alloy matrix is aluminum alloy matrix 5#.
[0094] Composite piston D1
[0095] Based on the composite material piston 1#, the main difference is that the heat conductive wear-resistant layer is the heat conductive wear-resistant layer D1.
[0096] The composite material pistons 1#-6# and D1 were subjected to performance tests, as shown in Table 2. The tensile strength was tested according to GB / T4338 "High-temperature tensile test method for metal materials".
[0097] Table 2
[0098]
[0099] The thermal conductivity of the aluminum alloy matrix in the composite material piston prepared by the present invention is 200-300 W·m -1 ·K -1 The thermal conductivity of the heat-conducting and wear-resistant layer is not less than 80W·m -1 ·K -1 The heat-conducting and wear-resistant layer plays the role of heat conduction and wear resistance at the same time, so that the temperature difference between the materials is reduced, and the wear with the cylinder body is reduced. The composite material piston of the present invention has a high-temperature tensile strength of 60-110 MPa at 360°C and has good mechanical properties; the friction factor of the heat-conducting and wear-resistant layer is not higher than 0.3, and the friction factor of the aluminum alloy matrix is not higher than 0.25.
[0100] In summary, the composite material piston prepared by the present invention has good mechanical properties, and a heat-conducting and wear-resistant layer is coated on the surface of the piston skirt, which plays the role of heat conduction and wear resistance at the same time.
[0101] The above description is only an embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent substitution, improvement, etc. made within the spirit and principle of the present invention should be included in the scope of the claims of the present invention.
Claims
1. A method for preparing a composite piston based on ordered graphene modification, It is characterized in that The invention comprises an aluminum alloy substrate and a heat-conducting and wear-resistant layer coated on a piston skirt, and the preparation method comprises the following steps: S1: sandblast the piston skirt surface to make the piston skirt surface roughness Ra not less than 20μm; S2: Ultrasonic dispersion of ferric chloride, graphene oxide and distilled water was performed under nitrogen protection, heated in a water bath at 50-70°C, and the pH was adjusted to 8-10 to obtain Fe 3 O 4 / GO; S3: The solid lubricating filler is ball-milled to mix a certain proportion of binder, solid lubricating filler, carbon fiber, bisphenol A epoxy resin and Fe 3 O 4 The / GO is subjected to ultrasonic treatment under vacuum conditions, and then a curing agent is added and mixed to obtain a mixture; S4: Directly inducing the mixture with an external magnetic field, first curing it at room temperature, then curing it at 100-130° C., and cooling it to obtain a heat conductive and wear-resistant layer; Among them, by mass fraction, the binder is 5-10%, the solid lubricating filler is 10-15%, the carbon fiber is 10-20%, the bisphenol A epoxy resin is 40-70% and the Fe 3 O 4 / GO10-15%; The ratio of curing agent to bisphenol A epoxy resin is 1:2-4; The preparation method of the aluminum alloy substrate comprises the following steps: S01: Heat and melt pure aluminum, then add copper-plated graphite powder, nickel-plated graphite powder and fluoride salt and mix them evenly, then add refined powder and cryolite to react at 800-900℃ and perform the first casting; S02: remelting the alloy after the first casting, adding single crystal silicon to melt, then adding aluminum-copper alloy and aluminum-nickel alloy to the melt, then adding aluminum-phosphorus alloy and rare earth to perform modification treatment, then adding magnesium block, adding degassing agent to perform degassing, and casting to obtain an aluminum alloy matrix; The purity of pure aluminum is greater than 99.9%; the aluminum content in the aluminum alloy matrix is greater than 85%, the silicon content is 8-12%, the copper content is greater than 5%, the magnesium content is 0.8-1%, and the nickel content is 1-2%; The average particle sizes of copper-coated graphite powder and galvanized graphite powder are both less than 100 μm.
2. The preparation method according to claim 1, It is characterized in that Binder 6-8%, solid lubricating filler 12-14%, carbon fiber 13-16%, bisphenol A epoxy resin 45-55% and Fe 3 O 4 / GO12-13%.
3. The preparation method according to claim 1, It is characterized in that The ratio of curing agent to bisphenol A epoxy resin is 1:
3.
4. The preparation method according to claim 1, It is characterized in that The binder is one of PE, PI and PAI; and / or the solid lubricating filler is one or more of graphite, molybdenum disulfide, boron nitride, zinc oxide, titanium dioxide, barium sulfate and silicate; And / or the curing agent is polyoxypropylene diamine.
5. The preparation method according to claim 1, It is characterized in that The average particle size of copper-coated graphite powder and galvanized graphite powder is less than 40 μm.
6. The preparation method according to claim 1, It is characterized in that The degassing agent is C 2 Cl 6 .
7. The preparation method according to claim 1, It is characterized in that The refined powder is one or more of dehydrated zinc chloride, manganese chloride, hexachloroethane, ferric chloride, and carbon tetrachloride; And / or the fluoride salt is one or more of potassium fluoroborate, potassium fluorotitanate, and potassium fluorozirconate.
8. The preparation method according to claim 1, It is characterized in that The mass ratio of the copper-plated graphite powder to pure aluminum is 1:2-4, and the mass ratio of the zinc-plated graphite powder to pure aluminum is 1:5-7.
9. A composite piston, It is characterized in that The composite material piston is prepared by any one of the preparation methods of claims 1-8.